A modified nanocellulose hydrogel and its preparation method and application
Through the preparation method of modified nanocellulose hydrogels, the modified nanocellulose is formed by using quaternized and lanthanization to form a stable hydrogel framework, which solves the problem of insufficient adsorption performance of spherical hydrogel adsorbents on phosphate salts. , significantly improves the removal efficiency and resource utilization rate of phosphate.
Patent Information
- Application Number
- CN202410576295.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-10
AI Technical Summary
The existing spherical hydrogel adsorbents have poor adsorption performance on phosphate in water, resulting in low utilization of phosphorus resources and environmental pollution.
The preparation method of modified nanocellulose hydrogels, including quaternization and lanthanization of modified nanocellulose, adding sodium alginate and lanthanum salt solutions to form a spherical hydrogel, and by polyethyleneimine and glutaraldehyde Modification, build a stable hydrogel skeleton to improve lanthanum loading and adsorption performance.
The adsorption performance of spherical modified nanocellulose hydrogel on phosphate in water is significantly improved, and its removal ability and reusability of phosphate are enhanced, solving the problem of insufficient adsorption performance in the prior art.
Smart Images

Figure CN118530477B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sewage treatment, and more specifically, to a modified nanocellulose hydrogel and a preparation method and application thereof. Background Art
[0002] Phosphorus is an essential element for all forms of life and is also one of the main components of agricultural fertilizers. With the rapid development of the economy, phosphorus has been widely used in industrial and agricultural production. However, in actual use, the utilization rate of phosphorus is not high. Most of the phosphorus enters the natural environment with sewage discharge, causing pollution to the natural environment and waste of phosphorus resources. In particular, when excessive phosphorus is discharged into the water body, it will cause eutrophication of the water body, breed toxic algae blooms, lead to water quality deterioration, and threaten human health. Therefore, it is particularly important to remove phosphorus from the water body.
[0003] Phosphorus in water bodies often exists in the form of phosphates, polyphosphates and organic phosphorus, among which phosphates are the main form. At present, the methods for removing phosphates from water bodies include biological methods, chemical precipitation methods, ion exchange methods and adsorption methods. Among them, the adsorption method has attracted much attention due to its simple operation and relatively low cost. In addition, the adsorption method can also avoid the secondary pollution of the water environment caused by the adsorbent during the adsorption process.
[0004] Hydrogel is a polymer material with a three-dimensional cross-linked network structure formed by chemical bonds, hydrogen bonds, van der Waals forces or physical entanglement. It swells in water but is insoluble in water itself. When used as an adsorbent, hydrogel can adsorb phosphates in water through electrostatic action to achieve the purpose of removing and recovering phosphorus in water. At present, hydrogel adsorbents have two forms: spherical and non-spherical. Compared with non-spherical hydrogels, spherical hydrogel adsorbents are not only easy to recycle and reuse, but also have a larger specific surface area, which can better adsorb phosphates in water. In addition, spherical hydrogel adsorbents usually have high durability and mechanical strength, and can withstand long-term use without being easily worn or broken. However, the adsorption performance of spherical hydrogel adsorbents on phosphates in water is poor.
[0005] Therefore, it is of great significance to develop a method for preparing modified nanocellulose hydrogels to improve the adsorption performance of spherical hydrogel adsorbents for phosphate in water. Summary of the invention
[0006] The purpose of the present invention is to solve the problem of poor adsorption performance of phosphate in water by spherical hydrogel adsorbents in the prior art, and to provide a modified nanocellulose hydrogel and a preparation method and application thereof.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] In a first aspect, the present invention provides a method for preparing a modified nanocellulose hydrogel, comprising the following steps:
[0009] S1. mixing nanocellulose and alkali, adding a quaternary ammonium agent for quaternary modification, adding a lanthanum agent for lanthanum modification, to obtain modified nanocellulose;
[0010] S2. adding the modified nanocellulose to sodium alginate to obtain a modified nanocellulose mixture;
[0011] S3. dropping the modified nanocellulose mixture into a lanthanum salt solution to obtain a hydrogel ball;
[0012] S4. adding polyethyleneimine to the hydrogel balls for mixing, and then adding glutaraldehyde for modification to obtain a modified nanocellulose hydrogel;
[0013] Wherein, the mass ratio of the nanocellulose to sodium alginate is (0.5-1.1):(1.5-2);
[0014] The mass ratio of the nanocellulose to the quaternizing agent is ≤0.475:2.81;
[0015] The mass ratio of the nanocellulose to the lanthanide reagent is ≤0.475:1.5;
[0016] The lanthanation reagent is lanthanum hydroxide and / or lanthanum nitrate.
