A kind of wear-resistant tempered glass and preparation method thereof
By spraying a protective layer composed of modified PMMA resin and glass fiber onto the surface of the glass plate, a layered structure is formed, which solves the problem of insufficient wear resistance of traditional glass products and achieves the effects of high wear resistance, high light transmittance and impact resistance.
Patent Information
- Application Number
- CN202410665671.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Traditional glass products have poor wear resistance, and existing protective layer materials are still insufficient in terms of wear resistance, making it difficult to meet the requirements of high-end fields.
A protective layer composed of modified PMMA resin, glass fiber, plasticizer, and dispersant is formed by spraying it onto the surface of a glass plate to create a layered structure. This, combined with the chemical bonding and network structure of the modified PMMA resin and hollow glass microspheres, improves the strength and wear resistance of the protective layer.
It significantly improves the wear resistance and light transmittance of glass, enhances its impact resistance and weather resistance, and meets the needs of high-end applications.
Smart Images

Figure CN118529945B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass, and in particular to wear-resistant tempered glass and a preparation method thereof. Background Art
[0002] Glass products are widely used in construction, home furnishings, automobiles, electronics and other fields due to their transparency, beauty and easy processing. However, traditional glass products have poor wear resistance and are easily worn and scratched during use, affecting their performance and appearance.
[0003] In order to improve the wear resistance of glass products, the prior art generally adopts a method of coating a protective layer on the glass surface. However, the existing protective layer materials still have deficiencies in wear resistance and are difficult to meet the requirements of high-end fields for the wear resistance of glass products. Summary of the invention
[0004] In order to improve the wear resistance of tempered glass, the present application provides a wear-resistant tempered glass and a preparation method thereof.
[0005] In the first aspect, the present application provides a wear-resistant tempered glass adopting the following technical solution:
[0006] A wear-resistant tempered glass comprises a glass plate and a protective layer; the protective layer is bonded to the glass plate; the protective layer is made of the following raw materials in parts by weight: 30-60 parts of modified PMMA resin; 10-20 parts of glass fiber; 2-7 parts of plasticizer; 1-2 parts of leveling agent; 40-60 parts of butyl acetate; and 1-3 parts of dispersant; the modified PMMA resin is made of the following raw materials: PMMA resin, hydroxypropyltriethoxysilane, hollow glass microspheres, tetraethyl orthosilicate and dibutyltin dilaurate.
[0007] By adopting the above technical scheme, the present application sprays a protective layer on the side of the glass plate, and the protective layer is evenly coated on the surface of the glass plate to form a hierarchical structure, so that the tempered glass has good wear resistance. Glass fiber is added to the protective layer to significantly improve the strength and stiffness of the protective layer. Butyl acetate is mixed with the modified PMMA resin as a solvent. The present application modifies the PMMA resin to improve the wear resistance of the PMMA resin, which originally has poor wear resistance. The protective layer is prepared by compounding various modified components, and the protective layer is sprayed on the tempered glass, which further improves the wear resistance of the glass.
[0008] Preferably, the preparation method of the modified PMMA resin is: 20-40 parts by weight of PMMA resin, 5-10 parts by weight of hydroxypropyltriethoxysilane, 5-10 parts by weight of hollow glass microspheres, 2-6 parts by weight of tetraethyl orthosilicate and 1-2 parts by weight of dibutyltin dilaurate are mixed, stirred and dried to obtain the modified PMMA resin.
[0009] By adopting the above-mentioned technical scheme, the present application modifies the PMMA resin, and the hollow glass microspheres can form a uniform pore structure in the PMMA resin, effectively reducing the density of the material. Hydroxypropyltriethoxysilane and the PMMA resin form a chemical bond, thereby improving the compatibility and interfacial adhesion between the two, thereby improving the mechanical properties and weather resistance of the PMMA resin. At the same time, tetraethyl orthosilicate forms a silica network structure in the component, which can form an interpenetrating network with the PMMA resin, thereby enhancing the hardness of the PMMA resin, thereby improving the wear resistance and weather resistance of the protective layer.
