A positive electrode material and preparation method thereof, secondary battery and electrical equipment

By optimizing the particle size, morphological distribution and carbon cladding of lithium iron phosphate, the poor battery performance problem caused by the large number of pores between the positive electrode particles of lithium iron phosphate is solved, and the energy density and rate performance of the battery are significantly improved.

CN118538912BActive Publication Date: 2024-11-19SHENZHEN BYD LITHIUM BATTERY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411003026.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-19
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing lithium iron phosphate positive electrode material has more pores between particles, resulting in a smaller compaction density of the electrode sheet and poor battery energy density and rate performance.

Method used

By optimizing the particle size and morphological distribution of lithium iron phosphate, the particle size distribution of the definite positive electrode material meets a specific formula: z=2.35+0.258*D150-0.121*D250-0.639*D3mo+0.3125*S+0.0142*n, 2.3≤ z≤2.79, combined with the use of carbon cladding, improve pore filling between particles and the density of conductive networks.

Benefits of technology

It significantly improves the compaction density of the electrode sheet, the energy density and rate performance of the battery, and solves the problem of poor battery performance caused by the large number of pores between the lithium iron phosphate positive electrode material particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118538912B_ABST
    Figure CN118538912B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides a positive electrode material and a preparation method thereof, a secondary battery and an electric device, wherein the positive electrode material provided by the embodiment of the present invention optimizes the particle size so that the particle size and morphology distribution satisfy: z=2.35+0.258*D 1 50‑0.121*D 2 50‑0.639*D 3 mo+0.3125*S+0.0142*n, 2.6≤z≤2.78, is beneficial to the grading of large and small particles and filling the pores between the particles, which can significantly improve the compaction density, thereby solving the problem that there are many pores between the particles of the existing lithium iron phosphate positive electrode material, which makes the compaction density of the electrode sheet small, resulting in low battery energy density and poor rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery manufacturing, and in particular to a positive electrode material and a preparation method thereof, a secondary battery and an electrical device. Background Art

[0002] Currently, lithium iron phosphate has been widely used in the fields of power batteries and energy storage because of its advantages as a positive electrode material for lithium-ion batteries, such as high cycle stability, good safety performance, and high charge and discharge efficiency.

[0003] However, when the existing lithium iron phosphate is used as the positive electrode material of lithium-ion batteries, the compaction density of the electrode is relatively small, which not only requires more electrolyte to fill the pores, resulting in reduced energy density, but also the conductive network of the electrode is not tightly constructed and the electrode membrane resistance is high, resulting in poor battery rate performance. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a positive electrode material, a secondary battery and an electrical device to improve the problem that there are many pores between the particles of the existing lithium iron phosphate positive electrode material, so that the compaction density of the electrode sheet is small, resulting in a small battery energy density and poor rate performance.

[0005] In order to solve the above problems, the present invention is achieved through the following technical solutions:

[0006] The present invention provides a positive electrode material, wherein:

[0007] The positive electrode material includes a first lithium iron phosphate, a second lithium iron phosphate, and a third lithium iron phosphate.

[0008] The particle size and morphology distribution of the positive electrode material meet the following requirements:

[0009] z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79;

[0010] Among them, D 1 50 refers to the D50 of the first lithium iron phosphate, D 2 50 refers to the D50 of the second lithium iron phosphate, D 3 mo refers to the particle size corresponding to the maximum volume fraction of the third lithium iron phosphate, S refers to the sphericity of the positive electrode material, and n refers to the mass ratio of the second lithium iron phosphate to the third lithium iron phosphate; 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3mo≤0.6μm, 0.6≤S≤1.0, 1≤n≤4.

[0011] Furthermore, in the positive electrode material, 2.6≤z≤2.79.

