A preparation method of modified asphalt and its application in porous graphite products
Through modified carbon nanotubes and asphalt pretreatment technology, the problem of poor oxidation resistance of modified asphalt is solved, the mechanical and thermal conductivity properties of porous graphite products are improved, and a more stable bonding effect is achieved.
Patent Information
- Application Number
- CN202410993342.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing modified asphalt has poor oxidation resistance, which leads to poor bonding performance after strong ultraviolet and high temperature treatment, affecting the mechanical properties and stability of porous graphite.
Modified carbon nanotubes and asphalt pretreatment methods are used to improve the wettability of carbon nanotubes and the fluidity and compatibility of asphalt through high-temperature purification, hydroxylation, ultrasonic treatment, epoxy coupling and mercaptoethylamine reaction to form Efficient modified asphalt.
It significantly improves the bonding performance and oxidation resistance of modified asphalt, improves the mechanical properties, stability and thermal conductivity of porous graphite products, and reduces the weight loss rate.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified asphalt, and specifically relates to a preparation method of modified asphalt and application of the modified asphalt in porous graphite products. Background Art
[0002] Porous graphite products are made of calcined coke as raw materials and asphalt as a binder, through a series of processes such as crushing, batching, kneading, molding, sintering, impregnation, graphitization, and mechanical processing. They are widely used in metallurgy, chemical industry, petroleum, high-energy physics, aerospace, electronics and other fields.
[0003] In the production process of porous graphite products, the kneading process uses asphalt as a binder to bind the non-molding particles and powdered aggregates together to form a raw product with a certain shape and strength; the asphalt binder is also transformed into the same carbon as the aggregate in the subsequent carbonization process, which binds the aggregate particles together. The combination of the binder and the aggregate directly affects the performance of the porous graphite product.
[0004] Therefore, when asphalt is used as a binder, improving the softening point of asphalt and enhancing its compatibility with aggregates are technical challenges that need to be urgently solved in the existing technology.
[0005] In this regard, the prior art discloses the following:
[0006] CN116462509A discloses an isostatic graphite for photovoltaic use and its preparation method and application, specifically disclosing that petroleum coke, pitch coke, carbon black, modified asphalt and modified carbon fiber are used as raw material components; wherein the preparation method of the modified asphalt is to add graphite powder to hydrogen peroxide for activation, and then treat it with kH570 to obtain modified graphite powder, melt elemental sulfur and zinc dihexyl dithioformate, add modified graphite powder and asphalt for reaction, and obtain modified asphalt;
[0007] The modified asphalt prepared by the above method heats and melts elemental sulfur to form a sulfur chain with a free radical at the end, which reacts with the unsaturated double bonds in the asphalt and the modified graphite powder to form a cross-linked network, thereby improving the homogeneity and mechanical properties of the isostatic graphite.
[0008] However, the modified asphalt produced by this patent has poor antioxidant ability. After being treated with strong ultraviolet rays and high temperature, its bonding performance deteriorates, thereby affecting the mechanical properties and stability of the isostatic graphite. Summary of the invention
[0009] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing modified asphalt and its application in porous graphite products. The modified asphalt has good bonding properties and strong antioxidant ability, and the porous graphite products prepared therefrom have strong mechanical properties and good stability.