[0010] Preferably, the weight ratio of the PMMA resin, hydroxypropyltriethoxysilane and hollow glass microspheres is 1:(0.24-0.28):(0.24-0.32).
[0011] By adopting the above technical scheme, when PMMA resin, hydroxypropyl triethoxysilane and hollow glass microspheres are in a specific weight ratio, hydroxypropyl triethoxysilane can form hydrogen bonds with the carbonyl groups in PMMA to enhance the interaction between the two, and at the same time, the silanol groups in hydroxypropyl triethoxysilane can combine with the hollow glass microspheres to make the hollow glass microspheres play a skeleton role in the PMMA resin; the three together form a three-dimensional network structure to further enhance the mechanical properties of the PMMA resin, so that the modified PMMA resin can act on the tempered glass to improve the wear resistance of the tempered glass.
[0012] Preferably, the hollow glass microspheres are modified hollow glass microspheres, and the preparation method of the modified hollow glass microspheres is: after mixing 10-20 parts by weight of hollow glass microspheres, 2-8 parts by weight of n-butanol, 5-10 parts by weight of ethylene glycol monobutyl ether and 5-10 parts by weight of cyclohexanone, 1-3 parts by weight of sodium hexametaphosphate, 1-5 parts by weight of zirconium sulfate and 2-8 parts by weight of sodium aluminate are added in sequence, heated and stirred, and the modified hollow glass microspheres are obtained after washing, drying and crushing.
[0013] By adopting the above technical scheme, the present application modifies the hollow glass microspheres. Sodium hexametaphosphate and zirconium sulfate are mixed to form a zirconium-phosphate complex. Sodium aluminate, as a strong base and weak acid salt, can undergo a hydrolysis reaction and combine with the metal ions in the components. Sodium hexametaphosphate, zirconium sulfate and sodium aluminate are mixed and then mixed with the hollow glass microspheres. The overall performance of the hollow glass microspheres can be improved, the stability of the hollow glass microspheres can be improved, the skeleton mechanical properties in PMMA resin can be further improved, and the wear resistance and mechanical properties of tempered glass can be improved.
[0014] Preferably, the weight ratio of the hollow glass microspheres, sodium hexametaphosphate, zirconium sulfate and sodium aluminate is 1: (0.1-0.14): (0.24-0.3): (0.2-0.4).
[0015] By adopting the above technical scheme, when the hollow glass microspheres, sodium hexametaphosphate, zirconium sulfate and sodium aluminate are in a specific weight ratio, the four cooperate together to form a complex on the surface of the hollow glass microspheres, so that the hollow glass microspheres can be better dispersed in the PMMA resin after modification, further improving the impact resistance and wear resistance of the PMMA resin, thereby improving the wear resistance of the protective layer sprayed on the surface of the glass plate.
[0016] Preferably, the particle size of the hollow glass microspheres is 110-250 nm.
[0017] By adopting the above technical solution and selecting a suitable hollow glass microbead particle size, the hollow glass microbead can be better dispersed in the PMMA resin, thereby improving the wear resistance of the PMMA resin.
[0018] Preferably, the plasticizer includes one of dioctyl phthalate, trimethyl phosphate and chlorinated paraffin.
[0019] Preferably, the dispersant includes one of ammonium polyacrylate and stearic acid monoglyceride.
[0020] By adopting the above technical solution and using a suitable plasticizer and dispersant, the wear resistance of the tempered glass obtained by spraying the protective layer on the glass plate can be improved.
[0021] Preferably, the weight ratio of the modified PMMA resin, dioctyl phthalate and glass fiber is 1:(0.12-0.15):(0.4-0.45).
