A perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor and its preparation method and application
By constructing an anti-interference sensing interface in an electrochemical sensor and combining molecular imprinting technology, an ultra-sensitive voltammetry sensor for detecting perfluorooctanoic acid in groundwater was prepared, which solves the high cost and complex operation of detection of PFOA equipment in the prior art. The problem has achieved efficient and low-cost on-site inspection.
Patent Information
- Application Number
- CN202411008026.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The prior art has problems of high equipment cost, complex operation and insufficient sensitivity when detecting perfluorooctanoic acid (PFOA) in groundwater. Especially under complex groundwater media, it is difficult to achieve efficient and low-cost on-site inspection.
Perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor, which includes basic electrodes, gold nanoparticles, zwitterionic polypeptide layers and molecular imprinting polymer films, is prepared by electrochemical polymerization using redox active probe molecules and functional monomers to enhance the The recognition ability of PFOA is detected by differential pulse voltammetry.
It realizes high sensitivity, strong anti-interference and convenient operation detection of PFOA in groundwater, low cost, suitable for sample substrates such as surface water, seawater and wastewater, and has high stability and operability.
Smart Images

Figure CN118533933B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical sensors, and in particular to a perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor and a preparation method and application thereof. Background Art
[0002] Since the 1940s, PFAS (perfluoroalkylated substances) have been used in a wide variety of everyday products and industrial applications for their water- and grease-repellent properties. Perfluorooctanoic acid (PFOA), one of the most common perfluorinated substances, has the ability to bind to proteins and accumulate in the body, resulting in a range of harmful effects such as kidney and liver damage, immunotoxicity, reproductive toxicity, and cancer.
[0003] At present, the detection of perfluorooctanoic acid in groundwater relies on the traditional chromatography-mass spectrometry technology. Although this method has high sensitivity, it requires professional technicians to guide the operation of large instruments, and the equipment cost is high and the sample pretreatment time is long. It is worth noting that the electrochemical method has the advantages of high sensitivity, fast response and simple operation, and has been widely used for on-site detection of new environmental pollutants. However, due to the extraordinary chemical stability of PFAS, it is challenging to detect PFAS using conventional electrochemical methods. Therefore, it is of great significance to develop a low-cost, highly portable and reliable electrochemical method for on-site detection of PFOA in various sample matrices such as surface water, seawater, groundwater and wastewater. Molecular imprinting technology, as a specific molecular recognition technology, is often used for directed synthesis to achieve targeted recognition of target molecules. Therefore, for the complex medium conditions of groundwater, constructing an anti-interference electrochemical sensing interface with enhanced electrical signals is one of the important methods to achieve the detection of new halogenated pollutants in groundwater. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor and its preparation method and application. The perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor provided by the present invention has the advantages of high sensitivity, good anti-interference performance, strong stability, high repeatability and high operability.
[0005] The first object of the present invention is to provide a perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor, comprising a base electrode, and gold nanoparticles, a zwitterionic polypeptide layer and a molecular imprinting polymer film (MIP film) sequentially loaded on the surface of the base electrode, wherein the molecular imprinting polymer film comprises a functional monomer and a redox active probe molecule. The molecular imprinting polymer film is prepared using β-CD as a functional monomer, methylene blue as both a functional monomer and a redox active probe, and perfluorooctanoic acid as a template molecule.
[0006] In some embodiments of the present invention, the base electrode is a glassy carbon electrode, a gold electrode or a screen-printed electrode;
[0007] and / or, the redox-active probe molecule is methylene blue (MB);
[0008] And / or, the zwitterionic polypeptide is CPEK, and the sequence is (KE)4(KE)2KEPPPPC;
[0009] And / or, the functional monomer is β-cyclodextrin (β-CD); the functional monomer is bonded to PFOA through host-guest recognition.
[0010] And / or, the particle size of the gold nanoparticles is 30 nm to 45 nm. The gold nanoparticles help to enhance the voltammetric response of the MB probe, and the optimization of the MIP film layer provides a higher peak change.
[0011] In the present invention, the redox active probe molecule has two functions. One is to act as a functional monomer to identify PFOA through hydrophobic interaction; the other is to act as a redox probe. When there is no PFOA in the molecular imprinting membrane, the electrons of PMB (methylene blue polymer) can be quickly transferred in the membrane. After PFOA is recognized, the electron transfer of PMB is blocked, resulting in a decrease in its electrical signal. Therefore, PMB can be used as a redox probe to react to the recognition process of PFOA.