[0012] Furthermore, in the positive electrode material, the sphericity of the first lithium iron phosphate is S1, the sphericity of the second lithium iron phosphate is S2, and the sphericity of the third lithium iron phosphate is S3, and S1, S2, and S3 satisfy: 0.6≤S1≤1.0, and / or, 0.6≤S2≤1.0, and / or, 0.6≤S3≤1.0.

[0013] Furthermore, in the positive electrode material, the mass ratio of the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate is (4-5):4:(1-2).

[0014] Furthermore, in the positive electrode material, at least one of the first lithium iron phosphate, the second lithium iron phosphate and the third lithium iron phosphate has a carbon coating layer.

[0015] Furthermore, in the positive electrode material, the thickness of the carbon coating layer is 2nm~5nm.

[0016] The present invention also provides a method for preparing the above-mentioned positive electrode material, comprising:

[0017] Obtaining lithium iron phosphate, wherein the lithium iron phosphate has a sphericity of 0.6 to 1.0;

[0018] The lithium iron phosphate is graded to obtain a first lithium iron phosphate, a second lithium iron phosphate, and a third lithium iron phosphate, wherein the D 1 50. D 2 50. D 3 Mo meets: 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3 mo≤0.6μm;

[0019] The first lithium iron phosphate, the second lithium iron phosphate and the third lithium iron phosphate are mixed to obtain the positive electrode material, wherein the mass ratio n of the second lithium iron phosphate to the third lithium iron phosphate satisfies: 1≤n≤4, and the sphericity S of the positive electrode material satisfies: 0.6≤S≤1.0; the positive electrode material satisfies:

[0020] z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79.

[0021] Optionally, in the preparation method, obtaining lithium iron phosphate includes:

[0022] Mixing iron phosphate and a lithium source to obtain a lithium iron phosphate precursor, grinding the lithium iron phosphate precursor, wherein the particle size D50 of the ground lithium iron phosphate precursor satisfies: 400nm≤D50≤800nm;

[0023] The ground lithium iron phosphate precursor is dried, sintered and crushed to obtain the lithium iron phosphate, and the sphericity of the lithium iron phosphate is 0.6-1.0.

[0024] Optionally, in the preparation method, the lithium source includes one or more of Li2CO3 and LiOH.

[0025] Optionally, in the preparation method, mixing iron phosphate and a lithium source to obtain a lithium iron phosphate precursor further comprises: adding a carbon source to the mixture, wherein the carbon source comprises one or more of glucose, starch, and phenolic resin.

[0026] Optionally, in the preparation method, the molar ratio of the iron phosphate, the carbon source, and the lithium source is 1:(0.15~0.2):(1~1.04).

[0027] The present invention also proposes a secondary battery, comprising a positive electrode plate, wherein the positive electrode plate comprises a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, and the positive electrode active material layer comprises the positive electrode material as described above or the positive electrode material prepared by the method for preparing the positive electrode material as described above.

[0028] The present invention further provides an electric device, which includes the above-mentioned secondary battery, and the secondary battery serves as a power supply for the electric device.

[0029] Compared with the prior art, the embodiments of the present invention have the following advantages:

[0030] In the embodiment of the present invention, the positive electrode material provided includes a first lithium iron phosphate, a second lithium iron phosphate, and a third lithium iron phosphate, and satisfies: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79; among them, D 1 50 refers to the D50 of the first lithium iron phosphate, D 2 50 refers to the D50 of the second lithium iron phosphate, D 3mo refers to the particle size corresponding to the maximum volume fraction of the third lithium iron phosphate, S refers to the sphericity of the positive electrode material, and n refers to the mass ratio of the second lithium iron phosphate to the third lithium iron phosphate; 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3 mo≤0.6μm, 0.6≤S≤1.0, 1≤n≤4. Among them, by optimizing the particle size, the particle size distribution of the positive electrode material is limited to meet: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79, is beneficial to the grading of large and small particles and filling the pores between the particles, which can significantly improve the compaction density, thereby solving the problem that there are many pores between the particles of the existing lithium iron phosphate positive electrode material, which makes the compaction density of the electrode sheet small, resulting in low battery energy density and poor rate performance.