[0022] By adopting the above technical scheme, when the modified PMMA resin, dioctyl phthalate and glass fiber are in a specific weight ratio, dioctyl phthalate combines the glass fiber with the modified PMMA resin, thereby improving the wear resistance and weather resistance of the modified PMMA resin, and is sprayed on the glass surface to form a protective layer, thereby further improving the acid resistance and light transmittance of the glass plate.
[0023] In a second aspect, the present application provides a method for preparing wear-resistant tempered glass using the following technical solution:
[0024] A method for preparing wear-resistant tempered glass, S1. After uniformly stirring modified PMMA resin, glass fiber, plasticizer and butyl acetate, adding a leveling agent and a dispersant, heating and stirring to obtain a protective liquid;
[0025] S2. After the glass plate is placed in a tempering furnace and heated to the tempering temperature, it is rapidly cooled and the protective liquid is sprayed evenly on both sides of the glass plate to obtain a protective layer. After cooling to room temperature, the wear-resistant tempered glass is obtained.
[0026] By adopting the above technical solution, the glass plate is first tempered, and then a protective layer is sprayed on the glass, thereby obtaining tempered glass with good wear resistance.
[0027] In summary, this application has the following beneficial effects:
[0028] 1. The present application sprays a protective layer on the side of the glass plate, and the protective layer is evenly coated on the surface of the glass plate to form a hierarchical structure, so that the tempered glass has good wear resistance. Glass fiber is added to the protective layer to significantly improve the strength and stiffness of the protective layer. Butyl acetate is mixed with the modified PMMA resin as a solvent. The present application modifies the PMMA resin to improve the wear resistance of the PMMA resin, which originally has poor wear resistance. The protective layer is prepared by compounding various modified components, and the protective layer is sprayed on the tempered glass, which further improves the wear resistance of the glass.
[0029] 2. In the present application, by modifying the PMMA resin, the hollow glass microspheres can form a uniform pore structure in the PMMA resin, effectively reducing the density of the material, forming a chemical bond between hydroxypropyltriethoxysilane and the PMMA resin, improving the compatibility and interfacial adhesion between the two, thereby improving the mechanical properties and weather resistance of the PMMA resin. At the same time, tetraethyl orthosilicate forms a silica network structure in the component, which can form an interpenetrating network with the PMMA resin, enhancing the hardness of the PMMA resin, thereby improving the wear resistance and weather resistance of the protective layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the overall structure of an embodiment of the present application.
[0031] Description of reference numerals:
[0032] 1. Glass plate; 2. Protective layer. DETAILED DESCRIPTION
[0033] The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0034] Example
[0035] Example 1
[0036] A method for preparing wear-resistant tempered glass comprises the following steps:
[0037] S1. 30kg modified PMMA resin, 10kg glass fiber, 2kg plasticizer and 40kg butyl acetate were stirred at a temperature of 60°C and a speed of 80r / min for 60min, and then 1kg leveling agent and 1kg dispersant were added and heated to 70°C and stirred for 30min to obtain a protective liquid;
[0038] S2. Reference Figure 1, put the glass plate 1 into a tempering furnace for heating, control the tempering temperature at 650℃, take it out after heating for 2 minutes, put the glass plate 1 into a quenching chamber for rapid cooling, and when the temperature drops to 200℃, spray the protective liquid evenly on both sides of the flat glass 1 to obtain a protective layer 2, and after the glass plate 1 is naturally cooled to room temperature, a tempered glass with high impact strength is obtained; the thickness of the glass plate 1 of the present application is 10mm. The plasticizer is chlorinated paraffin, the dispersant is polyacrylate ammonium (Guangdong Wengjiang reagent, model PC04931), and the leveling agent is TEGO-4500.
[0039] The preparation method of the modified PMMA resin is as follows: 20 kg PMMA resin, 5 kg hydroxypropyl triethoxysilane, 5 kg hollow glass microspheres, 2 kg tetraethyl orthosilicate and 1 kg dibutyltin dilaurate are mixed and stirred at 60°C for 10 min, then filtered under reduced pressure, transferred to an oven, and dried at 90°C for 2 h to obtain the modified PMMA resin. The particle size of the hollow glass microspheres is 110 nm.
