A gypsum material additive, an inorganic nano-gypsum composite material and a preparation method thereof
The bubble structure is adjusted by the composition in the gypsum material additives to improve the freezing durability and compressive strength of the gypsum material, and the problem of compressive strength attenuation under the freeze-thaw cycle in the prior art is solved, and the resistance to comply with national standards is achieved Freezing performance and multifunctional performance.
Patent Information
- Application Number
- CN202411002690.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing gypsum foaming materials have severe tensile and compressive strength attenuation under the freeze-thaw cycle in cold areas, making it difficult to meet the freezing and durability requirements of building walls.
Using a gypsum material additive, the number, size and wall thickness of the bubbles of the gypsum material are adjusted by combining the first composition and the second composition, the stability of the bubble body structure is enhanced, the durability of the frost resistance is improved, and polyoxidation is used. Ethylene, triethanolamine, potassium aluminum sulfate dodecanoate and other components improve compressive strength and waterproofing function.
It realizes that the gypsum material is not damaged after 15 freeze-thaw cycles and maintains compressive strength, complies with national standards, has excellent mechanical properties, thermal insulation effect, fire, sound insulation and moisture-proof functions, and is suitable for external insulation materials for building walls. .
Smart Images

Figure CN118529968B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a gypsum material additive, an inorganic nano-gypsum composite material and a preparation method thereof. Background Art
[0002] The durability of building materials has become a focus of attention in the engineering community, especially in cold areas. Damage and deterioration caused by freeze-thaw cycles will affect the durability of the structure. Therefore, the "Autoclaved Aerated Concrete Block" (GB / T11968-2020) requires that the strength loss is less than 20% after 15 freeze-thaw cycles.
[0003] The development of lightweight, high-strength, porous inorganic thermal insulation materials using gypsum (natural gypsum, solid waste gypsum) as raw materials is a very promising direction. At present, the method and process of gypsum foaming materials are simple. Generally, foaming is achieved by adding a foaming agent to the gypsum and then reacting and expanding it. Since the introduced bubbles increase the interface of the gypsum slurry, the system is prone to an unstable state, which directly affects the performance of the gypsum foaming material. Freeze-thaw has a great influence on the tensile and compressive strength of gypsum foaming materials. With the increase of the number of freeze-thaw cycles, the degree of attenuation of tensile and compressive strength increases.
[0004] Based on this, the present invention aims to study a gypsum material additive, which is applied to gypsum foaming to make its structure have better frost resistance and increase the frost resistance durability of the gypsum material to meet the application requirements of building walls, internal and external insulation materials, especially the requirements of exterior walls. Summary of the invention
[0005] In view of the above-mentioned technical problems and the deficiencies in the art, the present invention provides a gypsum material additive, a gypsum material additive. The present invention adjusts the structure of the gypsum material through the gypsum material additive of the formula, enhances the stability of the foam structure, and achieves good antifreeze durability. After 15 freeze-thaw cycle tests, the specimen is not damaged and still has compressive strength after freeze-thaw; the gypsum foaming additive can adjust the size, number, and wall thickness of the bubbles in the gypsum material to meet the requirements of specific application fields. The prepared gypsum material has excellent mechanical properties, a compressive strength of up to 9MPa, and also has good thermal insulation effect, and has fire prevention, sound insulation, and moisture-proof functions. The process is simple, green, and environmentally friendly.
[0006] The object of the present invention is to provide a gypsum material additive, comprising a first composition and a second composition, wherein the first composition comprises polyethylene oxide, triethanolamine, potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, sodium molybdate, pentaerythritol, silicone amide, nanocellulose ether, anhydrous calcium chloride, dimethyl silicone oil and water; and the second composition comprises hydrogen peroxide, polyanionic cellulose, polyethylene glycol, dimethyl siloxane and water.