[0031] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a schematic diagram of the structure of the positive electrode material provided by an embodiment of the present invention;

[0033] Figure 2 It is a schematic diagram of the structure of a two-stage series-connected turbine classifier provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] The applicant of the present invention has found that when the existing lithium iron phosphate is used as the positive electrode material of the lithium-ion battery, the compaction density of the electrode is relatively small, which not only requires more electrolyte to fill the pores, resulting in reduced energy density, but also the conductive network of the electrode is not tightly constructed, and the electrode membrane resistance is relatively high, resulting in poor rate performance of the battery.

[0036] In order to solve the above problems, the embodiment of the present invention provides a positive electrode material, wherein Figure 1 As shown, the positive electrode material includes a first lithium iron phosphate 11, a second lithium iron phosphate 12, and a third lithium iron phosphate 13. The particle size and morphology distribution of the positive electrode material satisfy: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D3 mo+0.3125*S+0.0142*n, and 2.3≤z≤2.79;

[0037] Among them, D 1 50 refers to D50 of the first lithium iron phosphate. 2 50 refers to the D50 of the second lithium iron phosphate, D 3 mo refers to the particle size corresponding to the maximum volume fraction of the third lithium iron phosphate, S refers to the sphericity of the positive electrode material, and n refers to the mass ratio of the second lithium iron phosphate to the third lithium iron phosphate; 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3 mo≤0.6μm, 0.6≤S≤1.0, 1≤n≤4.

[0038] Among them, D50 is the particle size corresponding to when the cumulative volume percentage of the lithium iron phosphate material in the Malvern particle size tester reaches 50%; Dmo is the particle size corresponding to when the volume fraction of the lithium iron phosphate material in the Malvern particle size tester is the largest.

[0039] In the embodiment of the present invention, by optimizing the particle size and morphology, the particle size distribution of lithium iron phosphate in the positive electrode material is limited to satisfy: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79, is beneficial to the grading of large and small particles and filling the pores between the particles, which can significantly improve the compaction density and make the conductive network of the electrode sheet tightly constructed, which can effectively improve the energy density and rate performance of the battery, thereby solving the problem that there are many pores between the particles of the existing lithium iron phosphate positive electrode material, which makes the compaction density of the electrode sheet small, resulting in small battery energy density and poor rate performance.

[0040] Optionally, in some embodiments, 2.6≤z≤2.79 is satisfied, which can make the particle size distribution of lithium iron phosphate in the positive electrode material more reasonable, can tightly fill the pores between the particles, can further improve the compaction density, and can also make the electrode conductive network construction more compact, thereby more effectively improving the energy density and rate performance of the battery.

[0041] Optionally, in one embodiment, the lithium iron phosphate of the above-mentioned particle sizes are all spherical in shape, which can not only effectively ensure the grading of large and small particles, but also make the positive electrode material have a more stable result and a more suitable specific surface area, further improving the electrochemical performance of the battery.

[0042] Optionally, in a specific embodiment, the sphericity of the first lithium iron phosphate is S1, the sphericity of the second lithium iron phosphate is S2, and the sphericity of the third lithium iron phosphate is S3, and S1, S2, and S3 satisfy: 0.6≤S1≤1.0, 0.6≤S2≤1.0, and 0.6≤S3≤1.0; the sphericity S1, S2, and S3 of each lithium iron phosphate satisfy 0.6≤S1≤1.0, and / or, 0.6≤S2≤1.0, and / or, 0.6≤S3≤1.0, for example, a range value of one or any two of 0.6, 0.7, 0.8, 0.9, and 1.0. The sphericity of lithium iron phosphate is within this range, which can better meet the stacking of the positive electrode material after mixing, and can further improve the structural stability of the positive electrode material.

