A N-type TBC double POLY battery and its preparation method
In the preparation of N-type TBC single crystal solar cells, phosphorus doping and boron diffusion are used to use the phosphorus slurry layer and mask layer, and combined with pickling and screen printing, the problems of laser groove and alkali etching are solved, realizing the Efficient N-zone preparation and battery conversion efficiency improvement.
Patent Information
- Application Number
- CN202410987743.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-23
AI Technical Summary
In the existing N-type TBC single crystal solar cell preparation process, the laser groove area is large, the BSG is dense, the alkali etching controllability is poor, and the N-zone etching depth is difficult to accurately control, resulting in low battery conversion efficiency and the failure to realize the back dual POLO structure. .
The preparation method of N-type TBC dual-zone POLY battery is adopted. The two-sided rough polishing of the N-type substrate is deposited and then the oxide layer and amorphous silicon layer are deposited. The phosphorus doping and boron diffusion are used to be used for phosphorus doping and boron diffusion. High temperature diffusion forms a polysilicon layer, combined with acid washing to remove the BSG layer and screen printing to form an interdigital emitter to avoid laser grooves and alkali etching.
The preparation of the back patterned N zone is realized, the POLY structure of N zone is retained, the battery conversion efficiency is improved, the process steps are simplified, the cost is reduced, the risk of leakage is avoided, and the current density is improved.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to an N-type TBC double POLY cell and a preparation method thereof. Background Art
[0002] At present, the conversion efficiency of N-type PERC monocrystalline solar cells has reached a bottleneck. TOPCON cells have a good passivation effect. The conversion efficiency of cells with this structure has been significantly improved. The current highest conversion efficiency has reached 26.5%. IBC monocrystalline solar cells can solve the problem of shading on the front grid line, and also have high cell conversion efficiency and potential. TBC products that superimpose the IBC structure and the TOPCON structure have been launched one after another. Compared with HJT cells, the theoretical limit efficiency of the single TOPCON structure on the back is still difficult to match. The current preparation method of BC cells mainly adopts the laser grooving + alkaline solution etching method.
[0003] Specifically, the current mainstream process path is: double-sided polishing - LPCVD deposition of tunneling layer and amorphous silicon layer - high temperature completion of boron expansion and crystallization - front etching + texturing - tube oxygen - laser grooving (opening the N area) - alkaline etching - double-sided deposition of aluminum oxide - double-sided deposition of silicon nitride - laser film opening - screen printing.
[0004] The existing process defects are as follows:
[0005] 1. The existing process route requires a large laser grooving area (opening the N region including the main gate), and the resulting BSG is relatively dense, which places high demands on the laser, reduces the laser life and increases the cost;
[0006] 2. Boron diffusion of amorphous silicon is difficult and the junction depth is often insufficient;
[0007] 3. The alkaline etching has poor controllability, and the etching depth of the N region cannot be accurately controlled, which easily leads to local leakage;
[0008] 4. After the N region is etched, the base region is thinned, which affects the final current density (the thinning of the silicon wafer will reduce the absorption ratio of photons in the matrix and reduce the current density of the battery);
[0009] 5. It is impossible to realize the double POLO structure on the back, which limits the conversion efficiency of the battery. Summary of the invention
[0010] The present invention provides a method for preparing an N-type TBC dual-zone POLY battery, comprising the following steps:
[0011] (1) N-type substrate double-sided rough polishing followed by polishing;
[0012] (2) Select one side as the back side and deposit a tunneling oxide layer and an amorphous silicon layer.
[0013] (3) Two layers of slurry are coated on the N-region patterned area on the back side of the substrate, and the operation is divided into two times. After each coating, the substrate is dried and annealed, so that the slurry first forms a phosphorus slurry layer on the back side of the silicon substrate, and then a mask layer is superimposed on the outside. The phosphorus slurry layer can dope phosphorus into the amorphous silicon in the coating area, and the outer mask layer can prevent boron from diffusing into the silicon substrate.
