A graphene printed radio frequency identification tag and preparation method thereof

By using a mixed solvent of dihydroglucosone and triacetin to treat graphene, a highly stable slurry is formed, which solves the problems of graphene's instability in aqueous solvents and the toxicity of alternative solvents, achieving low-cost, environmentally friendly, and Preparation of high-performance graphene printed radio frequency identification tags.

CN118536534BActive Publication Date: 2024-10-18CANGNAN ANTE SECURITY TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411010320.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-18
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Existing graphene is unstable in aqueous solvents. Alternative solvents such as sodium lauryl sulfate and n-methylpyrrolidone are toxic to the human body, and the solubility of dihydroglucosone is not enough to improve the stability of graphene nanosheets. , limiting the application of radio frequency antennas.

Method used

A mixed solvent of dihydroglucosone and triacetin is used as the stripping solvent for graphene and the ink carrier. Highly stable graphene slurry is formed through microwave treatment, ultrasonic stripping and centrifugation for printing ultra-high frequency radio frequency identification. Label.

Benefits of technology

It achieves high peeling efficiency and stability of graphene nanosheets, reduces production costs, and the solvent combination is non-toxic, suitable for the application of radio frequency antennas and tags, and has the advantages of environmental protection, low cost and high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118536534B_ABST
    Figure CN118536534B_ABST
Patent Text Reader

Abstract

The present invention discloses a graphene printed radio frequency identification label and a preparation method thereof. The label comprises a substrate, an antenna frame, a chip and a slurry. The antenna frame is an antenna structure processed from a silk screen. The antenna frame is placed on the substrate. The slurry is silk-screened on the surface of the antenna frame along a first direction to form a printed antenna. After the printed antenna is rolled, the chip is encapsulated in the center of the printed antenna to form a graphene printed radio frequency identification label. The graphene in the label uses a mixed solvent of dihydro-levorotatory glucose ketone and triacetin as a stripping solvent and an ink carrier, and has the advantages of low cost, non-toxicity, high stripping efficiency, high stability, and high performance. At the same time, the present invention also provides a preparation method, by using a mixed solvent of dihydro-levorotatory glucose ketone and triacetin as a stripping solvent and an ink carrier to prepare a printed label, the radio frequency identification label obtained by the method has the advantages of low cost, environmental protection, and high preparation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of radio frequency tags, and in particular to a graphene printed radio frequency identification tag and a preparation method thereof. Background Art

[0002] Printed RFID antennas form antenna structures by applying conductive paste to different substrates through printing. This processing technology has many advantages over the current mainstream metal acid-etched antenna processing technology, such as no pollution, high production efficiency, simple process, wide application range, stretchability, and bending resistance. Conductive paste is the core material of this type of processing technology, among which silver paste is the most commonly used conductive paste, which has the advantages of low resistance and high stability. However, the high price of silver powder will increase the cost of the antenna and limit its application range. Low-dimensional carbon materials, such as graphene and carbon nanotube paste, currently show the potential to replace low-temperature silver paste in the field of antenna processing due to their low cost.

[0003] China's public patent number CN117613537A (graphene film for RFID antenna, graphene RFID antenna and its preparation method and application) describes a method of printing radio frequency antenna through water-based graphene. China's public patent number (CN114590801A) uses n-methylpyrrolidone as a graphene carrier to achieve antenna printing. China's public patent number CN117735536A (a graphene RFID tag and its preparation method and application), SCI journal Nature Communication (DOI: 10.1038 / s41467-018-07632-w) and others describe graphene exfoliation and radio frequency antenna printing based on dihydro-levorotatory glucose ketone.

[0004] Water-based graphene is environmentally friendly and non-biotoxic, but graphene is highly unstable in water and requires surfactants such as sodium dodecyl sulfate and polyvinyl pyrrolidone to prevent secondary stacking of graphene, but surfactants will significantly reduce the conductivity of graphene. The use of solvents such as n-methylpyrrolidone (NMP) and dimethylacetamide (DMF) can avoid the use of surfactants, but the residues of the above solvents are highly toxic to the human body (listed as Very High Concern for reproductive toxicity in the EU) and are not suitable for the application of radio frequency antennas and tags. Cyrene is a green alternative to NMP. Although it has a higher solubility in graphene, the stability of graphene nanosheets in this solvent is still weaker than the former. Summary of the invention

[0005] The present invention provides a graphene printed radio frequency identification tag, which realizes the Hansen parameter correction of the solvent by combining dihydro-levorotatory glucosone and triacetin, improves the stripping efficiency and stability of graphene nanosheets, and prints an ultra-high frequency radio frequency identification tag based on the solvent slurry. The graphene in the tag uses a mixed solvent of dihydro-levorotatory glucosone and triacetin as a stripping solvent and ink carrier, and has the advantages of low cost, non-toxicity, high stripping efficiency, high stability, high performance, etc.