[0043] Optionally, in one embodiment, in the above-mentioned positive electrode material, the mass ratio of the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate is 4~5:4:1~2, which can be but is not limited to 4:4:1, 4:4:2, 4.5:4:1, 4.5:4:1.5, 4.5:4:2, 5:4:1, 5:4:2, which can effectively take into account the capacity density and structural stability of the material.

[0044] In the above-mentioned positive electrode materials, at least one of the first lithium iron phosphate, the second lithium iron phosphate and the third lithium iron phosphate has a carbon coating layer, and the carbon coating on the surface of the lithium iron phosphate can promote the transmission of charges on the surface of the particles, improve the conductivity, and can also act as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , ensuring the purity of the finished material.

[0045] Optionally, in a specific embodiment, the thickness of the carbon coating is 2nm~5nm, for example, it can be a range of one or any two of 2nm, 3nm, 4nm, 5nm. The thickness is moderate and can effectively take into account the electrical conductivity and energy density of the material.

[0046] The embodiment of the present invention further provides a method for preparing the above-mentioned positive electrode material, comprising steps 201 to 203:

[0047] Step 201: Obtain lithium iron phosphate, wherein the sphericity of the lithium iron phosphate is 0.6-1.0.

[0048] In one embodiment of the present invention, the iron phosphate and the lithium source may be mixed, ground, granulated, sintered, and air flow crushed to obtain lithium iron phosphate with an overall sphericity S satisfying 0.6≤S≤1.0. Lithium iron phosphate materials with sphericity satisfying the conditions may also be prepared by other conventional methods for obtaining lithium iron phosphate.

[0049] Step 202: Classify the lithium iron phosphate to obtain a first lithium iron phosphate, a second lithium iron phosphate, and a third lithium iron phosphate, wherein the D1 50. D 2 50. D 3 Mo meets: 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3 mo≤0.6μm.

[0050] In this step, the rotation speed of the classifying cage of the turbine airflow classifier is adjusted to obtain D 1 50The first lithium iron phosphate, D 2 50 The second lithium iron phosphate, D 3 The third lithium iron phosphate with mo in the range of 0.35μm~0.6μm.

[0051] In practical applications, two-stage series turbine classifiers are used for classification to obtain the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate. The two-stage series classifiers can be used to obtain lithium iron phosphate samples with different particle size distributions, and the distribution width is narrow.

[0052] Among them, the structure of the two-stage series turbine classifier is as follows: Figure 2 As shown, it includes a first turbine classifier 21 and a second turbine classifier 22 connected in series in sequence, collecting the first coarse powder after classification by the first turbine classifier as the first lithium iron phosphate, collecting the second fine powder after classification by the second turbine classifier as the second lithium iron phosphate, and the fine powder in the bag collector at the end of the second turbine classifier as the third lithium iron phosphate.

[0053] Step 203: Mix the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate to obtain the positive electrode material, wherein the mass ratio n of the second lithium iron phosphate to the third lithium iron phosphate satisfies: 1≤n≤4, and the sphericity S of the positive electrode material satisfies: 0.6≤S≤1.0; and the positive electrode material satisfies: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79.

[0054] In step 203, the obtained first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate are loaded into a mixing tank, and the mass ratio between the second lithium iron phosphate and the third lithium iron phosphate is controlled to be 1:1-4:1, and the sphericity of the positive electrode material is controlled to be 0.6-1.0, and the materials are mixed evenly using a drum mill, etc., so that the particle size and morphology of the product meet: z=2.35+0.258*D 150-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, and 2.3≤z≤2.79, to obtain the above-mentioned positive electrode material.

[0055] In the embodiment of the present invention, samples with large and small particles can be obtained by grading the finished lithium iron phosphate, and the lithium iron phosphate samples with different particle sizes can be matched according to the above formula z to obtain higher electrode compaction.

[0056] Optionally, in one implementation, the above step 201 includes steps 211 to 212:

[0057] Step 211 , mixing iron phosphate and a lithium source to obtain a lithium iron phosphate precursor, grinding the lithium iron phosphate precursor, and the particle size D50 of the lithium iron phosphate precursor after grinding satisfies: 400nm≤D50≤800nm.