[0012] In the present invention, the redox active probe molecule and the functional monomer respectively form a methylene blue polymer and a beta-cyclodextrin polymer during the polymerization process, and the prepared membrane is a mixed phase of the two polymers.
[0013] The second object of the present invention is to provide a method for preparing the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor, comprising the following steps:
[0014] Gold nanoparticles modify the base electrode to obtain a gold nanoparticle / base electrode;
[0015] Modifying the gold nanoparticle / basic electrode with zwitterionic polypeptide to obtain polypeptide / gold nanoparticle / basic electrode;
[0016] A mixed solution containing a functional monomer, a redox active probe molecule and a perfluorooctanoic acid molecular imprinting template is provided, and an electrochemical polymerization reaction is carried out on the surface of the polypeptide / gold nanoparticle / base electrode by using cyclic voltammetry, and then the perfluorooctanoic acid is eluted in a buffer solution, and finally the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor is obtained.
[0017] In some embodiments of the present invention, the step of modifying the base electrode with gold nanoparticles is as follows: immersing the base electrode in an aqueous solution of chloroauric acid, and obtaining gold nanoparticles / base electrode by chronoamperometry and cyclic voltammetry.
[0018] In some embodiments of the present invention, the concentration of the chloroauric acid aqueous solution is 0.25~1 mM, illustratively, it can be 0.25 mM, 0.5 mM, 1 mM, etc.; the chloroauric acid aqueous solution is prepared using 0.1 M NaClO4.
[0019] The specific steps of gold nanoparticle modification of the base electrode were as follows: First, 4.75 mL of NaClO4 solution (0.1 M) was added to 0.25 mL of chloroauric acid stock solution (10 mM) and prepared by chronoamperometry and cyclic voltammetry.
[0020] And / or, the test conditions of the chronoamperometry are: the initial potential is 0.8 V, the pulse width is 15 s; the test conditions of the cyclic voltammetry are: the potential range is -0.4 V to 0.3 V, the scanning speed is 50 mV / s, and the number of cycles is 50.
[0021] In some embodiments of the present invention, the step of modifying the gold nanoparticles / basic electrode with zwitterionic polypeptides is as follows: dropping the zwitterionic polypeptides onto the surface of the gold nanoparticles / basic electrode and incubating in the dark.
[0022] In some embodiments of the present invention, the concentration of the zwitterionic polypeptide is 0.05 mg / mL to 1 mg / mL; the incubation time is 20 min to 90 min. The main function of the zwitterionic polypeptide is to prevent other ions and organic matter in the water from adhering to the molecular imprinting membrane through the size exclusion effect, thereby reducing the recognition ability of the membrane.
[0023] In some embodiments of the present invention, the molar ratio of the functional monomer, the redox active probe molecule, and the perfluorooctanoic acid molecular imprinting template is (1~2):(1~2):(1~2). For example, it can be (1:1:1), (1:2:1), (1:1:2), (2:1:1), (2:2:1) (1:2:2), (2:1:2), etc.
[0024] In some embodiments of the present invention, the parameters of the electrochemical polymerization reaction are: the number of polymerization cycles in cyclic voltammetry is 3 to 15 cycles, and the scanning rate is 25 to 150 mV / s.
[0025] In some embodiments of the present invention, the specific steps for removing PFOA molecules are as follows: first, the MIP / CPEK / AuNPs / GCE surface is rinsed with deionized water, and eluted in a phosphate buffer solution (PBS) with a pH of 7.4 by CV to remove the PFOA molecules embedded in the imprinted membrane. The elution time is 90 s to 270 s, and illustratively, it can be 90 s, 180 s, 216 s, and 270 s. Finally, the sensor is air-dried and stored.