[0017] The modified nanocellulose hydrogel prepared by the present invention is spherical, contains positively charged quaternary ammonium ions, lanthanum ions and polyethyleneimine, and can adsorb phosphate in water through electrostatic action; at the same time, the present invention constructs a stable hydrogel skeleton by controlling the mass ratio of nanocellulose and sodium alginate, thereby better encapsulating lanthanum ions in a lanthanating agent, improving the lanthanum loading rate of the modified nanocellulose hydrogel, and further improving the adsorption performance of the spherical modified nanocellulose hydrogel on phosphate in water.
[0018] In addition, different forms of lanthanation reagents will affect the stability of the hydrogel skeleton constructed by nanocellulose and sodium alginate, thereby affecting the adsorption performance of spherical modified nanocellulose hydrogels to phosphate in water; moreover, the inventors have found through experiments that lanthanum hydroxide and lanthanum nitrate are suitable forms of lanthanation reagents.
[0019] The reason why the modified nanocellulose mixture is dripped into the lanthanum salt solution in step S3 of the present invention is to allow the carboxyl and hydroxyl groups of the sodium alginate in the modified nanocellulose mixture to undergo cross-linking reaction with the lanthanum ions in the lanthanum salt solution through ionic bonds to form a spherical hydrogel.
[0020] The reason why glutaraldehyde is added after the hydrogel spheres are modified with polyethyleneimine in the present invention is to make polyethyleneimine and glutaraldehyde undergo acetal reaction and Schiff base cross-linking reaction on the surface of the hydrogel spheres, thereby improving the success rate of polyethyleneimine modification.
[0021] The reason why the mass ratio of nanocellulose to quaternizing agent is selected to be ≤0.475:2.81 in the present invention is to ensure that there are enough quaternary ammonium ions to react with the hydroxyl groups on the nanocellulose molecules, thereby improving the efficiency of quaternization modification of nanocellulose.
[0022] The reason why the mass ratio of nanocellulose to lanthanide reagent is selected to be ≤0.475:1.5 in the present invention is to add an excess of lanthanide reagent to increase the lanthanum loading rate of the modified nanocellulose hydrogel.
[0023] Preferably, the mass ratio of the nanocellulose to sodium alginate is (0.5-1.1):(1.625-2).
[0024] More preferably, the mass ratio of the nanocellulose to sodium alginate is (0.5-1.1):2; specifically, the mass ratio of the nanocellulose to sodium alginate is (0.65-1.1):2.
[0025] Preferably, in step S1, the alkali is at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide; the mass ratio of the nanocellulose to the alkali is 0.475:(1.5-2.5), specifically, the mass ratio of the nanocellulose to the alkali is 0.475:2.
[0026] The purpose of adding alkali in step S1 of the present invention is to meet the alkaline environment required for quaternization modification.
[0027] Preferably, in step S1, the mixing and stirring time of the mixed nanocellulose and alkali is 0.5-1 h, specifically, the mixing and stirring time of the mixed nanocellulose and alkali is 0.5 h.
[0028] Preferably, in step S1, the quaternizing agent is at least one of 2,3-epoxypropyltrimethylammonium chloride, dimethyldiallylammonium chloride, bis(triphenylphosphine)ammonium chloride, O-(2-hydroxypropyltrimethylammonium chloride), and 3-chloro-2-hydroxypropyltrimethylammonium chloride.
[0029] Preferably, in step S1, the temperature of the quaternization modification is 60-70°C, and the time is 4-8 hours; specifically, the temperature of the quaternization modification is 65°C, and the time is 6 hours.
[0030] Preferably, in step S1, the temperature of the lanthanum modification is 80-100°C, and the time is 4-10 hours; specifically, the temperature of the lanthanum modification is 80°C, and the time is 4 hours.