[0006] At the same time, the present invention also provides a method for preparing the above-mentioned graphene printed radio frequency identification label, by using a mixed solvent of dihydro-levulinone and triacetin as a stripping solvent and an ink carrier to prepare a printed label, and the radio frequency identification label obtained by this method has the advantages of low cost, environmental protection, and high preparation efficiency.

[0007] The technical solution provided by the present invention is as follows:

[0008] The present invention provides a graphene printed radio frequency identification tag, comprising:

[0009] Substrate, antenna frame, chip and paste;

[0010] The antenna frame is an antenna structure processed by a silk screen, the antenna frame is placed on the substrate, the slurry is silk-screened on the surface of the antenna frame along a first direction to form a printed antenna, the printed antenna is rolled and then the chip is packaged in the center of the printed antenna to form the graphene printed RFID tag;

[0011] The slurry is graphene slurry, and the components and their mass percentages of the graphene slurry are:

[0012] 10~15wt% graphene;

[0013] 1~3 wt% cellulose acetate butyrate;

[0014] 15~25 wt% triacetin;

[0015] 60~70 wt% dihydrolevorotatory glucosone.

[0016] Furthermore, the components of the graphene slurry and their mass percentages are:

[0017] 13 wt% graphene;

[0018] 2 wt% cellulose acetate butyrate;

[0019] 20 wt% triacetin;

[0020] 65 wt% dihydrolevorotatory glucosone.

[0021] Further, the wire mesh is an 80-mesh wire mesh;

[0022] The substrate includes at least one of PET, paper, TPU and PI.

[0023] Furthermore, the viscosity of the graphene slurry is 5-13 mPa·s.

[0024] Furthermore, the chip is an NXP UCODE 8 chip, and the chip is welded to the center of the printed antenna through a packaging machine.

[0025] At the same time, the present invention also provides a graphene printed radio frequency identification tag and a preparation method thereof, which is used for the above-mentioned graphene printed radio frequency identification tag, comprising the following steps:

[0026] Prepare graphene slurry, wherein the components and their mass percentages in the prepared graphene slurry are: 13 wt% graphene, 2 wt% cellulose acetate butyrate, 20 wt% glyceryl triacetate, and 65 wt% dihydro-levorotatory glucosone, and the viscosity of the graphene slurry is 5-13 mPa·s;

[0027] Selecting an antenna frame, preparing a substrate, placing the antenna frame on the substrate, scraping the graphene slurry on the antenna frame along a first direction, and drying to form a printed antenna;

[0028] The printed antenna is rolled and then glued by a glue dispenser, a chip is welded at the center of the printed antenna after glue dispensing, and the graphene printed radio frequency identification tag is formed after heat pressing.

[0029] Furthermore, the preparation of graphene slurry comprises the following steps:

[0030] Forming expanded graphite by intercalating expandable graphite flakes through microwave treatment;

[0031] Dihydro-levorotatory glucosone and triacetin are mixed in a weight ratio of 3.4:1 to form a graphene exfoliation solvent;

[0032] The expanded graphite is coarsely ground, and then the stripping solvent is added, and then ultrasonic stripping is performed to form a graphene dispersion;

[0033] The graphene dispersion is subjected to low-speed centrifugation to remove unsuccessfully exfoliated graphite, and then subjected to high-speed centrifugation to obtain a graphene sediment;

[0034] vacuum drying the graphene deposit to obtain graphene powder;

[0035] 0.05 parts by weight of the graphene powder is added to 1 part by weight of the graphene exfoliation solvent, and the mixture is stirred. Then, 0.05 parts by weight of the graphene powder is added, and after continuous stirring, 0.04 parts by weight of the graphene powder and 0.02 parts by weight of cellulose acetate butyrate are added, and the graphene slurry is formed after ultrasonication and stirring.