[0007] The polyethylene oxide and triethanolamine of the present invention are mainly used as film-forming substances of the foam, which can fully improve the compressive strength of the inorganic foamed gypsum material, and triethanolamine has the function of stabilizing the foam structure, and obtains the mutually unconnected foam tissue through silicone amide, and controls the number and size of the foam with nanocellulose ether; potassium aluminum sulfate dodecahydrate mainly acts to enhance the waterproof function, and at the same time has the function of enhancing the compressive strength; hydroxyethylidene diphosphonic acid has a stable structure and is not easy to hydrolyze; anhydrous calcium chloride enables the inorganic foamed gypsum composite material to maintain acid-base balance and increase the density of the foam wall. The present invention adjusts the structure of the gypsum material through the gypsum material additive of the formula, and enhances the stability of the foam structure, achieves good antifreeze durability, and the test piece is not damaged after 15 freeze-thaw cycle tests and still has compressive strength after freeze-thaw.
[0008] The present invention controls the number and size of the bubbles by adjusting the amount of the first composition, and controls the wall thickness and overall strength of the bubbles by adjusting the amount of the second composition, so that the number, size and wall thickness of the bubbles in the gypsum material are controllable, and the specific requirements of different application fields for gypsum materials can be met. The inorganic nano gypsum material prepared by the present invention has excellent mechanical properties and thermal insulation properties, the compressive strength can reach 9MPa, and the thermal conductivity can be as low as 0.02W / m·K.
[0009] Further, the first composition includes the following components in percentage by weight:
[0010] Polyethylene oxide 1-25%
[0011] Triethanolamine 10-25%
[0012] Potassium aluminum sulfate dodecahydrate 10-20%
[0013] Hydroxyethylidene diphosphonic acid 10-15%
[0014] Sodium pyrophosphate 10-15%
[0015] Sodium molybdate 0.1-0.5%
[0016] Pentaerythritol 5-10%
[0017] Silicone amide 1-10%
[0018] Nanocellulose ether 5-10%
[0019] Anhydrous calcium chloride 1-5%
[0020] Dimethyl silicone oil 0.01-0.2%
[0021] The balance is water;
[0022] The second composition includes the following components in percentage by weight:
[0023] Hydrogen peroxide 10-50%
[0024] Polyanionic cellulose 10-25%
[0025] Polyethylene glycol 1-20%
[0026] Dimethicone 1-2%
[0027] The balance is water.
[0028] Furthermore, the molecular weight of polyethylene oxide is 50,000-150,000.
[0029] Furthermore, the molecular weight of the nanocellulose ether is 5,000-20,000.
[0030] The present invention also aims to provide an inorganic nano-gypsum material, comprising gypsum powder, magnesium sulfate heptahydrate, gypsum material additives and water.
[0031] Furthermore, the inorganic nano-gypsum material comprises the following components in parts by weight:
[0032] The mass fraction of the gypsum powder is 50-80 parts;
[0033] The mass fraction of the magnesium sulfate heptahydrate is 1-25 parts;
[0034] The mass fraction of the first composition is 1-10 parts;
[0035] The mass fraction of the second composition is 1-10 parts;
[0036] The mass fraction of the water is 1-50 parts.
[0037] The present invention also aims to provide a method for preparing an inorganic nano-gypsum material, comprising the steps of:
[0038] (1) Preparation of the first composition:
[0039] A. Weigh each component according to the ratio, add water into the reaction container, add sodium molybdate, disperse and mix evenly, add polyethylene oxide, and disperse and mix evenly after the polyethylene oxide is completely wetted;
[0040] B. Add nanocellulose ether, triethanolamine, silicone amide and pentaerythritol, and disperse and mix them evenly;
[0041] C. adding potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, anhydrous calcium chloride and dimethyl silicone oil, dispersing and mixing evenly to obtain a first composition;
[0042] (2) Preparation of the second composition:
[0043] Weigh each component according to the ratio, add water into the reaction device, add hydrogen peroxide, polyanionic cellulose, polyethylene glycol, and dimethylsiloxane, disperse and mix evenly to obtain a second composition;
[0044] (3) Weighing gypsum powder, water, magnesium sulfate heptahydrate, the first composition, and the second composition according to the proportion;
[0045] (4) Dispersing and mixing the weighed water, magnesium sulfate heptahydrate and the first composition uniformly;
[0046] (5) Add gypsum powder and disperse and mix evenly;
[0047] (6) Add the second composition, disperse and mix evenly to obtain an inorganic nano-gypsum material.