[0014] (4) Perform high-temperature diffusion on the back side, using boron trichloride or boron tribromide to achieve doping and crystallization of the amorphous silicon layer in the non-N-region patterned area, and convert the amorphous silicon layer in the non-N-region patterned area into a boron-doped polysilicon layer. At the same time, this high-temperature process pushes the phosphorus source in the N-region patterned area forward, converting the amorphous silicon layer in this area into a phosphorus-doped polysilicon layer.
[0015] (5) Etching and texturing the front side of the substrate. During texturing, pickling is performed to remove the BSG layer in the non-N graphic area on the back side, the residual phosphorus paste and mask layer in the N graphic area.
[0016] Specifically, the front side is first etched with a 70%-80% mass concentration HF solution to remove the front BSG, and then single-side texturing is performed. In the pickling section of the texturing process, a 70%-80% mass concentration HF solution is used to remove the BSG layer in the non-N-region patterned area on the back side and the phosphorus paste and mask layer in the N-region patterned area.
[0017] (6) Aluminum oxide film is deposited on both sides of the substrate.
[0018] (7) Silicon nitride film is deposited on both sides of the substrate.
[0019] (8) Using laser to perform patterning on the N region on the back side of the substrate to remove the aluminum oxide film and silicon nitride film of the N region.
[0020] (9) Screen printing is performed on the back side of the substrate to form an interdigitated emitter to produce an N-type TBC single crystal solar cell.
[0021] Preferably, the reflectivity of the polished substrate in step (1) is greater than 38%.
[0022] Preferably, after the base is polished in step (1), the size of the tower base is controlled to be 8-12 μm.
[0023] Preferably, the tunneling layer described in step (2) is 1-2 nm.
[0024] Preferably, the amorphous silicon layer in step (2) is 80-120 nm.
[0025] Preferably, the coating method in step (3) includes spraying, coating, printing, rolling and transfer.
[0026] Preferably, the phosphorus paste layer in step (3) is a phosphorus-doped silicon dioxide latex, and after drying and annealing, a phosphorus-doped silicon dioxide layer is formed.
[0027] Preferably, the slurry of the mask layer in step (3) may be a single-layer or multi-layer structure, and its components include one or more of silicon oxide, aluminum oxide, silicon nitride, and silicon oxynitride.
[0028] Preferably, the annealing temperature in step (3) is 550-800° C. and the time is 60-500 s.
[0029] Preferably, the drying temperature in step (3) is 80-200°C.
[0030] Preferably, the high temperature diffusion temperature in step (4) is 850-1050°C
[0031] Preferably, in step (4), the boron doping concentration of the polysilicon in the non-N region patterned area is 1E20-3E20 atoms / cm 3 The phosphorus doping concentration of polysilicon in the N-region patterned area is 2E20-4E20atoms / cm 3 .
[0032] Preferably, the suede reflectivity of the front side of the substrate in step (5) is 8%-11%.
[0033] Preferably, the thickness of the aluminum oxide in step (6) is 3-10 nm.
[0034] Preferably, the thickness of the silicon nitride in step (7) is 70-90 nm.
[0035] The advantages and benefits of the present invention are that it provides a method for preparing an N-type TBC dual POLY battery, which does not require laser grooving. The preparation of the patterned N region on the back of the battery can be achieved by washing away the phosphorus paste and the mask with high-concentration acid, while retaining the POLY structure of the N region. In addition, the superposition of the phosphorus paste and the modified mask can achieve different types of doping of the N region and non-N region POLY during the boron expansion process, that is, the preparation of the BC battery N region.
[0036] Compared with the existing technology, the present invention has the following advantages:
[0037] The existing process relies on laser to groove the BSG in the N region (including the main gate) and distinguish the P region and N region for alkali polishing. This method places high demands on the laser and limits the window for adjusting the boron diffusion process. This method also cannot retain the POLY layer in the N region. In addition, the alkali polishing process has poor controllability and is prone to local leakage.