[0010] In view of the above technical problems, the present invention adopts the following technical solutions:
[0011] A method for preparing modified asphalt includes the steps of modifying carbon nanotubes, pretreating asphalt, and mixing. The specific operations are as follows:
[0012] 1. Modified carbon nanotubes
[0013] (1) One-time modification
[0014] The carbon nanotubes are placed in a muffle furnace, heated to 220-260°C at a rate of 4.8-5.2°C / min, and kept at 220-260°C for 20-35min. After the heat preservation, the temperature is increased to 400-450°C at a rate of 2.6-3.4°C / min, and kept at 400-450°C for 1.0-1.4h. The treatment atmosphere is nitrogen. After the heat preservation, a primary modified carbon nanotube is obtained;
[0015] The particle size of the carbon nanotubes is 5-90 nm;
[0016] (2) Secondary modification
[0017] The primary modified carbon nanotubes are mixed with a hydrogen peroxide solution, and then subjected to ultrasonic treatment, wherein the ultrasonic time is 10-20 minutes and the ultrasonic frequency is 22-28 kHz. After the ultrasonic treatment, the mixture is dried, and then deionized water, ethylene glycol and PEG-30 glyceryl cocoate are added, and the ultrasonic treatment is continued for 20-30 minutes. After the ultrasonic treatment, the mixture is dried to obtain the secondary modified carbon nanotubes;
[0018] The mass concentration of the hydrogen peroxide solution is 20-24%;
[0019] The mass ratio of the primary modified carbon nanotubes, hydrogen peroxide solution, deionized water, ethylene glycol, and PEG-30 glyceryl cocoate is 16-20:137-143:121-130:2.8-3.2:2.0-2.2;
[0020] (3) Three modifications
[0021] The secondary modified carbon nanotubes are placed in a modification liquid, heated to 65-75°C and stirred for 9.0-11.0 hours. After the stirring is completed, the product is filtered, washed and dried to obtain a tertiary modified preliminary product. The tertiary modified preliminary product is placed in toluene, stirred evenly, and then mercaptoethylamine is added. The product is then heated to 105-115°C at a rate of 1.4-1.6°C / min for reflux reaction. The reflux reaction time is 4.5-5.5 hours. After the reaction is completed, the product is filtered, washed and dried to obtain modified carbon nanotubes.
[0022] The mass ratio of the secondary modified carbon nanotubes to the modified liquid is 10.2-10.4:56-60;
[0023] The mass ratio of the tertiary modified primary product, toluene and mercaptoethylamine is 8.2-8.6:98-103:2.6-2.8;
[0024] The preparation method of the modified liquid is as follows: γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 38-42wt% ethanol solution are mixed and stirred to obtain the modified liquid;
[0025] The mass ratio of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 38-42wt% ethanol solution is 1.1-1.5:0.4-0.6:63-67.
[0026] 2. Asphalt pretreatment
[0027] The asphalt is placed in 4.8-5.2 times the mass of tetrahydrofuran for ball milling treatment, the ball milling time is 25-35 minutes, the ball milling speed is 200-500rpm, and the ball-to-material ratio is 3-5:1. After the ball milling is completed, polyethylene glycol and castor oil polyoxyethylene ether are added, the speed is controlled to 300-700rpm, the ball-to-material ratio is 4-8:1, and the ball milling is continued for 20-30 minutes. After the ball milling is completed, a first-treated asphalt is obtained, and then vinyl tri(β-methoxyethoxy) silane is added, the temperature is raised to 60-65°C, and stirred for 1.7-2.5 hours. After the stirring is completed, it is dried to obtain the pretreated asphalt;
[0028] The asphalt is a mixture of 20# petroleum asphalt and 90# petroleum asphalt, and the mass ratio of the 20# petroleum asphalt to the 90# petroleum asphalt is 0.8-1.2:1;
[0029] The mass ratio of the asphalt, polyethylene glycol, castor oil polyoxyethylene ether and vinyl tri(β-methoxyethoxy)silane is 18-22:0.8-1.2:1.3-1.5:1.0-1.2.
[0030] 3. Mixing
[0031] The pretreated asphalt is heated to 161-165°C, and then modified carbon nanotubes, paraffin oil and phenolic resin are added for homogenization. The homogenization pressure is 5.0-5.4MPa, the homogenization time is 3.0-5.0min, and the homogenization times are 3 times. After the homogenization treatment, high-speed shearing treatment is performed. The shearing speed is 6000-7500rpm, and the shearing time is 17-23min. After the shearing is completed, the modified asphalt is obtained;
[0032] The mass ratio of the pretreated asphalt, modified carbon nanotubes, paraffin oil and phenolic resin is 47-53:6.3-6.5:2.0-2.4:13-15.