[0048] The present invention disperses and mixes the components of the first composition in a gypsum system first, and then adds the second composition into the mixture system of gypsum and the first composition, so that during the foaming process of the second composition, the first composition can better act on the foams, control the number and size of the foams, and stabilize the structure and function of the foams, and then the wall thickness and overall strength of the foams can be controlled by the second composition.
[0049] Furthermore, in the preparation of the first composition in step (1): the first dispersing stirring speed of step A is 1300-1600 r / min, and the dispersing stirring time is 50-65 min; the second dispersing stirring speed of step B is 1300-1600 r / min, and the dispersing stirring time is 15-45 min; the third dispersing stirring speed of step C is 1300-1600 r / min, and the dispersing stirring time is 15-45 min.
[0050] Furthermore, in the preparation of the second composition in step (2), the dispersion stirring speed is 600-1200 r / min, and the dispersion stirring time is 15-45 min.
[0051] Furthermore, in step (4), the dispersion stirring speed is 100-500 r / min, and the dispersion stirring time is 0.1-10 min; in step (5), the dispersion stirring speed is 500-1500 r / min, and the dispersion stirring time is 0.1-10 min; in step (6), the dispersion and mixing are uniform, and the dispersion stirring time is 0.1-10 min.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] (1) The present invention combines the first composition and the second composition to provide the gypsum material with a water-blocking function, thereby preventing a large amount of water molecules from entering the interior of the gypsum material foam. At the same time, the wall thickness density of the foam wall is increased to make the foam more solid and airtight to prevent the penetration of water molecules, thereby making the foam structure more stable and preventing the foam from being squeezed and deformed due to the expansion force and contraction force generated by the alternation of cold and hot (-15°C to 105°C). This greatly improves the frost resistance and durability of the gypsum material of the present invention, and achieves a strength loss rate of less than 20% after 15 freeze-thaw cycles, which meets the requirements of the national standard "Autoclaved Aerated Concrete Block" (GB / T 11968-2020) for frost resistance, and can be used as building walls, internal and external insulation materials, especially exterior walls;
[0054] (2) The present invention adjusts the number, size, and wall thickness of bubbles in gypsum foaming by using the first composition and the second composition. The number and size of the bubbles are controlled by adjusting the amount of the first composition added, and the wall thickness and overall strength of the bubbles are controlled by adjusting the amount of the second composition added. The pore density, size, and wall thickness of the gypsum material can be flexibly controlled to meet the specific requirements of different fields for foaming materials.
[0055] (3) The polyethylene oxide and triethanolamine used in the present invention are mainly used as film-forming substances for the foamed body, which fully improve the compressive strength of the inorganic foamed gypsum material. The polyanionic cellulose is used to adjust the number of foams according to the amount of polyanionic cellulose added to enhance the compressive strength. The wall thickness of the foams that are not interconnected in the inorganic gypsum composite material is adjusted together with materials such as hydrogen peroxide. The magnesium sulfate heptahydrate not only has a foaming catalytic effect in the inorganic gypsum composite material, but also improves the hardness of the inorganic gypsum composite material. The prepared foamed gypsum material is a lightweight and high-strength material with good mechanical strength, and the compressive strength can reach 9MPa.