[0040] Example 2
[0041] A method for preparing wear-resistant tempered glass comprises the following steps:
[0042] S1. 30kg modified PMMA resin, 10kg glass fiber, 2kg plasticizer and 40kg butyl acetate were stirred at a temperature of 60°C and a speed of 80r / min for 60min, and then 1kg leveling agent and 1kg dispersant were added and heated to 70°C and stirred for 30min to obtain a protective liquid;
[0043] S2. Reference Figure 1 , put the glass plate 1 into a tempering furnace for heating, control the tempering temperature at 650℃, take it out after heating for 2 minutes, put the glass plate 1 into a quenching chamber for rapid cooling, and when the temperature drops to 200℃, spray the protective liquid evenly on both sides of the flat glass 1 to obtain a protective layer 2, and after the glass plate 1 is naturally cooled to room temperature, a tempered glass with high impact strength is obtained; the thickness of the glass plate 1 of the present application is 10mm. The plasticizer is trimethyl phosphate, the dispersant is polyacrylate ammonium (Guangdong Wengjiang reagent, model PC04931), and the leveling agent is TEGO-4500.
[0044] The preparation method of the modified PMMA resin is as follows: 20 kg PMMA resin, 5 kg hydroxypropyl triethoxysilane, 5 kg hollow glass microspheres, 2 kg tetraethyl orthosilicate and 1 kg dibutyltin dilaurate are mixed and stirred at a temperature of 60°C for 10 minutes, and then filtered under reduced pressure, transferred to an oven, and dried at a temperature of 90°C for 2 hours to obtain the modified PMMA resin. The particle size of the hollow glass microspheres is 250 nm.
[0045] Example 3
[0046] A method for preparing wear-resistant tempered glass comprises the following steps:
[0047] S1. 30kg modified PMMA resin, 10kg glass fiber, 2kg plasticizer and 40kg butyl acetate were stirred at a temperature of 60°C and a speed of 80r / min for 60min, and then 1kg leveling agent and 1kg dispersant were added and heated to 70°C and stirred for 30min to obtain a protective liquid;
[0048] S2. Reference Figure 1 , put the glass plate 1 into a tempering furnace for heating, control the tempering temperature at 650℃, take it out after heating for 2 minutes, put the glass plate 1 into a quenching chamber for rapid cooling, and when the temperature drops to 200℃, spray the protective liquid evenly on both sides of the flat glass 1 to obtain a protective layer 2, and after the glass plate 1 is naturally cooled to room temperature, a tempered glass with high impact strength is obtained; the thickness of the glass plate 1 of the present application is 10mm. The plasticizer is dioctyl phthalate, the dispersant is polyacrylate ammonium (Guangdong Wengjiang reagent, model PC04931), and the leveling agent is TEGO-4500.
[0049] The preparation method of the modified PMMA resin is as follows: 20 kg PMMA resin, 5 kg hydroxypropyl triethoxysilane, 5 kg hollow glass microspheres, 2 kg tetraethyl orthosilicate and 1 kg dibutyltin dilaurate are mixed and stirred at a temperature of 60°C for 10 minutes, and then filtered under reduced pressure, transferred to an oven, and dried at a temperature of 90°C for 2 hours to obtain the modified PMMA resin. The particle size of the hollow glass microspheres is 200 nm.
[0050] Example 4
[0051] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that: the preparation method of modified PMMA resin is: 40kg PMMA resin, 10kg hydroxypropyl triethoxysilane, 10kg hollow glass microspheres, 6kg tetraethyl orthosilicate and 2kg dibutyltin dilaurate are mixed and stirred at a temperature of 60°C for 10 minutes, then filtered under reduced pressure, transferred to an oven, and dried at a temperature of 90°C for 2 hours to obtain the modified PMMA resin.