[0026] By using the above technical scheme, in 5 mM [Fe(CN)6] 3- / 4- Electrochemical impedance spectroscopy and cyclic voltammograms were used to characterize the electron transfer kinetics on different electrode surfaces in 0.1 M KCl solution. Figure 2 Based on the EIS graph, it can be seen that due to the excellent electron transfer ability of AuNPs / GCE, its electrochemical redox current is significantly higher than that of GCE; the effective surface areas of AuNPs / GCE and bare GCE calculated by the Randle-Sevcik equation are 0.095 cm 2 and 0.043cm 2 The prepared molecular imprinted membrane was characterized by cyclic voltammetry. Figure 2 As shown in the figure. It can be seen that in the first cycle diagram, there is a characteristic peak of MB monomer at -0.25 V. As the number of cycles increases, a characteristic peak of MB monomer gradually being oxidized appears at -0.1 V. The oxidation process of MB monomer is related to the formation of cations on its tertiary amine group. In addition, a new anodic peak is generated near +0.45 V, which is related to the formation of PMB. At the same time, during the polymerization of β-CD, clear cathode peaks are shown at -0.58 V and -1.05 V. As the number of cycles increases, the anode has two peaks at 0.72 V and 1.8 V, and increases with the number of cycles, which is related to the oxidation of hydroxyl carbon of β-CD and its further oxidation to carboxylic acid. Subsequently, esterification occurs between carboxylic acid and primary hydroxyl to form a dimer, and finally produces a β-CD polymer film. The CV curve recorded during the electropolymerization process is consistent with the previously reported electrochemical polymerization process, indicating that the MIP membrane was successfully prepared.
[0027] The third object of the present invention is to provide the use of the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor in detecting perfluorooctanoic acid.
[0028] Furthermore, during the preparation process, the MIP / CPEK / AuNPs / GCE was not incubated in the PFOA solution prepared in the laboratory, but was immersed in the groundwater sample for 80 min, and the subsequent DPV test was carried out with the same process.
[0029] Furthermore, in the DPV test, the potential range of the parameters is -0.5 ~ 0V (vs Ag / AgCl), the potential amplitude is 50 mV, the potential increment is 10 mV, the sampling width is 10 ms, and the pulse period is 100 ms.
[0030] Furthermore, the process of electrochemical detection of perfluorooctanoic acid is as follows: the MIP / CPEK / AuNPs / GCE electrochemical sensor measures the electrical signal of the PMB redox probe by using differential pulse voltammetry (DPV). The binding of PFOA to the MIP receptor cavity hinders the transfer of electrons through the adjacent PMB, which leads to a decrease in the electrochemical signal of PMB. Therefore, the change in the PMB oxidation peak indicates the interaction between the MIP membrane and PFOA. The electrochemical measurement process includes pre-washing, incubation and detection. During pre-washing, MIP / CPEK / AuNPs / GCE is gently rinsed with deionized water to clean the electrode surface; during incubation, it is incubated with 5 mL of perfluorooctanoic acid solution of different concentrations for 80 minutes; during detection, the DPV detection process is carried out in 5 mL of 0.2 M PBS with pH=7.0.
[0031] Through the above technical scheme, AuNPs / GCE, CPEK / AuNPs / GCE, MIP / CPEK / AuNPs / GCE and PFOA were identified and characterized by differential pulse voltammetry. The results are shown in Figure 3 As shown, it can be seen that the difference in DPV images after MIP / CPEK / AuNPs / GCE and PFOA recognition indicates that PFOA recognition can hinder the electron transfer on the electrode working surface. Combined with the scanning electron microscopy images of AuNPs / GCE and MIP / CPEK / AuNPs / GCE, as shown Figure 4 As shown, it can be seen that the MIP molecular imprinting sensitive membrane was successfully prepared.
[0032] Principle of the invention: The electrochemical sensor obtained by the invention (such as MIP / CPEK / AuNPs / GCE) uses methylene blue as the probe molecule. When PFOA is present, the electrical signal of PMB is suppressed, resulting in a lower signal response. When PFOA is eluted, the PMB probe is exposed, resulting in a higher current value. The eluted MIP / CPEK / AuNPs / GCE is measured by differential pulse voltammetry (DPV), and the signal change of the PMB probe before and after PFOA incubation is used to quantitatively analyze the PFOA concentration in the water sample.
[0033] The above technical solution of the present invention has the following advantages compared with the prior art:
[0034] 1. Based on GCE, the present invention constructs an anti-interference sensing interface and combines molecular imprinting recognition technology to prepare an ultra-sensitive voltammetric sensor for detecting perfluorooctanoic acid in groundwater. Among them, the surface of the GCE electrode is modified by AuNPs, which helps to enhance the electrical signal of the selected redox probe PMB. The CPEK sequence polypeptide is used to construct an anti-interference sensing interface to prevent the attachment of other organic matter and ions in groundwater. The MIP membrane modification is used for the recognition of perfluorooctanoic acid, and the optimization of the MIP layer provides a higher peak change. At the same time, the developed sensor has comparable analytical performance with high performance liquid chromatography tandem mass spectrometry in groundwater. The electrochemical sensor obtained by the present invention is used to detect PFOA in groundwater, and has the advantages of convenient operation, rapid response, high sensitivity, strong specificity, good stability and anti-interference.