[0058] Optionally, in a specific embodiment, mixing iron phosphate and a lithium source to obtain a lithium iron phosphate precursor further comprises: adding a carbon source to the mixture, wherein the carbon source comprises one or more of glucose, starch, and phenolic resin.

[0059] In this specific embodiment, the carbon source can coat the lithium iron phosphate sample with carbon during the high temperature synthesis process, promote the transfer of charge on the particle surface, improve the conductivity, and hinder the further growth of lithium iron phosphate grains to synthesize lithium iron phosphate crystals with a moderate particle size. At the same time, carbon can also act as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , to ensure the purity of the finished material; the carbon source can be glucose, starch, phenolic resin, etc., and the lithium source can be Li2CO3, LiOH, etc. Among them, the carbon source can form a 2-5nm thick carbon coating layer on the surface of lithium iron phosphate.

[0060] In this specific embodiment, the iron phosphate, the carbon source, and the lithium source are mixed and ground using a sand mill or the like, so that a lithium iron phosphate precursor with a particle size D50 of 400 nm to 800 nm can be obtained.

[0061] Among them, mixing iron phosphate, carbon source and lithium source in a mass ratio of 1:0.15~0.2:1~1.04 can not only ensure sufficient reaction but also avoid lithium waste. The carbon can form a 2~5nm thick coating layer on the surface of lithium iron phosphate. The thickness is moderate and can effectively take into account the electrical conductivity and energy density of the material.

[0062] Optionally, the grinding may be performed using a sand mill at a rotation speed of 470 r / min to 490 r / min, so that the particle size D50 after sand grinding is 400 nm to 800 nm.

[0063] Step 212: Dry, sinter and crush the ground lithium iron phosphate precursor to obtain the lithium iron phosphate, wherein the sphericity of the lithium iron phosphate is 0.6-1.0.

[0064] In the above step 212, the lithium iron phosphate precursor is dried and sintered to combine ferrous phosphate with lithium to form lithium iron phosphate, and then pulverized by air flow to obtain lithium iron phosphate with an overall sphericity S satisfying 0.6≤S≤1.0.

[0065] Optionally, the drying process can specifically adopt spray drying granulation, controlling the spray moisture to be less than or equal to 2%, the spray air inlet temperature to be 230°C~250°C, and the spray air outlet temperature to be 85°C~95°C, which can make particles of different particle sizes evenly distributed, facilitate subsequent sintering reaction, and improve the comprehensive performance of the material.

[0066] Optionally, the dry powder obtained by spraying is placed in a sintering furnace with a protective gas atmosphere such as nitrogen for sintering, the sintering temperature is controlled at 765°C~775°C, and the oxygen content in the sintering furnace is less than or equal to 10ppm, that is, the iron phosphate can react with the lithium source to generate lithium iron phosphate.

[0067] Optionally, the sintered block material is crushed by air flow, and the crushing air flow pressure is 0.15MPa~0.25MPa, so that lithium iron phosphate with a sphericity of 0.6~1.0 can be obtained.

[0068] In the embodiment of the present invention, the particle size distribution of the lithium iron phosphate positive electrode material is limited to satisfy z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, and 2.3≤z≤2.79, the grading of large and small particles is achieved, the pores between the particles are filled, and the compaction density of the material is improved, so that the lithium iron phosphate positive electrode material can give full play to the characteristics of high cycle stability, good safety performance and high charge and discharge efficiency.

[0069] In the actual preparation process, the particle size distribution of the positive electrode material can be adjusted to satisfy the above relationship by changing the ball milling parameters. Specifically, the particle size of the positive electrode material can be affected by adjusting the ball milling time and the rotation speed, thereby affecting the z value.