[0033] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0034] 1. The present invention uses modified carbon nanotubes for preparing modified asphalt. In the modification process of carbon nanotubes, the carbon nanotubes are first purified at high temperature and then subjected to secondary modification. The hydrogen peroxide in the secondary modification hydroxylates the carbon nanotubes. Then, ethylene glycol and PEG-30 glyceryl cocoate are used in combination with ultrasonic treatment to uniformly disperse the components inside the carbon nanotubes, thereby improving the wettability of the carbon nanotubes and increasing the hydroxyl groups on the surface of the carbon nanotubes. In the third modification step, an epoxy silane coupling agent is used for modification, so that the hydroxyl groups on the surface of the carbon nanotubes are bonded to the hydroxyl groups of the epoxy silane coupling agent, so that the surface of the carbon nanotubes is rich in epoxy groups. Then, the carbon nanotubes are treated with mercaptoethylamine, and the amino groups of the mercaptoethylamine bond to the surface of the carbon nanotubes. The epoxy groups of the pretreated asphalt react with the thiol groups on the surface of the carbon nanotubes, so that the surface of the modified carbon nanotubes is grafted with thiol groups; the petroleum asphalt is treated twice to increase the fluidity and compatibility of the asphalt, and the asphalt is mixed with the modified carbon nanotubes during the mixing process, and the vinyl groups of the pretreated asphalt react with the thiol groups on the surface of the carbon nanotubes, so that the binding force between the pretreated asphalt and the carbon nanotubes is strong, the compatibility is good, and the homogeneity of the modified asphalt is improved, so that the bonding performance of the modified asphalt is good. It is used to prepare porous graphite products, has strong permeability to aggregate carbon particles, good lubricity, and significantly improves the kneading strength. The antioxidant performance of the porous graphite products is significantly improved, the mechanical properties and stability are excellent, the weight loss rate is low, and the thermal conductivity is good;
[0035] 2. The modified asphalt prepared by the present invention is used in porous graphite products, and the thermal conductivity of the porous graphite products is 131-137W / m·K, the flexural strength is 72.5-78.6MPa, the compressive strength is 121.4-126.7MPa, and the bending strength is 91.4-95.3MPa;
[0036] 3. The modified asphalt prepared by the present invention is used in porous graphite products. The porous graphite products are placed in a closed environment, heated to 1600°C at a rate of 5°C / min in a nitrogen atmosphere, and kept at 1600°C for 12 hours. After the heat preservation treatment, the temperature is naturally lowered to room temperature, and then placed in a temperature with a strength of 760W / m 2 After irradiation for 7 days under ultraviolet light, the flexural strength of the porous graphite products was measured to be 69.0-76.0MPa, the compressive strength was 114.4-121.6MPa, and the bending strength was 86.6-91.9MPa.
[0037] 4. The modified asphalt prepared in the present invention is used in porous graphite products. The porous graphite products are placed in a tubular furnace, and the temperature is increased to 700°C at a rate of 5°C / min under an air flow rate of 10L / h. The products are kept at 700°C for 2h. After the insulation treatment, ventilation is stopped and the product is sealed, and the product is naturally cooled to room temperature. The weight loss rate after oxidation is measured to be 1.27-1.86%. DETAILED DESCRIPTION
[0038] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.
[0039] Example 1
[0040] 1. Modified carbon nanotubes
[0041] (1) One-time modification
[0042] The carbon nanotubes were placed in a muffle furnace, heated to 240°C at a rate of 5.0°C / min, and kept at 240°C for 30 minutes. After the heat preservation, the temperature was increased to 430°C at a rate of 3.0°C / min, and kept at 430°C for 1.2 hours. The treatment atmosphere was nitrogen. After the heat preservation, primary modified carbon nanotubes were obtained.