[0056] (4) Compared with ordinary gypsum materials, the inorganic gypsum composite material prepared by the present invention has light weight, convenient construction, can be used for heat preservation, has good heat preservation and sound insulation effects, and the thermal conductivity can be as low as 0.02W / m·K. The sound insulation and noise reduction test reaches 45dB. It has a certain protective effect (shielding effect) on some low-frequency electromagnetic waves (such as power line radiation). Other protective materials (such as metal) can also be added to achieve high-frequency electromagnetic radiation shielding. Gypsum, as a porous material, has high water absorption and water permeability. The material prepared by the present application enhances the waterproof and moisture-proof properties, and the water absorption rate is reduced to 5%;
[0057] (5) The crystal structure contained in the material of the present invention has high stability, which enables it to withstand high temperatures up to 1700°C. Its fire prevention is achieved by absorbing heat. When a fire occurs, the gypsum composite material can absorb heat energy, reduce the ambient temperature, and delay the spread of the fire. The fire prevention level is A1. In terms of fire extinguishing function, the inorganic gypsum composite material is an A1 non-combustible material. The product is heat-insulating and flame-retardant, and is a poor conductor of heat. During a fire, less heat is transferred to the back-fire surface, and its equilibrium temperature is low. It can avoid ignition or ignition of other objects due to the increase in the back-fire surface temperature for a long time. Even if the inorganic gypsum composite material faces the fire at a high temperature for 3.5 hours, the temperature of the back-fire side will not exceed 50°C, which effectively plays a role in fire insulation and flame retardancy. The foamed gypsum product of the present application is resistant to high temperature, heat insulation and fire prevention, does not catch fire, does not smolder, and does not carbonize. It is an A1-level fireproof material and can be widely used in the protective layer of the internal and external insulation system of various high-rise residential buildings and other civil buildings. In addition, the gypsum filler foamed with this additive has the effects of corrosion resistance, high temperature resistance, easy construction, and fireproof and heat insulation compartments, which can improve the corrosion resistance of the material, so that the gypsum product can maintain better stability under continuous high temperature and extend the service life;
[0058] (6) Compared with organic high temperature resistant fillers, the gypsum of the present invention is directly taken from nature and waste, and is a non-toxic, green and environmentally friendly inorganic raw material. The production and use of inorganic materials cause less pollution to the environment. The product uses water as a dispersion medium and has no adverse effects on environmental protection and health. In the event of a fire, the inorganic gypsum composite material only releases crystal water and converts it into water vapor. It will not produce any toxic suffocating combustion gases, nor will it volatilize any decomposed or combustion-supporting substances and smoke, which can also reduce casualties when a fire occurs. The gypsum material of the present invention has the advantages of being green, environmentally friendly, and natural and non-toxic;
[0059] (7) The gypsum composite material of the present invention has waterproof and moisture-proof properties. Gypsum is a porous material with high water absorption and water permeability. Therefore, at room temperature, gypsum is not waterproof and moisture-proof. However, the gypsum composite material of the present invention has waterproof and moisture-proof properties, which further expands the scope of use of gypsum;
[0060] (8) The gypsum composite material of the present invention has recyclability. The present invention uses only inorganic raw materials to foam gypsum, thereby obtaining high compressive strength and excellent frost resistance. In this process, no concrete or similar gel materials are added, and pure gypsum is used for foaming. Therefore, the present invention has good recyclability. The gypsum products produced by the present invention can be completely recycled and reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 It is a comparison diagram of the preparation of gypsum materials in Example 1 of the present invention and Comparative Example 1.
[0062] Among them, 1 is the gypsum composite material prepared in Example 1 of the present invention; 2 is the gypsum material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0063] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] Example 1
[0065] 1. Preparation of gypsum material additives
[0066] 1. Preparation of the first composition
[0067] Step A: Weigh by mass percentage: 38.7% water, 0.25% sodium molybdate, 2% polyethylene oxide (molecular weight 100,000), 5% nanocellulose ether (molecular weight 10,000), 15% triethanolamine, 5% pentaerythritol, 0.05% dimethyl silicone oil, 2% anhydrous calcium chloride, 2% silicone amide, 10% sodium pyrophosphate, 10% hydroxyethylidene diphosphonic acid, and 10% potassium aluminum sulfate dodecahydrate.