[0036] Further, the expanded graphite is coarsely ground by using a grinder at a rotation speed of 300 rpm for 1 hour;

[0037] The expanded graphite is coarsely ground and then added with the stripping solvent at 10 mg / ml;

[0038] The graphene dispersion is formed by ultrasonic exfoliation in a 180W 40kHz ultrasonic bath for 8 hours.

[0039] Further, the graphene dispersion is subjected to low-speed centrifugation to remove unsuccessfully exfoliated graphite, and then subjected to high-speed centrifugation to obtain a graphene sediment, specifically:

[0040] The graphene dispersion was subjected to two low-speed centrifugation treatments at 300 rpm for 10 minutes to obtain the supernatant, the dispersion after centrifugation was passed through a 300-mesh steel sieve to remove the unstripped graphite, and then subjected to high-speed centrifugation treatment at 1500 rpm for 10 minutes to obtain the sediment.

[0041] Furthermore, the antenna frame is processed by using 80 mesh screen;

[0042] The graphene slurry was stirred at 1000 rpm for 10 minutes before printing;

[0043] The conditions for drying to form the printed antenna are: drying at 125° C. for 15 minutes;

[0044] The printing antenna is rolled by: rolling the printed antenna three times with a metal roller at 165° C. and 6 MPa;

[0045] The hot pressing was performed under the conditions of 140° C. for 15 seconds.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The present invention provides a graphene printed radio frequency identification tag, which includes a substrate, an antenna frame, a chip and a slurry. The antenna frame is an antenna structure processed from a screen, the antenna frame is placed on the substrate, the slurry is screen-printed on the surface of the antenna frame along a first direction to form a printed antenna, and the printed antenna is rolled and then the chip is encapsulated in the center of the printed antenna to form a graphene printed radio frequency identification tag. The graphene in the tag uses a mixed solvent of dihydro-levorotatory glucosone and triacetin as a stripping solvent and ink carrier, and has the advantages of low cost, non-toxicity, high stripping efficiency, high stability, high performance, etc.

[0048] At the same time, the present invention also provides a method for preparing the above-mentioned graphene printed radio frequency identification label, by using a mixed solvent of dihydro-levulinone and triacetin as a stripping solvent and an ink carrier to prepare a printed label, and the radio frequency identification label obtained by this method has the advantages of low cost, environmental protection, and high preparation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 The Hansen space diagram of graphene and solvent and the relative solubility parameter diagram of solvent in the embodiment of the present invention, wherein (a) is the Hansen space diagram of graphene and solvent. (b) is the relative solubility parameter diagram of solvent;

[0050] Figure 2 This is a Raman comparison diagram of graphite before and after exfoliation in an embodiment of the present invention;

[0051] Figure 3 The following are the structure diagram of the printed antenna and the electron scanning microscope image of the surface of the printed antenna in the embodiment of the present invention, wherein (a) is the structure diagram of the printed graphene antenna, and (b) is the electron scanning microscope image of the surface of the antenna. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the embodiments described below are part of the embodiments of the present application, rather than all of the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.

[0053] Therefore, the detailed description of the embodiments of the present application provided below in conjunction with the accompanying drawings is intended to represent only selected embodiments of the present application, and is not intended to limit the scope of protection claimed in the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0054] The invention provides a graphene printed radio frequency identification tag, comprising a substrate, an antenna frame, a chip and slurry.

[0055] The antenna frame is an antenna structure processed by a screen. The antenna frame is placed on a substrate. The slurry is screen-printed on the surface of the antenna frame along a first direction to form a printed antenna. After the printed antenna is rolled, the chip is packaged in the center of the printed antenna to form a graphene printed RFID tag. The first direction is a vertical direction. The slurry is a graphene slurry, and the components of the graphene slurry and their mass percentages are:

[0056] 10~15wt% graphene;

[0057] 1~3 wt% cellulose acetate butyrate;

[0058] 15~25 wt% triacetin;

[0059] 60~70 wt% dihydrolevorotatory glucosone.