[0043] The particle size of the carbon nanotubes is 35-60 nm;
[0044] (2) Secondary modification
[0045] 18 g of primary modified carbon nanotubes were mixed with 140 g of hydrogen peroxide solution, and then subjected to ultrasonic treatment, the ultrasonic time was 15 min, the ultrasonic frequency was 25 kHz, and after the ultrasonic treatment, the mixture was dried. Then, 126 g of deionized water, 3.0 g of ethylene glycol and 2.1 g of PEG-30 glyceryl cocoate were added, and the ultrasonic treatment was continued for 23 min. After the ultrasonic treatment, the mixture was dried to obtain secondary modified carbon nanotubes.
[0046] The mass concentration of the hydrogen peroxide solution is 22%;
[0047] (3) Three modifications
[0048] 10.3 g of the secondary modified carbon nanotubes were placed in 58 g of the modified solution, heated to 69° C. and stirred for 10.0 h. After the stirring was completed, the solution was filtered, washed and dried to obtain a tertiary modified preliminary product. 8.4 g of the tertiary modified preliminary product was placed in 100 g of toluene, stirred evenly, and then 2.7 g of mercaptoethylamine was added. The solution was then heated to 108° C. at a rate of 1.5° C. / min for reflux reaction. The reflux reaction time was 5.0 h. After the reaction was completed, the solution was filtered, washed and dried to obtain modified carbon nanotubes.
[0049] The preparation method of the modified liquid is as follows: γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 40wt% ethanol solution are mixed and stirred to obtain the modified liquid;
[0050] The mass ratio of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 40 wt % ethanol solution is 1.3:0.5:65.
[0051] 2. Asphalt pretreatment
[0052] 20g of asphalt was placed in 5 times the mass of tetrahydrofuran for ball milling treatment. The ball milling time was 30min, the ball milling speed was 320rpm, and the ball-to-material ratio was 4:1. After the ball milling was completed, 1.0g of polyethylene glycol and 1.4g of castor oil polyoxyethylene ether were added, the speed was controlled to 540rpm, the ball-to-material ratio was 6:1, and the ball milling was continued for 25min. After the ball milling was completed, a first-treated asphalt was obtained, and then 1.1g of vinyl tri(β-methoxyethoxy)silane was added, the temperature was raised to 63°C, and stirred for 2h. After the stirring was completed, the asphalt was dried to obtain the pretreated asphalt;
[0053] The asphalt is a mixture of 20# petroleum asphalt and 90# petroleum asphalt, and the mass ratio of the 20# petroleum asphalt to the 90# petroleum asphalt is 1:1.
[0054] 3. Mixing
[0055] 50g of pretreated asphalt was heated to 163°C, and then 6.4g of modified carbon nanotubes, 2.2g of paraffin oil and 14g of phenolic resin were added for homogenization. The homogenization pressure was 5.2MPa, the homogenization time was 4.0min, and the number of homogenizations was 3 times. After the homogenization, high-speed shearing treatment was carried out with a shearing speed of 6800rpm and a shearing time of 20min. After the shearing, modified asphalt was obtained.
[0056] Example 2
[0057] 1. Modified carbon nanotubes
[0058] (1) One-time modification
[0059] The carbon nanotubes were placed in a muffle furnace, heated to 220°C at a rate of 4.8°C / min, and kept at 220°C for 20 minutes. After the heat preservation, the temperature was increased to 400°C at a rate of 2.6°C / min, and kept at 400°C for 1.0 hour. The treatment atmosphere was nitrogen. After the heat preservation, primary modified carbon nanotubes were obtained.