[0068] First, add a certain amount of water to the reactor, set the reactor temperature to 70°C, set the initial disperser speed to 500r / min, add sodium molybdate, set the disperser speed to 1500 r / min, wait for the reaction temperature to reach the set value of 70°C, and disperse for 10 minutes. Adjust the reactor temperature to 25°C, reduce the disperser speed to 500r / min, and then add polyethylene oxide. After the polyethylene oxide is fully wetted, increase the disperser speed (called the first disperser stirring speed) to 1500r / min, and the dispersion time is 60 minutes.
[0069] Step B: Then the speed of the dispersing mixer is set to 500 r / min, and the nanocellulose ether, triethanolamine, silicone amide, and pentaerythritol are added in sequence, and the speed of the dispersing mixer (called the second dispersing stirring speed) is increased to 1500 r / min, and the dispersing time is 30 minutes;
[0070] Step C: Finally, the disperser speed is set to 650 r / min, and potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, anhydrous calcium chloride, and dimethyl silicone oil are added in sequence, and the disperser speed (called the third disperser stirring speed) is set to 1500 r / min. Disperse for 20 minutes, close the reactor, and cool to room temperature to obtain the first composition.
[0071] Polyethylene oxide and triethanolamine are mainly used as film-forming substances for foams, which can fully improve the compressive strength of inorganic foamed gypsum materials and prevent the product from falling off after solidification. Triethanolamine has the functions of adjusting construction viscosity, pH value, reducing water, and stabilizing foam structure. Silicone amide and nanocellulose ether can control the number and size of foams; hydroxyethylidene diphosphonic acid can effectively inhibit the catalytic decomposition of hydrogen peroxide caused by metal ions. Sodium pyrophosphate mainly acts as a hydrogen peroxide stabilizer and can improve the strength of inorganic gypsum composite materials; pentaerythritol mainly acts as a surfactant, adhesive, and flame retardant; sodium molybdate is used as a foaming catalyst and corrosion inhibitor for metal materials to play an anti-corrosion role; anhydrous calcium chloride enables the inorganic foamed gypsum composite material to maintain acid-base balance and increase the density of the foam wall; dimethyl silicone oil is mainly used for penetration and defoaming.
[0072] 2. Preparation of the Second Composition
[0073] Weighed by mass percentage: 50% water, 10% polyanionic cellulose, 35% hydrogen peroxide, 3% polyethylene glycol and 2% dimethylsiloxane.
[0074] Water was added to the reaction kettle, the initial disperser speed was set to 650 r / min, hydrogen peroxide, polyanionic cellulose, polyethylene glycol, and dimethylsiloxane were added, and then the disperser speed was increased to 1000 r / min, and the mixture was dispersed for 20 minutes. After the reaction kettle was closed, the above-mentioned second composition was obtained.
[0075] The polyanionic cellulose in the second composition has heat stability and salt resistance, strong antibacterial properties, and does not mold or deteriorate. The number of foams is adjusted according to the amount of addition to enhance the compressive strength. Together with materials such as hydrogen peroxide, the inorganic gypsum composite material has the wall thickness of the foams that are not interconnected, and the compressive strength is adjusted to meet the specific needs of gypsum materials in different application fields. Polyethylene glycol is a surfactant that makes the inorganic foamed gypsum composite material have good lubrication, dispersion, and adhesion; dimethylsiloxane is mainly used to reduce surface tension and help lubrication and leveling.
[0076] 2. Preparation of gypsum composite materials
[0077] Weigh 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 1 part of the first composition, and 1 part of the second composition according to their mass fractions.