[0031] Preferably, in step S3, the lanthanum salt is at least one of lanthanum chloride, lanthanum nitrate, lanthanum carbonate and lanthanum sulfate; the mass fraction of the lanthanum salt solution is ≥2%, specifically, the mass fraction of the lanthanum salt solution is 3%.
[0032] The reason why the mass fraction of the lanthanum salt solution is selected in the present invention is that at this concentration, when the modified nanocellulose mixture is dripped into the lanthanum salt solution, it is conducive to promoting the cross-linking of sodium alginate and lanthanum ions into balls to form spherical hydrogels. When the mass fraction of the lanthanum salt solution is 3%, the cross-linking degree of sodium alginate and lanthanum ions and the mechanical strength of the formed hydrogel balls can be further improved.
[0033] Preferably, in step S4, the polyethyleneimine is a polyethyleneimine solution with a mass fraction of 1%-3%, specifically, the polyethyleneimine is a polyethyleneimine solution with a mass fraction of 2%.
[0034] The present invention selects the polyethyleneimine solution with a mass fraction of 1%-3% because when the mass fraction of the polyethyleneimine solution is too high, a film will be formed on the surface of the hydrogel ball, thereby reducing the adsorption amount of phosphate in the water body by the modified nanocellulose hydrogel.
[0035] Preferably, in step S4, the mass ratio of polyethyleneimine to glutaraldehyde is (1-3):(0.5-1).
[0036] More preferably, in step S4, the mass ratio of polyethyleneimine to glutaraldehyde is 2:0.75.
[0037] Preferably, the step S1 specifically comprises: ultrasonically mixing the nanocellulose and water, then adding alkali and stirring, then adding a quaternary ammonium agent and stirring to perform quaternary ammonium modification, then adding a lanthanating agent and stirring to perform lanthanum modification, and centrifugally washing to obtain modified nanocellulose.
[0038] More preferably, the centrifugal washing needs to be washed to pH ≤ 9.
[0039] Preferably, the step S2 specifically comprises: adding the modified nanocellulose dropwise into the sodium alginate solution, ultrasonicating, and stirring to obtain a modified nanocellulose mixture.
[0040] Preferably, step S4 is specifically as follows: soaking the hydrogel balls in water and repeatedly washing them, then adding polyethyleneimine to mix them, then adding glutaraldehyde to continue mixing them, and then soaking them in water and repeatedly washing them to obtain the modified nanocellulose hydrogel.
[0041] In a second aspect, the present invention provides a modified nanocellulose hydrogel prepared by the above preparation method.
[0042] In a third aspect, the present invention provides an application of a modified nanocellulose hydrogel in water treatment.
[0043] Preferably, the water treatment is to adsorb phosphate in the water.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The modified nanocellulose hydrogel prepared by the present invention is spherical, contains positively charged quaternary ammonium ions, lanthanum ions and polyethyleneimine, and can adsorb phosphate in water through electrostatic action; at the same time, the present invention constructs a stable hydrogel skeleton by controlling the mass ratio of nanocellulose and sodium alginate, thereby better encapsulating lanthanum ions in a lanthanating agent, improving the lanthanum loading rate of the modified nanocellulose hydrogel, and further improving the adsorption performance of the spherical modified nanocellulose hydrogel on phosphate in water.
[0046] In addition, different forms of lanthanation reagents will affect the stability of the hydrogel skeleton constructed by nanocellulose and sodium alginate, thereby affecting the adsorption performance of spherical modified nanocellulose hydrogels to phosphate in water; moreover, the inventors have found through experiments that lanthanum hydroxide and lanthanum nitrate are suitable forms of lanthanation reagents. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is the SEM image of the modified nanocellulose hydrogel in Example 1.
[0048] Figure 2 This is the SEM image of the cross section of the modified nanocellulose hydrogel in Example 1.
[0049] Figure 3 This is a graph showing the adsorption performance test results of the modified nanocellulose hydrogel in Example 1 at different pH values. DETAILED DESCRIPTION
[0050] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0051] The reagents used in the embodiments and comparative examples of the present invention are as follows:
[0052] Nanocellulose, nanocellulose solution, code number: XFJ107, item number: 102203, concentration: 3 wt% (water as solvent), Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.