[0060] The particle size of the carbon nanotubes is 5-35 nm;
[0061] (2) Secondary modification
[0062] 16 g of primary modified carbon nanotubes were mixed with 137 g of hydrogen peroxide solution, and then subjected to ultrasonic treatment, the ultrasonic time was 10 min, the ultrasonic frequency was 22 kHz, and after the ultrasonic treatment, the mixture was dried, and then 121 g of deionized water, 2.8 g of ethylene glycol and 2.0 g of PEG-30 glyceryl cocoate were added, and the ultrasonic treatment was continued, the ultrasonic time was 20 min, and after the ultrasonic treatment, the mixture was dried to obtain secondary modified carbon nanotubes;
[0063] The mass concentration of the hydrogen peroxide solution is 20%;
[0064] (3) Three modifications
[0065] 10.2 g of the secondary modified carbon nanotubes were placed in 56 g of the modified solution, heated to 65° C. and stirred for 9.0 h. After the stirring was completed, the solution was filtered, washed and dried to obtain a tertiary modified preliminary product. 8.2 g of the tertiary modified preliminary product was placed in 98 g of toluene, stirred evenly, and then 2.6 g of mercaptoethylamine was added. The solution was then heated to 105° C. at a rate of 1.4° C. / min for reflux reaction. The reflux reaction time was 4.5 h. After the reaction was completed, the solution was filtered, washed and dried to obtain modified carbon nanotubes.
[0066] The preparation method of the modified liquid is as follows: γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 38wt% ethanol solution are mixed and stirred to obtain the modified liquid;
[0067] The mass ratio of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 38 wt % ethanol solution is 1.1:0.4:63.
[0068] 2. Asphalt pretreatment
[0069] 18g of asphalt was placed in 4.8 times the mass of tetrahydrofuran for ball milling treatment. The ball milling time was 25min, the ball milling speed was 200rpm, and the ball-to-material ratio was 3:1. After the ball milling was completed, 0.8g of polyethylene glycol and 1.3g of castor oil polyoxyethylene ether were added, the speed was controlled to 300rpm, the ball-to-material ratio was 4:1, and the ball milling was continued for 20min. After the ball milling was completed, a first-treated asphalt was obtained, and then 1.0g of vinyl tri(β-methoxyethoxy)silane was added, the temperature was raised to 60°C, and stirred for 1.7h. After the stirring was completed, the asphalt was dried to obtain the pretreated asphalt;
[0070] The asphalt is a mixture of 20# petroleum asphalt and 90# petroleum asphalt, and the mass ratio of the 20# petroleum asphalt to the 90# petroleum asphalt is 0.8:1.
[0071] 3. Mixing
[0072] 47g of pretreated asphalt was heated to 161°C, and then 6.3g of modified carbon nanotubes, 2.0g of paraffin oil and 13g of phenolic resin were added for homogenization. The homogenization pressure was 5.0MPa, the homogenization time was 3.0min, and the number of homogenizations was 3 times. After the homogenization, high-speed shearing treatment was carried out with a shearing speed of 6000rpm and a shearing time of 17min. After the shearing, modified asphalt was obtained.
[0073] Example 3
[0074] 1. Modified carbon nanotubes
[0075] (1) One-time modification
[0076] The carbon nanotubes were placed in a muffle furnace, heated to 260°C at a rate of 5.2°C / min, and kept at 260°C for 35 minutes. After the heat preservation, the temperature was increased to 450°C at a rate of 3.4°C / min, and kept at 450°C for 1.4 hours. The treatment atmosphere was nitrogen. After the heat preservation, primary modified carbon nanotubes were obtained.
[0077] The particle size of the carbon nanotubes is 65-90 nm;
[0078] (2) Secondary modification
[0079] 20 g of primary modified carbon nanotubes were mixed with 143 g of hydrogen peroxide solution, and then subjected to ultrasonic treatment, the ultrasonic time was 20 min, the ultrasonic frequency was 28 kHz, and after the ultrasonic treatment, the mixture was dried, and then 130 g of deionized water, 3.2 g of ethylene glycol and 2.2 g of PEG-30 glyceryl cocoate were added, and the ultrasonic treatment was continued, the ultrasonic time was 30 min, and after the ultrasonic treatment, the mixture was dried to obtain secondary modified carbon nanotubes;
[0080] The mass concentration of the hydrogen peroxide solution is 24%;
[0081] (3) Three modifications
[0082] 10.4 g of the secondary modified carbon nanotubes were placed in 60 g of the modified solution, heated to 75° C. and stirred for 11.0 h. After the stirring was completed, the solution was filtered, washed and dried to obtain a tertiary modified preliminary product. 8.6 g of the tertiary modified preliminary product was placed in 103 g of toluene, stirred evenly, and then 2.8 g of mercaptoethylamine was added. The solution was then heated to 115° C. at a rate of 1.6° C. / min for reflux reaction. The reflux reaction time was 5.5 h. After the reaction was completed, the solution was filtered, washed and dried to obtain modified carbon nanotubes.