[0060] Among them, graphene is a conductive phase, providing the electronic signal transmission path required by the antenna. Cellulose acetate butyrate is a binder to improve the stability of graphene on the substrate. Too much cellulose acetate butyrate will reduce the conductivity of graphene. Triacetin and dihydro-L-glucose ketone are graphene solvents, which are used for the exfoliation and dispersion of graphene nanosheets.

[0061] Optionally, the components of the graphene slurry and their mass percentages are:

[0062] 13 wt% graphene;

[0063] 2 wt% cellulose acetate butyrate;

[0064] 20 wt% triacetin;

[0065] 65 wt% dihydrolevorotatory glucosone.

[0066] Optionally, the screen is an 80-mesh screen; and the substrate includes at least one of PET, paper, TPU, and PI.

[0067] Optionally, the viscosity of the graphene slurry is 5-13 mPa·s.

[0068] Optionally, the chip is an NXP UCODE 8 chip, and the chip is soldered to the center of the printed antenna by a packaging machine.

[0069] At the same time, the present invention also provides a method for preparing a graphene printed radio frequency identification tag, which is used for the above-mentioned graphene printed radio frequency identification tag, comprising the following steps:

[0070] Step S1, preparing graphene slurry, wherein the components and their mass percentages in the prepared graphene slurry are: 13 wt% graphene, 2 wt% cellulose acetate butyrate, 20 wt% glyceryl triacetate, and 65 wt% dihydro-levulinic acid ketone, and the viscosity of the graphene slurry is 5-13 mPa·s.

[0071] Step S2: Select an antenna frame, prepare a substrate, place the antenna frame on the substrate, scrape the graphene slurry on the antenna frame along a first direction, and dry it to form a printed antenna.

[0072] Step S3, rolling the printed antenna, and then using a glue dispenser to dispense glue, welding a chip in the center of the printed antenna after dispensing glue, and forming a graphene printed radio frequency identification tag after hot pressing.

[0073] Optionally, preparing the graphene slurry comprises the following steps:

[0074] Step S101, forming expanded graphite by intercalating expandable graphite flakes through microwave treatment.

[0075] Step S102, dihydro-levorotatory glucosone and triacetin are mixed in a weight ratio of 3.4:1 to form a graphene exfoliation solvent.

[0076] Step S103, after the expanded graphite is coarsely ground, a stripping solvent is added, and then ultrasonic stripping is performed to form a graphene dispersion.

[0077] Step S104: performing low-speed centrifugation on the graphene dispersion to remove unsuccessfully exfoliated graphite, and then performing high-speed centrifugation to obtain a graphene sediment.

[0078] Step S105: vacuum drying the few-layer graphene deposit to obtain graphene powder.

[0079] Step S106, adding 0.05 parts by weight of graphene powder to 1 part by weight of graphene exfoliation solvent, stirring, then adding 0.05 parts by weight of graphene powder, continuing to stir, then adding 0.04 parts by weight of graphene powder and 0.02 parts by weight of cellulose acetate butyrate, performing ultrasonication and stirring to form a graphene slurry.

[0080] Optionally, in step S103, the expanded graphite is coarsely ground by a grinder at 300 rpm for 1 hour. After the expanded graphite is coarsely ground, a stripping solvent is added at 10 mg / ml; and the graphene dispersion is formed by ultrasonic stripping in a 180W 40kHz ultrasonic pool for 8 hours.

[0081] Optionally, in step S104, the graphene dispersion is subjected to low-speed centrifugation to remove graphite that has not been successfully stripped, and then subjected to high-speed centrifugation to obtain a graphene sediment, specifically: the graphene dispersion is subjected to two low-speed centrifugation treatments, the centrifugation conditions are 300 rpm for 10 minutes to obtain the supernatant, the dispersion after centrifugation is passed through a 300-mesh steel sieve to remove graphite that has not been successfully stripped, and then subjected to high-speed centrifugation treatment, the centrifugation conditions are 1500 rpm for 10 minutes to obtain the sediment.

[0082] Optionally, in step S2, the antenna frame is processed by using a 80-mesh screen. The conditions for drying to form the printed antenna are: drying at a temperature of 125° C. for 15 minutes.