[0053] Example 1
[0054] This embodiment provides a modified nanocellulose hydrogel, and a preparation method thereof comprises the following steps:
[0055] S1. 15.83 g of nanocellulose solution (3 wt%) was diluted into 25 mL of water and ultrasonically mixed for 1 h, followed by adding 2 g of NaOH and stirring for 0.5 h, then adding 2.81 g of 2,3-epoxypropyltrimethylammonium chloride and stirring at 65 ° C for 5 h for quaternary ammonium modification, then adding 1.5 g of lanthanum hydroxide (0.0079 mol) and stirring at 80 ° C for 4 h for lanthanum modification, and centrifugally washing for multiple times until pH ≤ 9 to obtain modified nanocellulose;
[0056] S2. 1 g of sodium alginate was added to 25 mL of water to prepare a sodium alginate solution, and then the modified nanocellulose was added dropwise to the sodium alginate solution, ultrasonicated for 1 h, and stirred for 12 h to obtain a modified nanocellulose mixture;
[0057] S3. 16.70 g of lanthanum chloride hexahydrate (lanthanum chloride hexahydrate) was added to 400 mL of water to prepare a 3% lanthanum chloride solution, the modified nanocellulose mixture was loaded into a syringe, and the modified nanocellulose mixture was dripped into the lanthanum chloride solution using a syringe pump to obtain a hydrogel ball;
[0058] S4. Soaking the hydrogel balls in water and repeatedly washing them to remove lanthanum chloride attached to the surface of the hydrogel balls, then adding 100 mL of a 2% polyethyleneimine solution by mass to the hydrogel balls and stirring and mixing for 1 hour, then adding 1.5 mL of a 50% glutaraldehyde solution by mass to continue mixing at 50° C. for 6 hours, then soaking them in water and repeatedly washing them to obtain a modified nanocellulose hydrogel;
[0059] Among them, the mass ratio of nanocellulose and alkali NaOH is 0.475:2, the mass ratio of nanocellulose and quaternizing agent 2,3-epoxypropyltrimethylammonium chloride is 0.475:2.81, the mass ratio of nanocellulose and lanthanizing agent lanthanum hydroxide is 0.475:1.5, the mass ratio of nanocellulose and sodium alginate is 0.475:1; the mass ratio of polyethyleneimine and glutaraldehyde is 2:0.75.
[0060] Examples 2-6 and Comparative Examples 1-2
[0061] Examples 2-6 and Comparative Examples 1-2 provide different modified nanocellulose hydrogels, which differ from Example 1 in that the amounts of nanocellulose and sodium alginate used are different, and the rest are consistent with Example 1, as shown in the following table:
[0062] Table 1 Amounts of nanocellulose and sodium alginate in Examples 1-6 and Comparative Examples 1-2
[0063]
[0064] Example 7
[0065] This embodiment provides a modified nanocellulose hydrogel, which differs from Embodiment 1 in that in step S1, 2.57 g of lanthanum nitrate (0.0079 mol) is used as the lanthanation reagent instead of 1.5 g of lanthanum hydroxide (0.0079 mol), and the rest is consistent with Embodiment 1.
[0066] Comparative Example 3
[0067] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that 1.5 g of lanthanum hydroxide is not added in step S1 for lanthanum modification, and the rest is consistent with Example 1.
[0068] Comparative Example 4
[0069] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that in step S1, the lanthanation reagent is replaced by 2.8 g lanthanum chloride hexahydrate (0.0079 mol) instead of 1.5 g lanthanum hydroxide (0.0079 mol), and the rest is consistent with Example 1.
[0070] Comparative Example 5
[0071] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that in step S1, 1.5 g of lanthanum carbonate (0.0079 mol) is used as the lanthanation reagent instead of 1.5 g of lanthanum hydroxide (0.0079 mol), and the rest is consistent with Example 1.
[0072] Comparative Example 6
[0073] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that 100 mL of water is used in step S4 to replace 100 mL of 2% polyethyleneimine solution, that is, the hydrogel spheres are not modified with polyethyleneimine, and the rest is consistent with Example 1.
[0074] Comparative Example 7
[0075] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that 1.5 mL of 0.75% glutaraldehyde solution is not added in step S4, that is, the hydrogel spheres are not modified with glutaraldehyde, and the rest are consistent with Example 1.