[0083] The preparation method of the modified liquid is as follows: γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 42wt% ethanol solution are mixed and stirred to obtain the modified liquid;
[0084] The mass ratio of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 42 wt % ethanol solution is 1.5:0.6:67.
[0085] 2. Asphalt pretreatment
[0086] 22g of asphalt was placed in 5.2 times the mass of tetrahydrofuran for ball milling treatment, the ball milling time was 35min, the ball milling speed was 500rpm, and the ball-to-material ratio was 5:1. After the ball milling was completed, 1.2g of polyethylene glycol and 1.5g of castor oil polyoxyethylene ether were added, the speed was controlled to 700rpm, the ball-to-material ratio was 8:1, and the ball milling was continued for 30min. After the ball milling was completed, a first-treated asphalt was obtained, and then 1.2g of vinyl tri(β-methoxyethoxy)silane was added, the temperature was raised to 65°C, and stirred for 2.5h. After the stirring was completed, the asphalt was dried to obtain the pretreated asphalt;
[0087] The asphalt is a mixture of 20# petroleum asphalt and 90# petroleum asphalt, and the mass ratio of the 20# petroleum asphalt to the 90# petroleum asphalt is 1.2:1.
[0088] 3. Mixing
[0089] 53g of pretreated asphalt was heated to 165°C, and then 6.5g of modified carbon nanotubes, 2.4g of paraffin oil and 15g of phenolic resin were added for homogenization. The homogenization pressure was 5.4MPa, the homogenization time was 5.0min, and the number of homogenizations was 3 times. After the homogenization, high-speed shearing treatment was carried out with a shearing speed of 7500rpm and a shearing time of 23min. After the shearing, modified asphalt was obtained.
[0090] Comparative Example 1
[0091] Based on Example 1, the changes are that the secondary and tertiary modification steps of the carbon nanotubes are omitted, and in the mixing step, the modified carbon nanotubes are replaced with the primary modified carbon nanotubes in equal amounts, and the rest of the operations are the same.
[0092] Comparative Example 2
[0093] Based on Example 1, the changes are that the asphalt pretreatment step is omitted, and the pretreated asphalt is replaced with untreated asphalt in an equal amount in the mixing step, and the rest of the operations are the same.
[0094] Performance Testing
[0095] The asphalt-based binder prepared in Example 1-3 and Comparative Example 1-2 was mixed with 80-mesh artificial graphite, wherein the mass ratio of the artificial graphite to the asphalt-based binder was 3:1, and after pressing and molding, the mixture was heated to 400°C at a rate of 2.5°C / min in a nitrogen atmosphere, kept at 400°C for 2 hours, then heated to 1200°C at a rate of 3.5°C / min, kept at 2200°C for 15 hours, and finally graphitized at a graphitization temperature of 2200°C for 24 hours. After the graphitization treatment was completed, a porous graphite product was obtained;
[0096] (1) Kneading strength performance
[0097] The porous graphite products prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to strength performance tests, as follows:
[0098]
[0099] (2) Antioxidant properties
[0100] A. Strength performance retention rate
[0101] The porous graphite products prepared in Examples 1-3 and Comparative Examples 1-2 were placed in a closed environment, heated to 1600°C at a rate of 5°C / min in a nitrogen atmosphere, and kept at 1600°C for 12 hours. After the heat preservation treatment, the temperature was naturally lowered to room temperature, and then placed in a temperature range of 760 W / m 2 After irradiation for 7 days under ultraviolet light, the mechanical properties were tested. The specific results are as follows:
[0102]
[0103] B. Weight loss rate
[0104] The porous graphite products prepared in Examples 1-3 and Comparative Examples 1-2 were placed in a tubular furnace, heated to 700°C at a rate of 5°C / min under an air flow rate of 10 L / h, and kept at 700°C for 2 hours. After the heat preservation treatment, ventilation was stopped and the products were sealed, and naturally cooled to room temperature. The weight loss rate after oxidation was tested, and the specific results were as follows:
[0105]
[0106] Comparative Example 1 omits the secondary and tertiary modification steps of the carbon nanotubes, and uses single-modified carbon nanotubes in the mixing step. The carbon nanotubes have serious aggregation, poor dispersion performance, and poor wettability. They cannot be evenly dispersed in the asphalt system, and have poor bonding strength with asphalt, resulting in poor homogeneity of the modified asphalt, poor bonding performance, and poor antioxidant performance. They are used to prepare porous graphite products, which reduces the mechanical properties and thermal conductivity of the porous graphite products, and the mechanical properties are unstable and the weight loss rate is high.