[0052] Example 5
[0053] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that: in the process of preparing the modified PMMA resin, the input amount of PMMA resin is 25 kg, the input amount of hydroxypropyltriethoxysilane is 6 kg, and the input amount of hollow glass microspheres is 6 kg.
[0054] Example 6
[0055] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that: in the process of preparing the modified PMMA resin, the input amount of PMMA resin is 25 kg, the input amount of hydroxypropyltriethoxysilane is 7 kg, and the input amount of hollow glass microspheres is 8 kg.
[0056] Example 7
[0057] A method for preparing wear-resistant tempered glass, which is different from Example 6 in that: an equal amount of hollow glass microspheres are replaced with modified hollow glass microspheres, and the preparation method of the modified hollow glass microspheres is as follows: 10 kg of hollow glass microspheres, 2 kg of n-butanol, 5 kg of ethylene glycol monobutyl ether and 5 kg of cyclohexanone are mixed, 1 kg of sodium hexametaphosphate, 1 kg of zirconium sulfate and 2 kg of sodium aluminate are added in sequence, heated to 80 ° C and stirred for 30 min, washed and transferred to an oven, dried at 100 ° C for 2 h, and crushed to obtain modified hollow glass microspheres.
[0058] Example 8
[0059] A method for preparing wear-resistant tempered glass, which is different from Example 6 in that: hollow glass microspheres are replaced with modified hollow glass microspheres in equal amounts, and the preparation method of the modified hollow glass microspheres is as follows: 20 kg of hollow glass microspheres, 8 kg of n-butanol, 10 kg of ethylene glycol monobutyl ether and 10 kg of cyclohexanone are mixed, 3 kg of sodium hexametaphosphate, 5 kg of zirconium sulfate and 8 kg of sodium aluminate are added in sequence, heated to 80 ° C and stirred for 30 min, washed and transferred to an oven, dried at 100 ° C for 2 h, and crushed to obtain modified hollow glass microspheres.
[0060] Example 9
[0061] A method for preparing wear-resistant tempered glass, which is different from Example 8 in that the input amount of hollow glass microspheres is 15 kg, the input amount of sodium hexametaphosphate is 1.5 kg, the input amount of zirconium sulfate is 3.6 kg, and the input amount of sodium aluminate is 3 kg.
[0062] Example 10
[0063] A method for preparing wear-resistant tempered glass, which is different from Example 8 in that the input amount of hollow glass microspheres is 15 kg, the input amount of sodium hexametaphosphate is 2.1 kg, the input amount of zirconium sulfate is 4.5 kg, and the input amount of sodium aluminate is 6 kg.
[0064] Embodiment 11
[0065] A method for preparing wear-resistant tempered glass, which is different from Example 10 in that the input amount of modified PMMA resin is 40 kg, the input amount of dioctyl phthalate is 4.8 kg, and the input amount of glass fiber is 16 kg.
[0066] Example 12
[0067] A method for preparing wear-resistant tempered glass, which is different from Example 10 in that the input amount of modified PMMA resin is 40 kg, the input amount of dioctyl phthalate is 6 kg, and the input amount of glass fiber is 18 kg.
[0068] Comparative Example
[0069] Comparative Example 1
[0070] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that an equal amount of modified PMMA resin is replaced by PMMA resin.
[0071] Comparative Example 2
[0072] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that an equal amount of modified PMMA resin is replaced by epoxy resin.
[0073] Comparative Example 3
[0074] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that an equal amount of modified PMMA resin is replaced by polyurethane resin.
[0075] Comparative Example 4
[0076] A method for preparing wear-resistant tempered glass, which is different from Example 3 in that an equal amount of glass fiber is replaced by titanium dioxide.
[0077] Performance testing:
[0078] Light transmittance test: The wear-resistant tempered glass prepared in Examples 1-12 and Comparative Examples 1-4 was tested according to GB / T 40415-2021 “Light transmittance test method for photovoltaic glass assemblies for use in buildings”.