[0076] Comparative Example 8
[0077] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that in step S4, 100 mL of water is used instead of 100 mL of 2% polyethyleneimine solution, and 1.5 mL of 0.75% glutaraldehyde solution is not added, that is, the hydrogel balls are not modified with polyethyleneimine and glutaraldehyde, and the rest are consistent with Example 1.
[0078] Comparative Example 9
[0079] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that γ-aminopropyltriethoxysilane (APTEOS) is used instead of glutaraldehyde in step S4, and the rest is consistent with Example 1.
[0080] Comparative Example 10
[0081] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that after step S1, step S4 is performed first, and then steps S2 and S3 are performed, and the rest is consistent with Example 1, specifically comprising the following steps:
[0082] (1) 15.83 g of nanocellulose solution (3 wt%) was diluted into 25 mL of water, ultrasonically mixed for 1 h, then 2 g of NaOH was added and stirred for 0.5 h, then 2.81 g of 2,3-epoxypropyltrimethylammonium chloride was added and stirred at 65 ° C for 5 h for quaternary ammonium modification, then 1.5 g of lanthanum hydroxide was added and stirred at 80 ° C for 4 h for lanthanum modification, and centrifuged and washed several times until the pH was ≤9 to obtain modified nanocellulose;
[0083] (2) adding the modified nanocellulose to 100 mL of a 2% polyethyleneimine (PEI) solution and stirring and mixing for 1 h, then adding 1.5 mL of a 50% glutaraldehyde (GLA) solution at 50° C. and continuing to mix for 6 h, then soaking in water and repeatedly washing, to obtain PEI-modified nanocellulose;
[0084] (3) 1 g of sodium alginate was added to 25 mL of water to prepare a sodium alginate solution, and then the PEI-modified nanocellulose was added dropwise to the sodium alginate solution, ultrasonicated for 1 h, and stirred for 12 h to obtain a modified nanocellulose mixture;
[0085] (4) adding 16.70 g of lanthanum chloride hexahydrate into 400 mL of water to prepare a 3% lanthanum chloride solution, loading the modified nanocellulose mixture into a syringe, and then using a syringe pump to drop the modified nanocellulose mixture into the lanthanum chloride solution to obtain a modified nanocellulose hydrogel;
[0086] Among them, the mass ratio of nanocellulose and alkali NaOH is 0.475:2, the mass ratio of nanocellulose and quaternizing agent 2,3-epoxypropyltrimethylammonium chloride is 0.475:2.81, the mass ratio of nanocellulose and lanthanizing agent lanthanum hydroxide is 0.475:1.5, the mass ratio of nanocellulose and sodium alginate is 0.475:1; the mass ratio of polyethyleneimine and glutaraldehyde is 2:0.75.
[0087] Comparative Example 11
[0088] This comparative example provides a modified nanocellulose hydrogel, which differs from Example 1 in that the sodium alginate mixed with the modified nanocellulose is pre-modified with polyethyleneimine and glutaraldehyde, and the rest is consistent with Example 1, specifically comprising the following steps:
[0089] (1) 15.83 g of nanocellulose solution (3 wt%) was diluted into 25 mL of water, ultrasonically mixed for 1 h, then 2 g of NaOH was added and stirred for 0.5 h, then 2.81 g of 2,3-epoxypropyltrimethylammonium chloride was added and stirred at 65 ° C for 5 h for quaternary ammonium modification, then 1.5 g of lanthanum hydroxide was added and stirred at 80 ° C for 4 h for lanthanum modification, and centrifuged and washed several times until the pH was ≤9 to obtain modified nanocellulose;
[0090] (2) 1 g of sodium alginate was added to 25 mL of water to prepare a sodium alginate solution, and then 100 mL of 2% polyethyleneimine (PEI) solution was added and stirred for 1 h, and then 1.5 mL of 50% glutaraldehyde (GLA) was added and continued to mix at 50° C. for 6 h, and then immersed in water and repeatedly washed to obtain PEI-modified sodium alginate;
[0091] (3) adding the modified nanocellulose dropwise into the PEI-modified sodium alginate, ultrasonicating for 1 h, and stirring for 12 h to obtain a modified nanocellulose mixture;
[0092] (4) adding 16.70 g of lanthanum chloride hexahydrate into 400 mL of water to prepare a 3% lanthanum chloride solution, loading the modified nanocellulose mixture into a syringe, and then using a syringe pump to drop the modified nanocellulose mixture into the lanthanum chloride solution to obtain a modified nanocellulose hydrogel;
[0093] Among them, the mass ratio of nanocellulose and alkali NaOH is 0.475:2, the mass ratio of nanocellulose and quaternizing agent 2,3-epoxypropyltrimethylammonium chloride is 0.475:2.81, the mass ratio of nanocellulose and lanthanizing agent lanthanum hydroxide is 0.475:1.5, the mass ratio of nanocellulose and sodium alginate is 0.475:1; the mass ratio of polyethyleneimine and glutaraldehyde is 2:0.75.