[0035] 2. The present invention uses scanning electron microscopy (SEM) to characterize the surface morphology of AuNPs / GCE and MIP / CPEK / AuNPs / GCE, and studies the electrochemical behaviors of GCE, AuNPs / GCE and CPEK / AuNPs / GCE by electrochemical impedance spectroscopy (EIS) and cyclic voltammetry (CV). Differential pulse voltammetry is used to study the removal of PFOA by AuNPs / GCE, CPEK / AuNPs / GCE, and MIP / CPEK / AuNPs / GCE, and the electrical signal of PFOA recognition by MIP / CPEK / AuNPs / GCE. In addition, differential pulse voltammetry (DPV) is also used to study the electrochemical properties of AuNPs / GCE, CPEK / AuNPs / GCE, and MIP / CPEK / AuNPs / GCE in the range of 10 nM to 100 uM. The MIP electropolymerization process is optimized to minimize potential passivation and analyte saturation on the electrode surface, which is of great significance for on-site detection of PFAS in various sample matrices such as surface water, seawater, wastewater and sludge. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0037] Figure 1 The electrochemical impedance spectroscopy and cyclic voltammograms of CPEK / AuNPs / GCE, AuNPs / GCE and GCE of the present invention are shown;
[0038] Figure 2 is the cyclic voltammogram of the MIP / CPEK / AuNPs / GCE polymerization of the present invention;
[0039] Figure 3The differential pulse voltammograms of AuNPs / GCE, CPEK / AuNPs / GCE, MIP / CPEK / AuNPs / GCE (PFOA removal) and MIP / CPEK / AuNPs / GCE (after PFOA identification) of the present invention;
[0040] Figure 4 The scanning electron micrographs of AuNPs / GCE and MIP / CPEK / AuNPs / GCE of the present invention;
[0041] Figure 5 The differential pulse voltammogram and calibration curve in the PFOA concentration range of 10nM to 100uM of the present invention;
[0042] Figure 6 The selectivity of the MIP / CPEK / AuNPs / GCE sensor of the present invention for PFOA. DETAILED DESCRIPTION
[0043] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0044] Embodiment 1:
[0045] The preparation and application of the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor provided in this embodiment include the preparation of gold nanoparticles / glassy carbon electrode (AuNPs / GCE) S1, the preparation of anti-interference sensing interface polypeptide / gold nanoparticles / glassy carbon electrode (CPEK / AuNPs / GCE) S2, the preparation of anti-interference molecular imprinting sensor MIP / CPEK / AuNPs / GCE S3 and the analysis and detection of perfluorooctanoic acid S4, as shown below:
[0046] (1) Preparation of gold nanoparticles / glassy carbon electrode AuNPs / GCE S1 The operation steps are as follows:
[0047] AS1: The glassy carbon electrode (GCE) was first polished using 0.3 μm and 0.05 μm alumina slurries as the polishing material, and then ultrasonicated in ultrapure water for 10 min.
[0048] BS1: The GCE obtained in step AS1 was immersed in a 0.5 mM HAuCl4 aqueous solution (prepared with 0.1 M NaClO4) and AuNPs / GCE was prepared by chronoamperometry and cyclic voltammetry.
[0049] (2) Preparation of the anti-interference sensing interface peptide / gold nanoparticles / glassy carbon electrode (CPEK / AuNPs / GCE) S2 operation steps are as follows:
[0050] 0.05 mg / mL, 0.1 mg / mL, 0.2 mg / mL, 0.5 mg / mL, and 1 mg / mL of a zwitterionic peptide with the sequence (KE)4(KE)2KEPPPPC were dropped onto the surface of the AuNPs / GCE electrode and incubated in the dark at room temperature for 50 min to obtain the corresponding CPEK / AuNPs / GCE.