[0070] An embodiment of the present invention further provides a secondary battery, comprising a positive electrode plate, wherein the positive electrode plate comprises a positive electrode collector and a positive electrode active material layer disposed on the positive electrode collector, and the positive electrode active material layer comprises the positive electrode material as described above.

[0071] In some embodiments, the surface density of the positive electrode sheet is 360 mg / cm 2 ~440mg / cm 2 The surface density of the positive electrode sheet is within the above range, which can effectively take into account the battery's rate performance and energy density and slow down polarization.

[0072] Optionally, in one embodiment, the positive electrode plate further includes an adhesive and a conductive agent, and the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylic resin.

[0073] Optionally, in one embodiment, the conductive agent may be acetylene black, carbon fiber, carbon nanotube, Ketjen black, artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, etc.

[0074] Optionally, in one embodiment, during the homogenization of the positive electrode material, the positive electrode material accounts for 95wt% to 98wt%, the binder accounts for 0.5wt% to 3wt%, and the conductive agent accounts for 0.5wt% to 3wt%. The distribution ratio of each component is within the above range, which can effectively take into account the rate performance and energy density of the battery. For example, the positive electrode material accounts for 96.8wt%, the binder accounts for 2.42wt%, and the conductive agent accounts for 0.78wt%.

[0075] In some embodiments, the positive electrode sheet is prepared as follows: the components for preparing the positive electrode sheet, such as the positive electrode active material including the positive electrode material, the binder and any other components are dispersed in a solvent such as N-methylpyrrolidone to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector; after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0076] The positive electrode sheet provided in the embodiment of the present invention has a compaction density of 2.3 g / cm under a pressure of 40 tons. 3 ~2.79g / cm 3 It not only takes into account the rate performance and energy density, but also significantly reduces the belt breakage.

[0077] The secondary battery provided by the embodiment of the present invention further includes a negative electrode plate, a separator and an electrolyte.

[0078] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer may include at least one of artificial graphite, natural graphite, hard carbon, soft carbon, and carbon black.

[0079] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode, and the electrolyte can be liquid, gel or all-solid. In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent, and the electrolyte salt is a lithium salt.

[0080] An embodiment of the present invention further provides an electric device, which includes the above-mentioned secondary battery, and the secondary battery serves as a power supply for the electric device.

[0081] For the above-mentioned secondary battery embodiments and electrical equipment embodiments, their positive electrode plates include a positive electrode active material layer, and the above-mentioned positive electrode active material layer includes the above-mentioned positive electrode material, and can achieve the same technical effects. In order to avoid repetition, they will not be described here. For relevant matters, please refer to the partial description of the positive electrode material embodiment.

[0082] In order to make the invention purpose, technical scheme and beneficial effect of the present invention clearer, the present invention is further described below in conjunction with embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0083] The present invention is described in detail below by way of examples.

[0084] Performance Testing Methods

[0085] (1) Sphericity test:

[0086] The LFP pole piece after rolling was cut into 20*20μm samples, and the cutting was photographed at intervals of 50nm. The grayscale value was automatically identified using the large law method, and the minimum particle size was set to 50nm to establish a 3D model for statistical sphericity.

[0087] Carbon coating thickness test: Use a transmission electron microscope to detect the thickness of the carbon coating of lithium iron phosphate. (3) Compacted density test:

[0088] The pole piece after rolling is punched into a disc with a radius of 20 mm, and the thickness of the disc is tested with a micrometer to calculate the compaction of the pole piece.

[0089] (4) FIB-SEM test:

[0090] The LFP pole piece after rolling was cut into 20*20μm samples, and the cutting was photographed at intervals of 50nm. The grayscale value was automatically identified using the large law method, and the minimum particle size was set to 50nm.