[0078] Add the first composition and magnesium sulfate heptahydrate to the weighed water and mix them evenly with a mixer or disperser at a speed of 180r / min; add gypsum powder after about 1 minute and disperse it with a mixer or disperser at a speed of 1000r / min to make the gypsum powder and solution fully mixed; add the second composition after mixing for 2 minutes, pour it into the mold or filling product after dispersing for 1 minute, and cure to obtain the inorganic nano foaming composite material. The gypsum composite material prepared by this formula has a foaming ratio of 2 times, and its density is measured to be 800.5kg / m 3 , thermal conductivity is 0.095W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0079] Example 2
[0080] According to the weight percentage, 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 1 part of the first composition, and 2 parts of the second composition were weighed, and the preparation process was the same as that of Example 1. The gypsum composite material prepared by this formula had a foaming ratio of 4 times, and its density was measured to be 650.6 kg / m 3 , thermal conductivity is 0.068W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0081] Example 3
[0082] According to the weight percentage, 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 2 parts of the first composition, and 1 part of the second composition were weighed, and the preparation process was the same as that of Example 1. The gypsum composite material prepared by this formula had a foaming ratio of 2.2 times, and its density was measured to be 750.8 kg / m 3 The thermal conductivity is 0.073W / m·K, the sound insulation and noise reduction test reaches 31-45dB, and the fire protection performance test reaches A1 level fire protection.
[0083] Example 4
[0084] According to the weight percentage, 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 3 parts of the first composition, and 3 parts of the second composition were weighed, and the preparation process was the same as that of Example 1. The gypsum composite material prepared by this formula had a foaming ratio of 4 times, and its density was measured to be 350.7 kg / m 3 , thermal conductivity is 0.051W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0085] Example 5
[0086] According to the weight percentage, 50 parts of gypsum powder, 1.6 parts of magnesium sulfate heptahydrate, 32 parts of water, 3 parts of the first composition, and 6 parts of the second composition were weighed, and the preparation process was the same as that of Example 1. The gypsum composite material prepared by this formula had a foaming ratio of 30 times and a measured density of 80.2 kg / m 3 , thermal conductivity is 0.021W / m·K, sound insulation and noise reduction test reaches 31-45dB, and fire protection performance test reaches A1 level fire protection.
[0087] Comparative Example 1
[0088] 100 parts by mass of hemihydrate gypsum, 50 parts by mass of anhydrous gypsum, 0.05 parts by mass of polycarboxylic acid aqueous agent, 0.1 parts by mass of polyethylene oxide, 0.05 parts by mass of protein retarder for gypsum, and 0.06 parts by mass of starch ether are added into a dry mixer and mixed evenly; then 8 parts by mass of sodium alkylbenzene sulfonate, 0.5 parts by mass of polyacrylamide, and 300 parts by mass of water are mixed evenly to obtain a foaming liquid, and the foaming liquid is placed in a foaming machine for foaming to form foam for 4 minutes; then 100 parts by mass of water is added to the mixed dry powder and stirred to obtain a mixed slurry; then the mixed slurry is evenly mixed with the foam and put into a mold for final shaping. The density of the gypsum material prepared as above is measured to be 403.1 kg / m 3 .
[0089] Performance Tests of Examples 1-5 and Comparative Example 1
[0090] 1. Internal structure comparison:
[0091] The gypsum composite material obtained is as follows Figure 1 As shown, 1 is the gypsum composite material prepared in Example 1 of the present invention, and 2 is the gypsum material prepared in Comparative Example 1. As can be seen from the figure, the gypsum composite material prepared in Example 1 of the present invention has uniform, dense and relatively regular shaped foams, and the stable foam structure enables the gypsum composite material prepared in the present invention to have good antifreeze durability, while the conventional gypsum material prepared in Comparative Example 1, although it has a more substantial structure on the surface, basically does not have antifreeze durability.