[0038] The present invention adopts spraying, coating, printing or transfer to realize phosphorus paste deposition on the patterned N area on the back of the BC battery (after drying and annealing, a silicon dioxide layer doped with phosphorus is formed, which can diffuse the POLY phosphorus underneath under the condition of high-temperature boron diffusion) and mask deposition (the mask can prevent boron from diffusing into the phosphorus paste layer underneath during high-temperature diffusion).
[0039] This method does not require laser grooving, the alkaline etching process is simple and there is no risk of leakage, and the thickness of the N-region silicon wafer will not be reduced, which will not affect the current density of the battery (thinning the silicon wafer will lead to a decrease in the absorption ratio of photons in the matrix, reducing the current density of the battery).
[0040] The battery prepared by the present invention has higher conversion efficiency, fewer process steps, simple operation, and is conducive to large-scale production of batteries. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the embodiments.
[0042] Embodiment 1, a method for preparing an N-type TBC battery, comprising the following steps:
[0043] (1) N-type single crystal substrate double-sided rough polishing and then polishing
[0044] In this embodiment, the damaged layer on the surface of the silicon wafer is first removed in a mixed solution of NaOH / KOH and H2O2, and then double-sided polishing is performed in a sodium hydroxide solution or a potassium hydroxide solution with a mass concentration of 3% and a temperature of 65°C. The surface of the silicon wafer forms a flat surface, the tower base is 8μm, and the reflectivity is controlled to be 42%.
[0045] (2) The tunneling layer (1.5 nm) and the intrinsic amorphous silicon layer (90 nm) are prepared on the back side of the silicon wafer using the LPCVD process.
[0046] (3) A phosphorus paste layer is first coated on the N-region patterned area on the back of the BC battery, and then a mask layer is coated. After each coating, the substrate is dried (temperature: 120°C) and chain annealed (annealing temperature: 650°C, time: 120s).
[0047] In some embodiments, the phosphorus paste and the mask layer can be covered by spraying, coating, printing, rolling, and transfer, etc. This embodiment adopts the rolling coating method.
[0048] In some embodiments, the phosphorus slurry is a silicon dioxide latex doped with phosphorus. A layer of phosphorus slurry is covered on the N-region patterned area on the back of the silicon wafer, and after drying and annealing, a silicon dioxide layer doped with phosphorus is formed. The high temperature during the high-temperature diffusion process can cause the phosphorus therein to diffuse into the POLY layer below, thereby achieving phosphorus doping of the N-region POLY layer. The phosphorus slurry coverage thickness of this embodiment is 5nm.
[0049] In some embodiments, the mask layer may be a single layer or a multilayer structure, and its components include one or more of silicon oxide, aluminum oxide, silicon nitride, and silicon oxynitride. In this embodiment, the mask layer is a single layer structure, and its components include a mixture of silicon oxide and silicon nitride, and the thickness of the mask layer is 30nm.
[0050] On the basis of the original phosphorus paste N-zone patterned area on the back of the silicon wafer, a mask layer is covered again. After the covering is completed, it is dried and annealed to form a stable mask layer on the surface. The mask layer can block boron from diffusing into the underlying phosphorus paste layer and avoid affecting the phosphorus diffusion of the N-zone POLY layer.
[0051] (4) Using tubular diffusion equipment to perform high-temperature diffusion on the back side of the silicon wafer, using boron trichloride or boron tribromide to achieve doping and crystallization of the amorphous silicon layer in the non-N-region patterned area, converting the amorphous silicon layer in the non-N-region patterned area into a boron-doped polycrystalline silicon layer, and at the same time converting the amorphous silicon layer in the N-region patterned area into a phosphorus-doped polycrystalline silicon layer.
[0052] In this embodiment, the high temperature diffusion temperature is 950°C, and the boron doping concentration of the polysilicon in the non-N region patterned area after diffusion is 1.5E20atoms / cm 3 The phosphorus doping concentration of polysilicon in the N-region patterned area is 2E20atoms / cm 3 The junction depth is affected by the POLY layer below and is 90nm.