[0051] (3) Preparation of anti-interference molecular imprinting sensor MIP / CPEK / AuNPs / GCE S3 The operation steps are as follows;
[0052] AS3: First, prepare 20 mL of phosphate buffer solution (pH=7.0) containing β-cyclodextrin (0.0227 g) and methylene blue (0.0128 g) functional monomer materials and target molecule perfluorooctanoic acid (0.0166 g) molecular imprinting template, and then use cyclic voltammetry CV to carry out electrochemical polymerization. The polymerization conditions are: 10 CV cycles in the potential range of −2.0 V to +2.2 V at a scan rate of 100 mV / s to obtain MIP / CPEK / AuNPs / GCE;
[0053] BS3: Secondly, the electrochemical polymerization parameters were optimized, which included simultaneously changing and analyzing the three main influencing factors: the molar ratio of monomer material / imprint template, the number of CV cycles and the scanning speed. Among them, the molar ratio of β-cyclodextrin, redox active probe molecule and perfluorooctanoic acid molecule was 1:2:2, the number of CV cycle polymerization circles was 10, and the scanning speed was 100 mV / s.
[0054] CS3: After the electropolymerization was completed, the MIP / CPEK / AuNPs / GCE surface was first rinsed with deionized water, and the PFOA molecules embedded in the molecular imprinting sensitive membrane were removed by scanning for 180 s in the range of 0-0.9 V using cyclic voltammetry. Finally, the sensing interface was dried and stored.
[0055] In 5 mM [Fe(CN)6] 3- / 4- Electrochemical impedance spectroscopy and cyclic voltammetry were used to characterize the electrochemical behaviors of CPEK / AuNPs / GCE, AuNPs / GCE and GCE in solution. Figure 1 As shown in the EIS graph, as AuNPs are deposited on the electrode surface, the electron transfer ability of AuNPs / GCE is enhanced, and its R ctThe CV current increased. With the modification of CPEK peptide ((KE)4(KE)2KEPPPPC) on the electrode surface, the electrochemical impedance value increased significantly, and the current value in the CV graph decreased significantly. In addition, the effective surface areas of AuNPs / GCE and bare GCE were calculated to be 0.095 cm 2 and 0.043 cm 2 , M.I. P The polymerization was characterized by cyclic voltammetry, and the results were as follows Figure 2 As shown in the figure, in the first cycle diagram, there is a characteristic peak of methylene blue monomer at -0.25 V. As the number of cycles increases, a characteristic peak of methylene blue monomer gradually being oxidized appears at -0.1 V. The oxidation of methylene blue monomer is related to the cation formed by the tertiary amine group in its structure. In addition, a new anodic peak is generated near +0.45 V, which is related to the formation of polymethylene blue (PMB). At the same time, during the polymerization of β-CD, clear cathode peaks are shown at -0.58 V and -1.05 V. As the number of cycles increases, the anode has two peaks at 0.72 V and 1.8 V, and the peaks increase with the number of cycles, which is related to the oxidation of the hydroxyl carbon of β-CD and its further oxidation to carboxylic acid. Subsequently, esterification occurs between the carboxylic acid and the primary hydroxyl group to form a dimer and finally produce poly-β-CD.
[0056] (4) The S4 operation steps for the analysis and detection of perfluorooctanoic acid are as follows:
[0057] AS4: The MIP / CPEK / AuNPs / GCE electrochemical sensor measures the electrical signal of the PMB redox probe by differential pulse voltammetry (DPV). The binding of PFOA to the MIP receptor cavity hinders the transfer of electrons through the adjacent PMB, which leads to a decrease in the electrochemical signal of PMB. Therefore, the change in the PMB oxidation peak indicates the interaction between the MIP membrane and PFOA. The electrochemical measurement process includes pre-washing, incubation and detection. During pre-washing, MIP / CPEK / AuNPs / GCE was gently rinsed with deionized water to clean the electrode surface; during incubation, it was incubated with 5 mL of perfluorooctanoic acid solution of different concentrations for 80 minutes; during detection, the DPV detection process was detected in 5 mL of 0.2 M PBS with pH=7.0.
[0058] The removal of PFOA by AuNPs / GCE, CPEK / AuNPs / GCE, and MIP / CPEK / AuNPs / GCE and the recognition of PFOA by MIP / CPEK / AuNPs / GCE were characterized by differential pulse voltammetry. The results are shown in Figure 3As shown in the figure, it can be seen that at around -0.28 V, bare GCE, AuNPs / GCE, and CPEK / AuNPs / GCE have no current response. After the molecular imprinting MIP membrane is polymerized, an obvious current response appears, indicating that the electrical signal is generated by the PMB in the molecular imprinting MIP membrane. Furthermore, since PFOA hinders the electron transfer in the MIP cavity after recognition, its current value is significantly reduced. AuNPs / GCE and MIP / CPEK / AuNPs / GCE are characterized by scanning electron microscopy. Figure 4 As shown, it can be seen that the existence of the MIP membrane before and after electropolymerization is confirmed by SEM images.