[0079] Abrasion resistance test: The abrasion-resistant tempered glasses prepared in Examples 1-12 and Comparative Examples 1-4 were tested according to GB / T6739-2006.
[0080] Acid resistance: According to GB / T7962.14-1987 "Test method for acid resistance of colorless optical glass", the acid resistance of the tempered glass prepared in Examples 1-17 and Comparative Examples 1-4 was tested.
[0081] Light transmittance (%) hardness Acid resistance Example 1 89.7 5H Level 3 Example 2 89.3 5H Level 3 Example 3 90.1 5H Level 3 Example 4 90.2 5H Level 3 Example 5 91.8 6H Level 3 Example 6 92.1 6H Level 3 Example 7 93.4 7H Level 2 Example 8 93.2 7H Level 2 Example 9 93.7 8H Level 1 Example 10 93.8 8H Level 1 Embodiment 11 96.1 8H Level 1 Example 12 96.4 8H Level 1 Comparative Example 1 86.8 2H Level 3 Comparative Example 2 86.1 4H Level 3 Comparative Example 3 87.5 3H Level 3 Comparative Example 4 82.8 4H Level 3
[0082] According to the data comparison of Examples 1-4 and Comparative Examples 1-4, the present application sprays a protective layer on the side of the glass plate, and the protective layer is evenly coated on the surface of the glass plate to form a hierarchical structure, so that the tempered glass has good wear resistance. The addition of glass fiber to the protective layer significantly improves the strength and stiffness of the protective layer. Butyl acetate is mixed with the modified PMMA resin as a solvent. The present application modifies the PMMA resin, so that the wear resistance of the PMMA resin with originally poor wear resistance is improved. The protective layer prepared by compounding various modified components is sprayed on the tempered glass, which further improves the wear resistance of the glass.
[0083] According to the data comparison of Examples 3-6, it can be obtained that when the PMMA resin, hydroxypropyl triethoxysilane and hollow glass microspheres are in a specific weight ratio, hydroxypropyl triethoxysilane can form hydrogen bonds with the carbonyl groups in PMMA to enhance the interaction between the two. At the same time, the silanol groups in hydroxypropyl triethoxysilane can combine with the hollow glass microspheres to make the hollow glass microspheres play a skeleton role in the PMMA resin. The three together form a three-dimensional network structure to further enhance the mechanical properties of the PMMA resin, so that the modified PMMA resin can act on the tempered glass to improve the wear resistance of the tempered glass.
[0084] According to the data comparison of Examples 6-8, the present application modifies the hollow glass microspheres, and sodium hexametaphosphate and zirconium sulfate are mixed to form a zirconium-phosphate complex. Sodium aluminate, as a strong base and weak acid salt, can undergo a hydrolysis reaction and combine with the metal ions in the components. Sodium hexametaphosphate, zirconium sulfate and sodium aluminate are mixed and then mixed with the hollow glass microspheres, which can improve the overall performance of the hollow glass microspheres, improve the stability of the hollow glass microspheres, further improve the skeleton mechanical properties in PMMA resin, and thus improve the wear resistance and mechanical properties of tempered glass.
[0085] According to the data comparison of Examples 8-10, it can be obtained that when the hollow glass microspheres, sodium hexametaphosphate, zirconium sulfate and sodium aluminate are in a specific weight ratio, the four cooperate together to form a complex on the surface of the hollow glass microspheres, so that the hollow glass microspheres can be better dispersed in the PMMA resin after modification, further improving the impact resistance and wear resistance of the PMMA resin, thereby improving the wear resistance of the protective layer sprayed on the surface of the glass plate.
[0086] According to the data comparison of Examples 10-12, when the modified PMMA resin, dioctyl phthalate and glass fiber are in a specific weight ratio, dioctyl phthalate combines the glass fiber with the modified PMMA resin, improves the wear resistance and weather resistance of the modified PMMA resin, and is sprayed on the glass surface to form a protective layer, further improving the acid resistance of the glass plate.