[0083] In step S3, the graphene slurry is stirred at 1000 rpm for 10 minutes before printing. The printed antenna is rolled as follows: the printed antenna is rolled three times with a metal roller at 165° C. and 6 MPa;

[0084] The hot pressing was performed under the conditions of 140° C. for 15 seconds. Example 1

[0085] This embodiment provides a method for preparing a graphene printed radio frequency identification tag, comprising the following steps:

[0086] Step 1. Treat the intercalated expandable graphite flakes with 800W microwaves (2.45GHz) for 45 seconds to form expanded graphite. Under this condition, the volume of the graphite flakes expands significantly without ablation (observed with the naked eye), indicating that the π-π stacking force between graphite layers is weakened.

[0087] Step 2. Mix dihydro-levorotatory glucosone and triacetin in a weight ratio of 3.4:1 (the molar ratio after fusion is 2:1) to form a graphene exfoliation solvent, and calculate the Hansen parameters (such as Figure 1 The results (shown) and experimental results (reference to comparative example) both show that the solubility and stability of the solvent for single-layer graphene are optimal under this ratio. Figure 1 (a) in the figure is the Hansen space diagram of graphene and solvent. The shorter the spatial distance between the solvent and graphene, the higher the stripping efficiency and stability. Figure 1 (b) in the figure is the relative solubility parameter of the solvent (graphene is 1). The closer the solubility parameter is to 1, the better the solubility.

[0088] Step 3. After the expanded graphite is coarsely ground (300rpm for 1 hour), grinding for too long or too fast will introduce defects, and grinding too short will reduce the subsequent stripping efficiency. The ground expanded graphite is added with a stripping solvent at 10 mg / ml, and the expanded graphite-stripping solvent mixture is ultrasonically stripped in a 180W 40kHz ultrasonic bath for 8 hours to form a graphene dispersion. During the stripping process, ice cubes are continuously added to the ultrasonic bath to cool down and prevent oxidation.

[0089] Step 4. The graphene dispersion is subjected to two low-speed centrifugation treatments at 300 rpm for 10 minutes to obtain the supernatant, and the dispersion after centrifugation is passed through a 300-mesh steel sieve to remove the graphite that has not been successfully exfoliated, and then subjected to high-speed centrifugation treatment at 1500 rpm for 10 minutes to obtain the sediment and remove the undersized graphene fragments.

[0090] Step 5. The graphene deposit was vacuum dried at 200°C, 300Pa, for 2 hours. The graphene exfoliated by this method was weighed to yield 53% of the original expanded graphite weight, with few layers and no defects (Raman spectroscopy, such as Figure 2 as shown). Figure 2 This is a Raman comparison of graphite before and after exfoliation. The absence of a D peak (near 1350cm-1) in Raman indicates that no defects were introduced by exfoliation. The 2D peak of unexfoliated graphite (near 2700cm-1) has obvious side peaks, which is a characteristic of graphite. After exfoliation, the side peaks disappear, which is a characteristic of graphene.

[0091] Step 6. Add 0.05 parts by weight of dried graphene powder to 1 part by weight of stripping solvent and stir at 500 rpm. After stirring for 20 minutes, add another 0.05 parts by weight of graphene powder. After continuing stirring for 20 minutes, add 0.04 parts by weight of graphene powder and 0.02 parts by weight of cellulose acetate butyrate (the final weight is 65% dihydro-levulinone, 20% triacetin, 13% few-layer graphene and 2% cellulose acetate butyrate), probe ultrasonicate for 30 minutes (120W, 20kHz), stir at 500 rpm for 1 hour to form a graphene slurry with a slurry viscosity of 5-13 mPa·s (viscometer, shear rate 100 s-1).

[0092] Step 7. Select 80 mesh screen to process the antenna structure (such as Figure 3 As shown in the figure), the slurry was stirred at 1000rpm for 10 minutes before printing. The substrates included PET, paper, TPU, PI and other common packaging materials. Figure 3 After scraping twice in the direction shown, the printed antenna was dried at 125° C. for 15 minutes.

[0093] Figure 3 (a) in the figure is the structure diagram of the printed antenna. Figure 3 (b) is an electron scanning microscope image of the printed antenna surface, and the graphene sheet size is 0.5-1.5 microns.