[0091] (5) First charge capacity test:

[0092] The rolled pole pieces were punched into small discs and assembled into button cells in a glove box. The glove box environment was: 25°C, water <0.1ppm, oxygen <1ppm;

[0093] Discharge the assembled button battery at 0.1C to 5mV, let it stand for 5 minutes, discharge it at 0.05mA to 5mV, let it stand for 5 minutes, discharge it at 0.01mA to 5mV, let it stand for 5 minutes, charge it at 0.1C to 3.8V, measure the battery capacity, and calculate the battery gram capacity.

[0094] (6) Energy density test:

[0095] At room temperature 25℃, charge and discharge at a constant current of 1 / 3C to 2.0V-3.8V, record the discharge capacity as C, the average discharge voltage as V, the battery mass as M, and calculate the energy density as C*V / M.

[0096] (7) Rate performance test:

[0097] At room temperature of 25℃, use a battery test cabinet to conduct discharge tests at voltages of 2.5V-3.8V at rates of 1 / 3C, 0.5C, 1C, and 2C, and calculate the discharge capacity retention rate as the rate performance indicator.

[0098] Example 1

[0099] (1) Preparation of positive electrode materials:

[0100] a. Mixing iron phosphate, a carbon source and a lithium source in a mass ratio of 1: 0.2: 1.04, and grinding the mixture with a sand mill at a speed of 480 r / min to obtain a particle size D50 of 680 nm after sand milling; wherein the carbon source is phenolic resin and the lithium source is LiOH;

[0101] b. Use spray drying to granulate the sand-milled material, control the spray moisture content to be less than or equal to 2%, the spray inlet temperature to be 240°C, and the spray outlet temperature to be 90°C;

[0102] c. Place the dry powder obtained by spraying into a sintering furnace with a protective gas atmosphere such as nitrogen for sintering, and control the sintering temperature to 770°C and the sintering time to 9 hours;

[0103] d. Adjust the speed of the first and second stage classification cages of the two-stage series-connected turbine classifier to 800r / min, use compressed air as the working medium, collect the first coarse powder first lithium iron phosphate after the first stage classification, the second fine powder second lithium iron phosphate after the second stage classification, and the fine powder third lithium iron phosphate in the bag collector; wherein, the D50 (D 1 50) is 2 microns; the D50 (D 2 50) is 1.5 microns; Dmo (D 3 mo) is 0.378 microns;

[0104] e. The first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification were mixed in a drum mill at a mass ratio of 4:4:2 until the sphericity was 0.73 to obtain a positive electrode material.

[0105] (2) Preparation of positive electrode

[0106] The positive electrode material prepared above, PVDF and conductive carbon black were dispersed in NMP at a mass ratio of 96.8:2.42:0.78 to form a slurry, and evenly coated on the positive electrode collector. After high-temperature drying, rolling, cutting and stripping, the positive electrode sheet was prepared, wherein the roller press pressure was controlled to be 40T.

[0107] (3) Preparation of negative electrode sheet

[0108] The negative electrode materials hard carbon, styrene-butadiene rubber (SBR), conductive carbon black and sodium carboxymethyl cellulose (CMC) were homogenized in a mass ratio of 93.3:0.03:0.02:0.015 and evenly coated on the negative electrode current collector. The surface density of the electrode sheet was controlled to be 8 mg / cm 2 After high-temperature drying, rolling, cutting and slitting, the negative electrode sheet is prepared.

[0109] (4) Preparation of lithium-ion batteries

[0110] The positive electrode, negative electrode and separator are wound and packaged, and the electrolyte is injected (the composition of the electrolyte is LiPF6, EC, EMC, DEC, DMC=12%:22.5%:52.5%:6.5%:6.5%) to prepare a lithium-ion battery.

[0111] Example 2

[0112] The difference between Example 2 and Example 1 is that in step (a), iron phosphate, a carbon source, and a lithium source are mixed in a mass ratio of 1: 0.18: 1.03;

[0113] In step (c), the sintering temperature is adjusted to 775°C;

[0114] In step (d), the rotation speed of the first stage classification cage and the second stage classification cage is adjusted to 600 r / min, and the D50 of the first lithium iron phosphate collected is 3 microns; the D50 of the second lithium iron phosphate is 1.97 microns; the Dmo of the third lithium iron phosphate in the bag collector is 0.6 microns;

[0115] In step (e), the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification were mixed in a drum mill at a mass ratio of 4:4:2 until the sphericity reached 0.78.