[0059] Embodiment 2
[0060] Similar to Example 1, the difference is that in step (2), the incubation time at room temperature in the dark is 20 min, 30 min, 60 min, and 90 min, respectively, to obtain the corresponding CPEK / AuNPs / GCE.
[0061] Embodiment 3
[0062] Similar to Example 1, the difference is that in step (3) BS3, the ratios of β-cyclodextrin, redox active probe molecule and perfluorooctanoic acid molecule are adjusted to 1:1:1, 1:2:1, 1:1:2, 2:1:1, 2:2:1 and 2:1:2 respectively.
[0063] Embodiment 4
[0064] Similar to Example 1, the difference is that in step (3) BS3, the number of CV cycle polymerization cycles is adjusted to 3, 5, 12, and 15, respectively.
[0065] Embodiment 5
[0066] Similar to the first embodiment, the difference is that in step (3) BS3, the scanning speed is 25 mV / s, 50 mV / s, and 150 mV / s.
[0067] Test example:
[0068] The MIP / CPEK / AuNPs / GCE obtained in Example 1 was used for PFOA detection in groundwater. Instead of incubating in the PFOA solution prepared in the laboratory, it was immersed in the groundwater sample for 80 minutes and then subjected to subsequent DPV testing using the same process. The experimental results are shown in Figure 2. Figure 5 shown.
[0069] The DPV test has a potential range of -0.5 to 0 V (vs Ag / AgCl), a potential amplitude of 4 mV, a potential increment of 50 mV, a sampling width of 50 ms, and a pulse period of 500 ms.
[0070] The differential pulse voltammogram and calibration curve in the concentration range of 10 nM~100 uM PFOA are shown in the figure below. Figure 5 As shown in the figure, it can be seen that the oxidation peak of PMB decreases gradually at about -0.28V with the increase of PFOA concentration. The calibration curve shows that in the range of 10 nM~100 uM PFOA, the developed sensor has a high sensitivity to PFOA, and the correlation coefficient R 2 It is 0.9905.
[0071] When in use, in the preparation S1 of gold nanoparticles / glassy carbon electrode (AuNPs / GCE), the preparation S2 of anti-interference sensing interface polypeptide / gold nanoparticles / glassy carbon electrode (CPEK / AuNPs / GCE), the preparation S3 of anti-interference molecular imprinting sensor MIP / CPEK / AuNPs / GCE and the analysis and detection S4 of perfluorooctanoic acid, the preparation and detection were carried out according to AS1, BS1, AS2, AS3, BS3, CS3 and AS4 respectively. In the preparation S1 of gold nanoparticles / glassy carbon electrode (AuNPs / GCE), the electrochemical behavior of AuNPs / GCE was characterized by CV and impedance. The current value was significantly higher than that of bare GCE, indicating that AuNPs helped to enhance the electrical signal of the selected redox probe PMB. The effective surface areas of AuNPs / GCE and bare GCE were calculated by Randle-Sevcik equation to be 0.095 cm 2 and 0.043 cm 2 . At the same time, in the preparation process of the anti-interference sensing interface polypeptide / gold nanoparticles / glassy carbon electrode (CPEK / AuNPs / GCE) S2, the formation exclusion effect of the CPEK interface was used to prevent the attachment of other organic matter and ions in the groundwater. During the preparation process of the anti-interference molecular imprinting sensor MIP / CPEK / AuNPs / GCE S3, the PMB-PCD / PFOA polymerization was characterized by cyclic voltammetry, indicating that the MIP membrane was successfully prepared. In the process of perfluorooctanoic acid PFOA analysis and detection S3, AuNPs / GCE, CPEK / AuNPs / GCE, MIP / CPEK / AuNPs / GCE (PFOA removal) and MIP / CPEK / AuNPs / GCE (PFOA recognition) were characterized by differential pulse voltammetry, and the results are as follows. Figure 3As shown in the figure, it can be seen that near -0.28 V, AuNPs / GCE and CPEK / AuNPs / GCE have no current response, and an obvious current response appears after the molecular imprinting membrane is polymerized, indicating that the electrical signal is generated by the PMB in the molecular imprinting MIP membrane. Furthermore, since PFOA hinders the electron transfer in the MIP cavity after recognition, its current value is significantly reduced. AuNPs / GCE and MIP / CPEK / AuNPs / GCE were characterized by scanning electron microscopy, combined with Figure 4 As shown, it can be seen that the existence of the MIP membrane before and after electropolymerization is confirmed by SEM images. The experimental equipment and conditions are low, the cost is low, the operation is safe and simple, and the prepared electrochemical sensor is convenient to operate, responds quickly, has high sensitivity, strong specificity, good stability and anti-interference, and the electrochemical sensor has good current response, strong stability, high repeatability and high operability.