[0094] Step 8. The antenna was rolled three times with metal rollers at 165°C and 6MPa to increase the contact area between graphene sheets. A dispensing machine (DELOMONOPOX AC268) was used to dispense glue, and a chip (NXPUCODE 8 chip, read sensitivity -23 dBm) was welded in the center of the antenna using a packaging machine. After hot pressing (140°C for 15s), an RFID tag was formed. Example 2

[0095] Comparative Example 1: Dihydro-levorotatory glucose ketone graphene printed antenna

[0096] This embodiment is the same as step S101 in embodiment 1. In step S102, the mixture of dihydro-levoglucose ketone and triacetin (molar ratio after fusion is 2:1) in a weight ratio of 3.4:1 is replaced with dihydro-levoglucose ketone solvent. Steps S103-S105 are repeated. Step S106 is replaced with:

[0097] The graphene powder was re-dissolved into the dihydro-L-glucose ketone solvent at 10 mg / ml, probe ultrasonic dispersion was performed for 5 minutes (120W, 20kHz), 1 mg / ml cellulose acetate butyrate was added, and vacuum oil bath rotary evaporation was concentrated (160°C, 300Pa) until the volume shrank to 1 / 8 of the original solution (the final weight was 90% dihydro-L-glucose ketone, 9% few-layer graphene, 1% cellulose acetate butyrate), and stirred at 500 rpm for 1 hour to form graphene slurry. If the weight of the few-layer graphene is concentrated to 13% (the same as in this example), the slurry will be too viscous and difficult to apply ink during screen printing. Example 3

[0098] Comparative Example 2: N-methylpyrrolidone (NMP) graphene printed antenna

[0099] This embodiment is the same as step S101 in embodiment 1. In step S102, the mixture of dihydro-levorotatory glucosone and triacetin (molar ratio after fusion is 2:1) in a weight ratio of 3.4:1 is replaced with N-methylpyrrolidone solvent. Steps S103-S105 are repeated. Step S106 is replaced with:

[0100] 0.04 parts by weight of dried graphene powder was added to 1 part by weight of a mixed solvent of N-methylpyrrolidone solvent and divalent acid resin in a ratio of 2:1, and stirred at 500 rpm. After stirring for 20 minutes, 0.04 parts by weight of graphene powder was added again. After stirring for 20 minutes, 0.04 parts by weight of graphene powder and 0.01 parts by weight of cellulose acetate butyrate (the final weight was 43% N-methylpyrrolidone, 43% divalent acid resin, 13% graphene powder and 1% cellulose acetate butyrate) were added. The mixture was ultrasonicated for 30 minutes (120 W, 20 kHz) and stirred at 500 rpm for 1 hour to form a graphene slurry.

[0101] Step S2 and step S3 in Embodiment 2 and Embodiment 3 are the same as those in Embodiment 1.

[0102] Comparison of the peeling efficiency between Example 1 (this example), Example 2 (Comparative Example 1), and Example 3 (Comparative Example 2):

[0103] The exfoliated graphene was dried in a vacuum oven and then weighed, and the weight was compared with that of the expandable graphite before exfoliation.

[0104] Table 1 Stripping efficiency comparison table

[0105]

[0106] Peeling quality comparison:

[0107] Atomic force microscope scans of exfoliated graphene (spin-coated onto a silicon substrate), and 50 graphene sheets are randomly selected for thickness analysis.

[0108] Table 2 Comparison of graphene exfoliation sheet thickness

[0109]

[0110] The above is only the best specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions within the technical scope disclosed in the present application shall be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A graphene printed radio frequency identification tag, characterized in that: include: Substrate, antenna frame, chip and paste; The antenna frame is an antenna structure processed by a silk screen, the antenna frame is placed on the substrate, the slurry is silk-screened on the surface of the antenna frame along a first direction to form a printed antenna, the printed antenna is rolled and then the chip is packaged in the center of the printed antenna to form the graphene printed RFID tag; The slurry is graphene slurry, and the components and their mass percentages of the graphene slurry are: 10~15wt% graphene; 1~3 wt% cellulose acetate butyrate; 15~25 wt% triacetin; 60~70 wt% dihydrolevorotatory glucosone.

2. The graphene printed RFID tag according to claim 1, characterized in that: The components of the graphene slurry and their mass percentages are: 13 wt% graphene; 2 wt% cellulose acetate butyrate; 20 wt% triacetin; 65 wt% dihydrolevorotatory glucosone.

3. The graphene printed RFID tag according to claim 1, characterized in that: The wire mesh is 80 mesh; The substrate includes at least one of PET, paper, TPU and PI.