[0107] Comparative Example 2 omits the pretreatment step for asphalt, and the fluidity of asphalt is poor and its compatibility with carbon nanotubes is poor, which affects the bonding and antioxidant properties of the modified asphalt, thereby reducing the mechanical properties and stability of the porous graphite products and affecting the thermal conductivity.
[0108] The present invention adopts modified carbon nanotubes for preparing modified asphalt. In the modification process of carbon nanotubes, the carbon nanotubes are first purified at high temperature and then subjected to secondary modification. The hydrogen peroxide in the secondary modification hydroxylates the carbon nanotubes. Then, ethylene glycol and PEG-30 glyceryl cocoate are used in combination with ultrasonic treatment to uniformly disperse the components inside the carbon nanotubes, thereby improving the wettability of the carbon nanotubes and increasing the hydroxyl groups on the surfaces of the carbon nanotubes. In the third modification step, an epoxy silane coupling agent is used for modification, so that the hydroxyl groups on the surfaces of the carbon nanotubes are bonded with the hydroxyl groups of the epoxy silane coupling agent, so that the surfaces of the carbon nanotubes are rich in epoxy groups. Then, the carbon nanotubes are treated with mercaptoethylamine, and the amino groups of the mercaptoethylamine and the epoxy groups on the surfaces of the carbon nanotubes are bonded. The pretreated asphalt is mixed with the modified carbon nanotubes during the mixing process, and the vinyl groups of the pretreated asphalt react with the thiol groups on the surface of the carbon nanotubes, so that the pretreated asphalt and the carbon nanotubes have a strong bonding force and good compatibility, and the homogeneity of the modified asphalt is improved, thereby making the modified asphalt have good bonding properties and good antioxidant properties. It is used to prepare porous graphite products, has strong permeability to aggregate carbon particles, good lubricity, and significantly improved kneading strength. The antioxidant properties of porous graphite products are significantly improved, and the mechanical properties and stability are excellent, the weight loss rate is low, and the thermal conductivity is good.
[0109] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0110] Unless otherwise specified, the ratios described in the present invention are all mass ratios, and the percentages described are all mass percentages.