[0092] 2. Freeze-thaw test:
[0093] Freeze-thaw test method (refer to the test experiment on frost resistance in "Test Method for Performance of Autoclaved Aerated Concrete" (GB / T 11969-2020)):
[0094] Freeze-thaw is to immerse the freeze-thaw specimen in a constant temperature water tank with a water temperature of (20±2)℃ for 48 hours. The water surface is at half the height of the freeze-thaw specimen for the first 24 hours, and the water surface is 30mm higher than the freeze-thaw specimen for the last 24 hours. Then take it out and put it in a sealed plastic bag and let it stand for 24 hours. Then put it in a low temperature box that has been cooled to (-15±2)℃ in advance. When the temperature drops to -15℃ again, record the time and keep it for no less than 8 hours before taking it out. The taken out freeze-thaw specimen is placed in a constant temperature and humidity box with a temperature of (20±2)℃ and a relative humidity of 95% and kept for no less than 6 hours. Freeze for 8 hours and thaw for 6 hours as one freeze-thaw cycle until the freeze-thaw specimen completes 15 freeze-thaw cycles. Place the freeze-thaw specimens after freeze-thaw in an electric forced air drying oven, keep them at (60±5)℃ for 24h, then keep them at (80±5)℃ for 24h, and then bake them at (105±5)℃ until constant quality. After sealing and cooling to room temperature, measure the compressive strength of the specimens.
[0095] The freeze-thaw test results are shown in the following table:
[0096]
[0097] The present invention adopts a combination of the first composition and the second composition, and the frost resistance is significantly improved compared with Comparative Example 1, and can pass 15 freeze-thaw tests. Comparative Example 1 softens directly after the first freeze-thaw. At the same time, Examples 1-5 can not only pass 15 freeze-thaw tests, but also have a strength loss rate of less than 20%, which meets the national standard "Autoclaved Aerated Concrete Blocks" (GB / T11968-2020) for frost resistance. The requirements, which shows that the gypsum material of the present invention has excellent frost resistance, and the gypsum material of Comparative Example 1 which does not use the first and second compositions of the present invention basically has no frost resistance.
[0098] It can be seen from the above examples 1-5 that to obtain gypsum products with the same performance, it can be achieved by adjusting the addition amounts of the first composition and the second composition. The strength, density, thermal conductivity, etc. of gypsum products made from the first composition and the second composition with different addition amounts are different and can be adjusted according to actual needs.
[0099] The ratio of the first composition and the second composition in Example 1 can thicken the bubble wall; the ratio of the two groups of compositions in Example 2 can make the bubble larger; the ratio of the two groups of compositions in Example 3 can enhance the overall strength of the bubble; the ratio of the two groups of compositions in Example 4 can increase the number of bubbles; the ratio of the two groups of compositions in Example 5 can increase the volume.
[0100] Therefore, the present invention uses the first composition and the second composition in combination, so that the gypsum material has a water-blocking function, preventing a large number of water molecules from entering the interior of the gypsum material foam. At the same time, the wall thickness density of the foam wall is increased to make the foam stronger and the foam has sealing properties to prevent the penetration of water molecules, so that the structure of the foam is more stable, so that it will not be squeezed and deformed due to the expansion force and contraction force generated by the alternation of hot and cold (-15°C to 105°C). The frost resistance and durability of the gypsum material of the present invention are greatly improved, and the strength loss rate of the gypsum product after 15 freeze-thaw cycles is less than 20%, which meets the requirements of the national standard "Autoclaved Aerated Concrete Block" (GB / T 11968-2020) for frost resistance, and can be used as a material for building walls, especially exterior walls.
[0101] The number, size and wall thickness of gypsum foaming bubbles are adjusted by the first composition and the second composition. The number and size of the foam bodies are controlled by adjusting the addition amount of the first composition. The wall thickness and overall strength of the foam bodies are controlled by adjusting the addition amount of the second composition. The pore density, size and wall thickness of the gypsum material can be flexibly controlled to meet the specific requirements of foaming materials in different fields.
[0102] The above embodiments are only used to illustrate the present invention, rather than to limit the present invention. Those skilled in the relevant technical field may make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions should also belong to the scope of the present invention and should be defined by the claims.