4. The graphene printed RFID tag according to any one of claims 1 to 3, characterized in that: The viscosity of the graphene slurry is 5-13 mPa·s.

5. The graphene printed RFID tag according to claim 4, characterized in that: The chip is an NXP UCODE 8 chip, and the chip is welded to the center of the printed antenna by a packaging machine.

6. A method for preparing a graphene printed radio frequency identification tag, for preparing the graphene printed radio frequency identification tag according to any one of claims 1 to 5, characterized in that: The following steps are involved: Prepare a graphene slurry, wherein the components and their mass percentages in the prepared graphene slurry are: 13 wt% graphene, 2 wt% cellulose acetate butyrate, 20 wt% glyceryl triacetate, and 65 wt% dihydro-levorotatory glucosone, and the viscosity of the graphene slurry is 5-13 mPa·s; Selecting an antenna frame, preparing a substrate, placing the antenna frame on the substrate, scraping the graphene slurry on the antenna frame along a first direction, and drying to form a printed antenna; The printed antenna is rolled and then glued by a glue dispenser, a chip is welded at the center of the printed antenna after glue dispensing, and the graphene printed radio frequency identification tag is formed after heat pressing.

7. The method for preparing a graphene printed radio frequency identification tag according to claim 6, characterized in that: The preparation of graphene slurry comprises the following steps: Forming expanded graphite by intercalating expandable graphite flakes through microwave treatment; Dihydro-levorotatory glucosone and triacetin are mixed in a weight ratio of 3.4:1 to form a graphene exfoliation solvent; The expanded graphite is coarsely ground, and then the stripping solvent is added, and then ultrasonic stripping is performed to form a graphene dispersion; The graphene dispersion is subjected to low-speed centrifugation to remove unsuccessfully exfoliated graphite, and then subjected to high-speed centrifugation to obtain a graphene sediment; vacuum drying the graphene deposit to obtain graphene powder; 0.05 parts by weight of the graphene powder is added to 1 part by weight of the graphene exfoliation solvent, and the mixture is stirred. Then, 0.05 parts by weight of the graphene powder is added, and after continuous stirring, 0.04 parts by weight of the graphene powder and 0.02 parts by weight of cellulose acetate butyrate are added, and the graphene slurry is formed after ultrasonication and stirring.

8. The method for preparing a graphene printed radio frequency identification tag according to claim 7, characterized in that: The expanded graphite was coarsely ground using a grinder at a speed of 300 rpm for 1 hour; The expanded graphite is coarsely ground and then added with the stripping solvent at 10 mg / ml; The graphene dispersion is formed by ultrasonic exfoliation in a 180W 40kHz ultrasonic pool for 8 hours.

9. The method for preparing a graphene printed radio frequency identification tag according to claim 7 or 8, characterized in that: The graphene dispersion is subjected to low-speed centrifugation to remove unsuccessfully exfoliated graphite, and then subjected to high-speed centrifugation to obtain a graphene sediment, specifically: The graphene dispersion was subjected to two low-speed centrifugation treatments at 300 rpm for 10 minutes to obtain the supernatant, the dispersion after centrifugation was passed through a 300-mesh steel sieve to remove the unstripped graphite, and then subjected to high-speed centrifugation treatment at 1500 rpm for 10 minutes to obtain the sediment.

10. The method for preparing a graphene printed radio frequency identification tag according to claim 9, characterized in that: The antenna frame is made of 80 mesh screen; The graphene slurry was stirred at 1000 rpm for 10 minutes before printing; The conditions for drying to form the printed antenna are: drying at 125° C. for 15 minutes; The printing antenna is rolled by: rolling the printed antenna three times with a metal roller at 165° C. and 6 MPa; The hot pressing was performed under the conditions of 140° C. for 15 seconds.

Citation Information

Patent Citations

  • Graphene RFID tag and preparation method and application thereof

    CN114590801A

  • Graphene film for RFID antenna, graphene RFID antenna and preparation method and application thereof

    CN117613537A

  • Graphene RFID tag and preparation method and application thereof

    CN117735536A

  • Conductive ink, RFID antenna, electronic tag and preparation method

    CN110577771A

  • Graphene conductive paste, preparation method and RFID electronic tag

    CN112349448A