Claims
1. A method for preparing modified asphalt, characterized in that: It includes the steps of modifying carbon nanotubes, pre-treating asphalt and mixing; The modified carbon nanotubes include primary modification, secondary modification and tertiary modification; The first modification step is to place the carbon nanotubes in a muffle furnace, heat them to 220-260°C at a rate of 4.8-5.2°C / min, keep them at 220-260°C for 20-35min, heat them to 400-450°C at a rate of 2.6-3.4°C / min after the heat preservation, and keep them at 400-450°C for 1.0-1.4h, the treatment atmosphere is nitrogen, and after the heat preservation, the first modified carbon nanotubes are obtained; The secondary modification step comprises mixing the primary modified carbon nanotubes with a hydrogen peroxide solution, and then performing ultrasonic treatment, wherein the ultrasonic time is 10-20 minutes and the ultrasonic frequency is 22-28 kHz. After the ultrasonic treatment, drying is performed, and then deionized water, ethylene glycol and PEG-30 glyceryl cocoate are added, and the ultrasonic treatment is continued, wherein the ultrasonic time is 20-30 minutes. After the ultrasonic treatment, drying is performed to obtain the secondary modified carbon nanotubes. The three-time modification step is to place the secondary modified carbon nanotubes in a modification solution, heat it to 65-75°C and stir it for 9.0-11.0 hours, filter, wash and dry it after the stirring is completed to obtain a three-time modified preliminary product, place the three-time modified preliminary product in toluene, stir it evenly, add mercaptoethylamine, and then heat it to 105-115°C at a rate of 1.4-1.6°C / min for reflux reaction, and the reflux reaction time is 4.5-5.5 hours. After the reaction is completed, filter, wash and dry it to obtain modified carbon nanotubes; The preparation method of the modified liquid is as follows: γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 38-42wt% ethanol solution are mixed and stirred to obtain the modified liquid; The asphalt pretreatment step is to place the asphalt in 4.8-5.2 times the mass of tetrahydrofuran for ball milling, the ball milling time is 25-35 minutes, the ball milling speed is 200-500rpm, the ball-to-material ratio is 3-5:1, after the ball milling is completed, polyethylene glycol and castor oil polyoxyethylene ether are added, the speed is controlled to 300-700rpm, the ball-to-material ratio is 4-8:1, and the ball milling is continued for 20-30 minutes. After the ball milling is completed, a once-treated asphalt is obtained, and then vinyl tri(β-methoxyethoxy) silane is added, the temperature is raised to 60-65°C, and stirred for 1.7-2.5 hours. After the stirring is completed, drying is performed to obtain the pretreated asphalt; The mixing step is to heat the pretreated asphalt to 161-165° C., then add modified carbon nanotubes, paraffin oil and phenolic resin for homogenization, the homogenization pressure is 5.0-5.4 MPa, the homogenization time is 3.0-5.0 min, the homogenization times are 3 times, after the homogenization treatment is completed, high-speed shearing treatment is performed, the shearing speed is 6000-7500 rpm, the shearing time is 17-23 min, after the shearing is completed, the modified asphalt is obtained; The mass ratio of the pretreated asphalt, modified carbon nanotubes, paraffin oil and phenolic resin is 47-53:6.3-6.5:2.0-2.4:13-15.
2. The method for preparing modified asphalt according to claim 1, characterized in that: In the first modification step, the particle size of the carbon nanotubes is 5-90 nm.
3. The method for preparing modified asphalt according to claim 1, characterized in that: In the secondary modification step, the mass concentration of the hydrogen peroxide solution is 20-24%; The mass ratio of the primary modified carbon nanotubes, hydrogen peroxide solution, deionized water, ethylene glycol, and PEG-30 glyceryl cocoate is 16-20:137-143:121-130:2.8-3.2:2.0-2.
2.
4. The method for preparing modified asphalt according to claim 1, characterized in that: In the step of the third modification, the mass ratio of the second modified carbon nanotubes to the modified liquid is 10.2-10.4:56-60; In the modified solution, the mass ratio of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane, fatty acid polyoxyethylene ester, and 38-42wt% ethanol solution is 1.1-1.5:0.4-0.6:63-67; The mass ratio of the tertiary modified initial product, toluene and mercaptoethylamine is 8.2-8.6:98-103:2.6-2.
8.
5. The method for preparing modified asphalt according to claim 1, characterized in that: In the step of asphalt pretreatment, the asphalt is a mixture of 20# petroleum asphalt and 90# petroleum asphalt, and the mass ratio of the 20# petroleum asphalt to the 90# petroleum asphalt is 0.8-1.2:1; The mass ratio of the asphalt, polyethylene glycol, castor oil polyoxyethylene ether and vinyl tri(β-methoxyethoxy)silane is 18-22:0.8-1.2:1.3-1.5:1.0-1.
2.
6. Use of the modified asphalt prepared according to any one of the preparation methods of claims 1 to 5 in porous graphite products.