[0053] (5) With the front side facing down, use a chain device to etch the front side of the substrate with HF at a mass concentration of 80%, and then enter the texturing tank machine. First, remove the organic contamination on the surface of the silicon wafer in a mixed solution of KOH / NaOH and H2O2, and then texturing in a sodium hydroxide solution or a potassium hydroxide solution. A pyramid velvet surface is formed on the surface of the silicon wafer. The size of the pyramid velvet surface is 1.2μm, and the reflectivity is 10.8%. Finally, before exiting the tank for drying, soak in HF at a mass concentration of 70% to remove the BSG layer in the non-N graphic area on the back, the phosphorus paste and mask layer in the N graphic area.
[0054] (6) Double-sided deposition of aluminum oxide film.
[0055] In this embodiment, an aluminum oxide film with a thickness of 10 nm is deposited on the front and back sides of an N-type single crystal silicon wafer using an ALD device.
[0056] (7) Silicon nitride film is deposited on both sides.
[0057] In this embodiment, a PECVD device is used to deposit a silicon nitride film with a thickness of 85 nm on the front and back sides of an N-type single crystal silicon wafer.
[0058] (8) Using laser to pattern the N region on the back of the silicon substrate to remove the aluminum oxide film and silicon nitride film in the N region.
[0059] (9) Screen printing is performed on the back side of the substrate to form an interdigitated emitter to produce an N-type TBC double POLY single crystal solar cell.
[0060] Comparative Example 1, (1) N-type single crystal substrate double-sided rough polishing and then polishing
[0061] In this comparative example, the loss layer on the surface of the silicon wafer is also removed in a mixed solution of NaOH / KOH and H2O2, and then double-sided polishing is performed in a sodium hydroxide solution or a potassium hydroxide solution with a mass concentration of 3% and a temperature of 65°C. A flat surface is formed on the surface of the silicon wafer, the tower base is 8μm, and the reflectivity is controlled to be 42%.
[0062] (2) The tunneling layer (1.5 nm) and the intrinsic amorphous silicon layer (90 nm) are prepared on the back side of the silicon wafer using the LPCVD process.
[0063] (3) Using tubular diffusion equipment to perform high-temperature boron diffusion and crystallization on the back of the silicon wafer, using boron trichloride or boron tribromide to achieve doping and crystallization of the amorphous silicon layer, and converting the amorphous silicon layer into a boron-doped polycrystalline silicon layer.
[0064] In this embodiment, the high-temperature boron diffusion temperature is 950°C, and the boron doping concentration of the back polysilicon after diffusion is 1.5E20atoms / cm 3 The boron doping concentration of the polysilicon in the N-region patterned area is 1.5E20atoms / cm 3 , junction depth 90nm.
[0065] (4) Front etching and texturing
[0066] The front side is facing down and etched with HF at a mass concentration of 80% using a chain device. The silicon wafer then enters a texturing tank machine to remove organic contamination on the surface of the silicon wafer in a mixed solution of KOH / NaOH and H2O2. Then, the silicon wafer is texturized in a sodium hydroxide solution or a potassium hydroxide solution. A pyramid velvet surface is formed on the surface of the silicon wafer. The size of the pyramid velvet surface is 1.2μm, and the reflectivity is 10.8%.
[0067] (5) Using tubular high-temperature equipment, the back of the silicon wafer is oxidized at a process temperature of 700°C in an oxygen-filled atmosphere.
[0068] (6) Use laser to perform patterned grooving of the N region on the back side of the base.
[0069] (7) Alkali etching
[0070] A mixed solution of NaOH / KOH and H2O2 was used to remove the damaged layer of the patterned N region on the back of the substrate caused by laser grooving. Then, the patterned N region was polished in a sodium hydroxide solution or potassium hydroxide solution with a concentration of 3% and a temperature of 65°C to form a flat surface structure at the N region position, with a tower base of 12μm.