[0094] Sample characterization
[0095] Figure 1 This is the SEM image of the modified nanocellulose hydrogel in Example 1. Figure 2 This is a SEM image of the cross section of the modified nanocellulose hydrogel in Example 1. Figure 1-2It can be seen that the modified nanocellulose hydrogel prepared by the present invention is spherical, and has a large number of wrinkles on its surface and a large number of pores inside, which can provide more adsorption sites, which is conducive to the modified nanocellulose hydrogel to adsorb phosphate in water.
[0096] The SEM images of the modified nanocellulose hydrogels of Examples 2-7 of the present invention and that of Example 1 Figure 1 resemblance.
[0097] Performance Testing
[0098] 1. The modified nanocellulose hydrogels of each embodiment and comparative example were tested for their adsorption performance of phosphate in water. The specific test method is as follows:
[0099] First, observe whether the modified nanocellulose hydrogel is spherical. If the modified nanocellulose hydrogel is spherical, continue with the subsequent experiments; if the modified nanocellulose hydrogel is non-spherical, do not conduct the subsequent experiments;
[0100] Subsequent experiments: Referring to the national standard GB11893-89 "Determination of total phosphorus in water quality - ammonium molybdate spectrophotometry", the initial total phosphorus content A1 (mg / L) of 1L 10mg / L potassium dihydrogen phosphate solution was measured, and then 0.4g of dry weight of modified nanocellulose hydrogel was added and oscillated at a frequency of 160r / min for 24h; after the experiment was completed, the final total phosphorus content A2 (mg / L) of the potassium dihydrogen phosphate solution was tested again with reference to GB11893-89, and the phosphorus adsorption and phosphate removal rate of the modified nanocellulose hydrogel were calculated according to the following formula:
[0101] Phosphorus adsorption of modified nanocellulose hydrogel (mg / g) = [(A1-A2) mg / L × 1L] / 0.4 g;
[0102] Phosphate removal rate of modified nanocellulose hydrogel (%) = (A1-A2) / A1×100%;
[0103] The experimental results are shown in the following table:
[0104] Table 2 Performance test results of various embodiments and comparative examples
[0105]
[0106] As can be seen from Table 2, the modified nanocellulose hydrogel prepared by the present invention is spherical, which improves the adsorption performance of the spherical hydrogel adsorbent for phosphate in water, specifically:
[0107] By comparing Examples 1-6 and Comparative Examples 1-2, it can be seen that the present invention constructs a stable hydrogel skeleton by controlling the mass ratio of nanocellulose and sodium alginate to be (0.5-1.1): (1.5-2), thereby better encapsulating the lanthanum ions in the lanthanation reagent, improving the lanthanum loading rate of the modified nanocellulose hydrogel, and thus improving the adsorption performance of the spherical modified nanocellulose hydrogel to phosphate in the water body. When the mass ratio of nanocellulose and sodium alginate is not within the range of (0.5-1.1): (1.5-2), the constructed hydrogel skeleton cannot well encapsulate the lanthanum ions in the lanthanation reagent, thereby reducing the lanthanum loading rate of the modified nanocellulose hydrogel and its adsorption performance to phosphate in the water body.
[0108] By comparing Examples 1 and 7 with Comparative Examples 4-5, it can be seen that different forms of lanthanating agents will affect the stability of the hydrogel skeleton constructed by nanocellulose and sodium alginate, thereby affecting the adsorption performance of the spherical modified nanocellulose hydrogel for phosphate in water; moreover, in the present invention, lanthanum hydroxide and lanthanum nitrate are suitable forms of lanthanating agents.