[0087] The specific embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A wear-resistant tempered glass, characterized in that: It comprises a glass plate (1) and a protective layer (2); the protective layer (2) is bonded to the glass plate (1); the protective layer (2) is made of the following raw materials in parts by weight: 30-60 parts of modified PMMA resin; 10-20 parts of glass fiber; 2-7 parts of plasticizer; 1-2 parts of leveling agent; 40-60 parts of butyl acetate; 1-3 parts of dispersant; the modified PMMA resin comprises the following raw materials: PMMA resin, hydroxypropyl triethoxysilane, hollow glass microspheres, tetraethyl orthosilicate and dibutyltin dilaurate; the preparation method of the modified PMMA resin is: 20-40 parts by weight of PMMA resin, 5-10 parts by weight of hydroxypropyl triethoxysilane, 5-10 parts by weight of hollow glass microspheres, 2-6 parts by weight of tetraethyl orthosilicate and 1-2 parts by weight of dibutyltin dilaurate are mixed and stirred, and then dried to obtain the modified PMMA resin.
2. The wear-resistant tempered glass according to claim 1, characterized in that: The weight ratio of the PMMA resin, hydroxypropyltriethoxysilane and hollow glass microspheres is 1: (0.24-0.28): (0.24-0.32).
3. The wear-resistant tempered glass according to claim 1, characterized in that: The hollow glass microspheres are modified hollow glass microspheres. The preparation method of the modified hollow glass microspheres is as follows: 10-20 parts by weight of hollow glass microspheres, 2-8 parts by weight of n-butanol, 5-10 parts by weight of ethylene glycol monobutyl ether and 5-10 parts by weight of cyclohexanone are mixed, 1-3 parts by weight of sodium hexametaphosphate, 1-5 parts by weight of zirconium sulfate and 2-8 parts by weight of sodium metaaluminate are added in sequence, heated and stirred, and the modified hollow glass microspheres are obtained after washing, drying and crushing.
4. The wear-resistant tempered glass according to claim 3, characterized in that: The weight ratio of the hollow glass microspheres, sodium hexametaphosphate, zirconium sulfate and sodium aluminate is 1: (0.1-0.14): (0.24-0.3): (0.2-0.4).
5. The wear-resistant tempered glass according to claim 3, characterized in that: The particle size of the hollow glass microspheres is 110-250 nm.
6. The wear-resistant tempered glass according to claim 1, characterized in that: The plasticizer includes one of dioctyl phthalate, trimethyl phosphate and chlorinated paraffin.
7. The wear-resistant tempered glass according to claim 1, characterized in that: The weight ratio of the modified PMMA resin, dioctyl phthalate and glass fiber is 1: (0.12-0.15): (0.4-0.45).
8. The wear-resistant tempered glass according to claim 1, characterized in that: The dispersant includes one of ammonium polyacrylate and stearic acid monoglyceride.
9. A method for preparing wear-resistant tempered glass, characterized in that: The method for preparing the wear-resistant tempered glass according to any one of claims 1 to 8 comprises the following steps: S1. After the modified PMMA resin, glass fiber, plasticizer and butyl acetate are uniformly stirred, a leveling agent and a dispersant are added and heated and stirred to obtain a protective liquid; S2. The glass plate (1) is placed in a tempering furnace and heated to a tempering temperature, then rapidly cooled and the protective liquid is sprayed evenly on both sides of the glass plate (1) to obtain a protective layer (2), and the wear-resistant tempered glass is obtained after cooling to room temperature.
Citation Information
Patent Citations
Double-component glass thermal insulation coating and preparation method thereof
CN108410353A
Tempered film and preparation method thereof
CN111253871A
Toughened glass with high impact strength and preparation method thereof
CN115851091A
Lightweight heat-insulation self-leveling floor coating
CN117363172A
Rigid surface covering plastic material
US20170152666A1