[0071] (8) Double-sided deposition of aluminum oxide film.
[0072] In this comparative example, an aluminum oxide film with a thickness of 10 nm is deposited on the front and back sides of an N-type single crystal silicon wafer using an ALD device.
[0073] (9) Silicon nitride film is deposited on both sides.
[0074] In this comparative example, a PECVD device is used to deposit a silicon nitride film with a thickness of 85 nm on the front and back sides of an N-type single crystal silicon wafer.
[0075] (10) In the N region on the back side of the silicon substrate, a laser is used to perform patterning and mold opening to remove the aluminum oxide film and silicon nitride film in the N region.
[0076] (11) Screen printing is performed on the back side of the substrate to form an interdigitated emitter to produce an N-type TBC single crystal solar cell.
[0077] The photovoltaic cells of the above embodiment 1 and comparative example 1 were subjected to electrical performance tests to obtain parameters such as the open circuit voltage (Voc), short circuit cell (Isc), fill factor (FF), energy conversion efficiency (Eta) of the cells, as shown in Table 1 below:
[0078] Table 1
[0079] Voc (mV) Isc(A) Rs (Ω) FF(%) Eta(%) Example 1 738.4 13.753 1.21 85.87 26.41 Comparative Example 1 693.1 13.593 1.22 83.47 23.82
[0080] Compared with comparative example 1, embodiment 1 forms a double POLY area on the back of the silicon wafer, which has a better passivation effect, resulting in a 2.4% increase in Voc 45mV and FF. In addition, since laser BSG grooving is not used, leakage and parasitic current can be reduced, and there is no loss of silicon wafer thickness in the laser grooving area, so Isc can also be increased by 0.16A. The comprehensive optimization can make the Eta of embodiment 1 increase by 2.59%.
[0081] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing an N-type TBC double POLY battery, It is characterized in that The steps include: (1) N-type substrate double-sided rough polishing followed by polishing; (2) selecting one side as the back side, and depositing a tunneling oxide layer and an amorphous silicon layer; the amorphous silicon layer has a thickness of 80-120 nm; (3) coating a phosphorus paste layer and a mask layer in sequence on the N-region patterned area on the back side of the substrate, and drying and annealing the substrate after each coating; the annealing temperature is 550-800° C.; (4) High-temperature diffusion is performed on the back side of the substrate to convert the amorphous silicon layer in the non-N-region patterned area into a boron-doped polysilicon layer, and the amorphous silicon layer in the N-region patterned area into a phosphorus-doped polysilicon layer; (5) Etching and texturing of the front side of the substrate. During texturing, pickling is performed to remove the BSG layer in the non-N graphic area on the back side, the residual phosphorus slurry and mask layer in the N graphic area; (6) Aluminum oxide film is deposited on both sides of the substrate; (7) Deposition of silicon nitride film on both sides of the substrate; (8) Using a laser to perform patterning on the N region on the back side of the substrate to remove the aluminum oxide film and the silicon nitride film of the N region; (9) Screen printing is performed on the back side of the substrate to form an interdigitated emitter to produce an N-type TBC single crystal solar cell.
2. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The reflectivity of the polished substrate in step (1) is greater than 38%, and the size of the tower base is controlled at 8-12 μm.
3. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The phosphorus paste layer in step (3) is a silicon dioxide latex doped with phosphorus.
4. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The coating method in step (3) includes spraying, coating, printing, rolling and transfer.
5. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The annealing time in step (3) is 60-500s.
6. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The drying temperature in step (3) is 80-200°C.
7. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The high temperature diffusion temperature in step (4) is 850-1050°C.
8. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The front etching and pickling in step (5) adopts HF solution with a mass concentration of 70%-80%.
9. The method for preparing the N-type TBC double POLY battery according to claim 1, It is characterized in that The suede reflectivity of the front side of the substrate in step (5) is 8%-11%.
10. An N-type TBC double POLY battery prepared according to the method according to any one of claims 1 to 9.