[0109] By comparing Example 1 with Comparative Examples 3, 6-8, it can be seen that if any one of the lanthanide reagent, polyethyleneimine, and glutaraldehyde is missing, the adsorption performance of the modified nanocellulose hydrogel of the present invention on phosphate in water will be greatly reduced.
[0110] By comparing Example 1 and Comparative Examples 9-11, it can be seen that by replacing glutaraldehyde with γ-aminopropyltriethoxysilane (APTEOS) or changing the order of the experimental steps of the preparation method of the modified nanocellulose hydrogel of the present invention, a spherical hydrogel adsorbent cannot be obtained.
[0111] 2. The modified nanocellulose hydrogel of Example 1 was tested for the amount of addition. The specific test method is as follows:
[0112] Referring to the national standard GB11893-89 "Determination of total phosphorus in water quality - ammonium molybdate spectrophotometry", the initial total phosphorus content A1 (mg / L) of 1L 10mg / L potassium dihydrogen phosphate solution was measured, and then 0.1g, 0.2g, 0.4g, 0.5g, 0.6g, and 0.7g of modified nanocellulose hydrogel with dry weight were added respectively, and the mixture was oscillated at a frequency of 160r / min for 12h; after the experiment was completed, the final total phosphorus content A2 (mg / L) of the potassium dihydrogen phosphate solution was tested again with reference to GB11893-89, and the phosphorus adsorption amount and phosphate removal rate when different dry weights of modified nanocellulose hydrogel were added were calculated according to the following formula:
[0113] Phosphorus adsorption of modified nanocellulose hydrogel (mg / g) = [(A1-A2) mg / L × 1L] / M;
[0114] Phosphate removal rate of modified nanocellulose hydrogel (%) = (A1-A2) / A1×100%;
[0115] Wherein, M is the dry weight of the modified nanocellulose hydrogel in g, and its value can be 0.1 g, 0.2 g, 0.4 g, 0.5 g, 0.6 g or 0.7 g;
[0116] The experimental results are shown in the following table:
[0117] Table 3 Test results of the amount of modified nanocellulose hydrogel added in Example 1
[0118]
[0119] As shown in Table 3, as the addition amount increases from 0.1 g / L to 0.7 g / L, the phosphorus adsorption of the modified nanocellulose hydrogel decreases from 45.61 mg / g to 16.12 mg / g, and the phosphate removal rate of the modified nanocellulose hydrogel increases from 39.74% to 99.34%. Considering the phosphorus adsorption amount and the utilization rate of the modified nanocellulose hydrogel, it is believed that the addition amount of 0.4 g / L of the modified nanocellulose hydrogel is more appropriate for a 10 mg / L potassium dihydrogen phosphate solution.
[0120] 3. The adsorption performance of the modified nanocellulose hydrogel under different phosphorus concentrations was tested. The specific test method was as follows:
[0121] Referring to the national standard GB11893-89 "Determination of total phosphorus in water quality - ammonium molybdate spectrophotometry", the initial total phosphorus content A1 (mg / L) of 1L potassium dihydrogen phosphate solution with different initial concentrations was measured, and then 0.4g of modified nanocellulose hydrogel with a dry weight was added, and the mixture was oscillated at a frequency of 160r / min, and the timing was started. Samples were taken every hour and the real-time total phosphorus content A3 (mg / L) of the potassium dihydrogen phosphate solution was tested with reference to GB11893-89. When it was found that the real-time total phosphorus content A3 of the potassium dihydrogen phosphate solution no longer changed, it was considered that the adsorption equilibrium was reached, and the time at this time was recorded as the equilibrium time (h) for reaching the adsorption equilibrium, and the phosphate removal rate of the modified nanocellulose hydrogel was calculated according to the following formula:
[0122] Phosphate removal rate of modified nanocellulose hydrogel (%) = (A1-A3) / A1×100%;
[0123] The experimental results are shown in the following table:
[0124] Table 4 Adsorption performance test results of modified nanocellulose hydrogel at different phosphorus concentrations
[0125]
[0126]
[0127] It can be seen from Table 4 that the modified nanocellulose hydrogel of the present invention has a good adsorption effect on phosphate in water.