[0072] Perfluorononanoic acid (PFNA), tridecafluoroheptanoic acid (PFHPA), and nonadecafluorodecanoic acid (PFDA) were selected as interfering substances to study the selectivity of the prepared MIP / CPEK / AuNPs / GCE sensor for PFOA. The experimental results are shown in Figure 6 Since the template molecule used in the synthesis of the MIP / CPEK / AuNPs / GCE sensor is PFOA, the MIP / CPEK / AuNPs / GCE can specifically recognize perfluorooctanoic acid for PFOA, but has no recognition performance for other substances, indicating that the MIP / CPEK / AuNPs / GCE sensor obtained by the present invention has good selective recognition ability for PFOA.
[0073] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor, characterized in that: The invention comprises a basic electrode, and gold nanoparticles, a zwitterionic polypeptide layer and a molecular imprinting polymer film which are sequentially loaded on the surface of the basic electrode, wherein the molecular imprinting polymer film comprises a β-cyclodextrin polymer and a methylene blue polymer, and the sequence of the zwitterionic polypeptide is (KE)4(KE)2KEPPPPC; wherein β-cyclodextrin and methylene blue are functional monomers, and methylene blue is a redox active probe molecule, and the functional monomer is bonded to PFOA through host-guest recognition; and the particle size of the gold nanoparticles is 30-45 nm.
2. The perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor according to claim 1, characterized in that: The basic electrode is a glassy carbon electrode, a gold electrode or a screen-printed electrode.
3. A method for preparing the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor according to claim 1 or 2, characterized in that: The following steps are involved: Gold nanoparticles modify the base electrode to obtain a gold nanoparticle / base electrode; Modifying the gold nanoparticle / basic electrode with zwitterionic polypeptide to obtain polypeptide / gold nanoparticle / basic electrode; A mixed solution containing β-cyclodextrin, methylene blue and perfluorooctanoic acid molecular imprinting template is provided, and an electrochemical polymerization reaction is carried out on the surface of the polypeptide / gold nanoparticle / base electrode by cyclic voltammetry, and perfluorooctanoic acid is eluted in a buffer solution, and finally the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor is obtained; the molar ratio of the β-cyclodextrin, methylene blue and perfluorooctanoic acid molecular imprinting template is (1-2): (1-2): (1-2).
4. The preparation method according to claim 3, characterized in that: The steps of modifying the base electrode with gold nanoparticles are as follows: immersing the base electrode in an aqueous solution of chloroauric acid, and obtaining a gold nanoparticle / base electrode by chronoamperometry and cyclic voltammetry.
5. The preparation method according to claim 4, characterized in that: The concentration of the chloroauric acid aqueous solution is 0.25 mM~1 mM.
6. The preparation method according to claim 3, characterized in that: The step of modifying the gold nanoparticle / basic electrode surface with zwitterionic polypeptide is as follows: dropping the zwitterionic polypeptide onto the surface of the gold nanoparticle / basic electrode and incubating in the dark to obtain the product.
7. The preparation method according to claim 6, characterized in that: The concentration of the zwitterionic polypeptide is 0.05-1 mg / mL; the incubation time is 20-90 min.
8. The preparation method according to claim 3, characterized in that: Parameters of electrochemical polymerization reaction: the number of polymerization cycles of cyclic voltammetry is 3 to 15 cycles, and the scanning speed is 25 to 150 mV / s.
9. Use of the perfluorooctanoic acid anti-interference electrochemical molecular imprinting sensor according to claim 1 or 2 in detecting perfluorooctanoic acid.
Citation Information
Cited By
Screen-printed electrode assembly, preparation method thereof, molecularly imprinted field effect transistor sensor and application of molecularly imprinted field effect transistor sensor
CN121805357A