Claims
1. A gypsum material additive, characterized in that: The invention comprises a first composition and a second composition, wherein the first composition comprises the following components in percentage by weight: Polyethylene oxide 1-25% Triethanolamine 10-25% Potassium aluminum sulfate dodecahydrate 10-20% Hydroxyethylidene diphosphonic acid 10-15% Sodium pyrophosphate 10-15% Sodium molybdate 0.1-0.5% Pentaerythritol 5-10% Silicone amide 1-10% Nanocellulose ether 5-10% Anhydrous calcium chloride 1-5% Dimethyl silicone oil 0.01-0.2% The balance is water; The second composition includes the following components in percentage by weight: Hydrogen peroxide 10-50% Polyanionic cellulose 10-25% Polyethylene glycol 1-20% Dimethicone 1-2% The balance is water.
2. A gypsum material additive according to claim 1, characterized in that: The molecular weight of the polyethylene oxide is 50,000-150,000; the molecular weight of the nanocellulose ether is 5,000-20,000.
3. An inorganic nano-gypsum material, characterized in that: The invention comprises gypsum powder, magnesium sulfate heptahydrate, the gypsum material additive according to claim 1 or 2, and water.
4. An inorganic nano-gypsum material according to claim 3, characterized in that: The following components are included in parts by weight: The mass fraction of the gypsum powder is 50-80 parts; The mass fraction of the magnesium sulfate heptahydrate is 1-25 parts; The mass fraction of the first composition is 1-10 parts; The mass fraction of the second composition is 1-10 parts; The mass fraction of the water is 1-50 parts.
5. A method for preparing the inorganic nano-gypsum material according to claim 4, characterized in that: The following steps are included: (1) Preparation of the first composition: A. Weigh each component according to the ratio, add water into the reaction container, add sodium molybdate, disperse and mix evenly, add polyethylene oxide, and disperse and mix evenly after the polyethylene oxide is completely wetted; B. Add nanocellulose ether, triethanolamine, silicone amide and pentaerythritol, and disperse and mix them evenly; C. adding potassium aluminum sulfate dodecahydrate, hydroxyethylidene diphosphoric acid, sodium pyrophosphate, anhydrous calcium chloride and dimethyl silicone oil, dispersing and mixing evenly to obtain a first composition; (2) Preparation of the second composition: Weigh each component according to the ratio, add water into the reaction device, add hydrogen peroxide, polyanionic cellulose, polyethylene glycol and dimethylsiloxane, disperse and mix evenly to obtain a second composition; (3) weighing gypsum powder, water, magnesium sulfate heptahydrate, the first composition, and the second composition according to the proportion; (4) Dispersing and mixing the weighed water, magnesium sulfate heptahydrate and the first composition uniformly; (5) Add gypsum powder and disperse and mix evenly; (6) Add the second composition, disperse and mix evenly to obtain an inorganic nano-gypsum material.
6. The method for preparing the inorganic nano-gypsum material according to claim 5, characterized in that: In step (1) of preparing the first composition, The first dispersing stirring speed of step A is 1300-1600 r / min, and the dispersing stirring time is 50-65 min; The second dispersing stirring speed of step B is 1300-1600 r / min, and the dispersing stirring time is 15-45 min; The third dispersing stirring speed of step C is 1300-1600 r / min, and the dispersing stirring time is 15-45 min.
7. The method for preparing the inorganic nano-gypsum material according to claim 5, characterized in that: In step (2), the dispersion stirring speed in the preparation of the second composition is 600-1200 r / min, and the dispersion stirring time is 15-45 min.
8. The method for preparing the inorganic nano-gypsum material according to claim 5, characterized in that: In step (4), the dispersion stirring speed is 100-500 r / min, and the dispersion stirring time is 0.1-10 min; in step (5), the dispersion stirring speed is 500-1500 r / min, and the dispersion stirring time is 0.1-10 min; in step (6), the dispersion and mixing are uniform, and the dispersion stirring time is 0.1-10 min.