[0128] 4. The adsorption performance of the modified nanocellulose hydrogel was tested at different pH values. The specific test method is as follows:
[0129] The pH value of 10 mg / L potassium dihydrogen phosphate solution was adjusted with HCl and NaOH, and the initial total phosphorus content A1 (mg / L) of 1L 10 mg / L potassium dihydrogen phosphate solution at different pH values was measured with reference to the national standard GB11893-89 "Determination of total phosphorus in water quality - ammonium molybdate spectrophotometry", and then 0.4 g of modified nanocellulose hydrogel with a dry weight was added and oscillated at a frequency of 160 r / min for 12 h; after the experiment was completed, the final total phosphorus content A2 (mg / L) of the potassium dihydrogen phosphate solution was tested again with reference to GB11893-89, and the phosphorus adsorption and phosphate removal rate of the modified nanocellulose hydrogel were calculated according to the following formula:
[0130] Phosphorus adsorption of modified nanocellulose hydrogel (mg / g) = [(A1-A2) mg / L × 1L] / 0.4 g;
[0131] Phosphate removal rate of modified nanocellulose hydrogel (%) = (A1-A2) / A1×100%;
[0132] The experimental results are shown in the following table:
[0133] Table 5 Adsorption performance test results of modified nanocellulose hydrogel at different pH values
[0134]
[0135] Figure 3 The graphs are the test results of the adsorption performance of the modified nanocellulose hydrogel at different pH values of Example 1. The test results of the adsorption performance of the modified nanocellulose hydrogel at different pH values of Examples 2-7 of the present invention are similar to those of Example 1. Figure 3 Similarly, the highest phosphate removal rate was achieved at pH = 3.
[0136] from Figure 3 As shown in Table 5, the pH value of the use environment of the modified nanocellulose hydrogel of the present invention is relatively wide, and within the range of pH=3-7, it has a good adsorption effect on phosphate in water.
[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a modified nanocellulose hydrogel, characterized in that: The steps include: S1. mixing nanocellulose and alkali, adding a quaternary ammonium agent for quaternary modification, adding a lanthanum agent for lanthanum modification, to obtain modified nanocellulose; S2. adding the modified nanocellulose dropwise into the sodium alginate solution to obtain a modified nanocellulose mixture; S3. dropping the modified nanocellulose mixture into a lanthanum salt solution to obtain a hydrogel ball; S4. adding polyethyleneimine to the hydrogel balls for mixing, and then adding glutaraldehyde for modification to obtain a modified nanocellulose hydrogel; Wherein, the mass ratio of the nanocellulose to sodium alginate is (0.5-1.1):(1.5-2); The mass ratio of the nanocellulose to the quaternizing agent is ≤0.475:2.81; The mass ratio of the nanocellulose to the lanthanide reagent is ≤0.475:1.5; The lanthanation reagent is lanthanum hydroxide and / or lanthanum nitrate; In step S4, the polyethyleneimine is a polyethyleneimine solution with a mass fraction of 1%-3%.
2. The method for preparing the modified nanocellulose hydrogel according to claim 1, characterized in that: In step S1, the quaternizing agent is at least one of 2,3-epoxypropyltrimethylammonium chloride, dimethyldiallyl ammonium chloride, bis(triphenylphosphine)ammonium chloride, O-(2-hydroxypropyltrimethylammonium chloride), and 3-chloro-2-hydroxypropyltrimethylammonium chloride.
3. The method for preparing the modified nanocellulose hydrogel according to claim 1, characterized in that: In step S1, the base is at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide.
4. The method for preparing the modified nanocellulose hydrogel according to claim 1, characterized in that: In step S3, the lanthanum salt is at least one of lanthanum chloride, lanthanum nitrate, lanthanum carbonate and lanthanum sulfate.
5. The method for preparing the modified nanocellulose hydrogel according to claim 1, characterized in that: In step S1, the mass ratio of the nanocellulose to the alkali is 0.475:(1.5-2.5).
6. The method for preparing the modified nanocellulose hydrogel according to claim 1, characterized in that: In step S3, the mass fraction of the lanthanum salt solution is ≥ 2%.
7. The method for preparing the modified nanocellulose hydrogel according to claim 1, characterized in that: In step S4, the mass ratio of polyethyleneimine to glutaraldehyde is (1-3):(0.5-1).
8. A modified nanocellulose hydrogel prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the modified nanocellulose hydrogel according to claim 8 in water treatment, characterized in that: The water treatment is to adsorb phosphate in the water.