[0116] Example 3

[0117] The difference between Example 3 and Example 1 is that in step (a), iron phosphate, a carbon source, and a lithium source are mixed in a mass ratio of 1: 0.19: 1.03;

[0118] In step (c), the sintering temperature is adjusted to 772°C;

[0119] In step (d), the rotation speed of the first stage classification cage and the second stage classification cage is adjusted to 200 r / min, and the D50 of the first lithium iron phosphate collected is 2.2 microns; the D50 of the second lithium iron phosphate is 1.8 microns; the Dmo of the third lithium iron phosphate in the bag collector is 0.52 microns;

[0120] In step (e), the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification were mixed in a drum mill at a mass ratio of 4:4:2 until the sphericity reached 0.69.

[0121] Example 4

[0122] The difference between Example 4 and Example 1 is that in step (e), the first lithium iron phosphate, the second lithium iron phosphate and the third lithium iron phosphate collected by classification are mixed in a drum mill at a mass ratio of 5:4:1 until the sphericity is 0.73.

[0123] Example 5

[0124] The difference between Example 5 and Example 1 is that in step (e), the first lithium iron phosphate, the second lithium iron phosphate and the third lithium iron phosphate collected by classification are mixed in a drum mill at a mass ratio of 4.5:4:1.5 to a sphericity of 0.73.

[0125] Example 6

[0126] The difference between Example 6 and Example 1 is that in step (e), the first lithium iron phosphate, the second lithium iron phosphate and the third lithium iron phosphate collected by classification are mixed in a drum mill at a mass ratio of 4:4:4 until the sphericity is 0.73.

[0127] Example 7

[0128] The difference between Example 7 and Example 1 is that in step (d), the rotation speed of the first stage grading cage and the second stage grading cage is adjusted to 700 r / min, and the D50 of the first lithium iron phosphate collected is 1 micron; the D50 of the second lithium iron phosphate is 0.8 micron; and the Dmo of the third lithium iron phosphate in the bag collector is 0.35 micron.

[0129] Example 8

[0130] The difference between Example 8 and Example 1 is that in step (d), the rotation speed of the first stage grading cage and the second stage grading cage is adjusted to 750 r / min, and the D50 of the first lithium iron phosphate collected is 2 microns; the D50 of the second lithium iron phosphate is 1.99 microns; and the Dmo of the third lithium iron phosphate in the bag collector is 0.6 microns.

[0131] Example 9

[0132] The difference between Example 9 and Example 1 is that in step (e), the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification are adjusted to be mixed by using a drum mill to have a sphericity of 0.6.

[0133] Example 10

[0134] The difference between Example 10 and Example 1 is that in step (e), the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification are adjusted to be mixed by using a drum mill to have a sphericity of 1.

[0135] Comparative Example 1

[0136] The difference between Comparative Example 1 and Example 1 is that in step (d), the rotation speeds of the first stage classification cage and the second stage classification cage are adjusted to 500 r / min and 200 r / min, and the D50 of the first lithium iron phosphate collected is 2 microns; the D50 of the second lithium iron phosphate is 1.99 microns; the Dmo of the third lithium iron phosphate in the bag collector is 0.59 microns;

[0137] In step (e), the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification were mixed in a drum mill at a mass ratio of 4:4:2 until the sphericity reached 0.69.

[0138] Comparative Example 2

[0139] The difference between Comparative Example 2 and Example 1 is that in step (d), the rotation speeds of the first stage classification cage and the second stage classification cage are adjusted to 600 r / min and 670 r / min, and the D50 of the first lithium iron phosphate collected is 3 microns; the D50 of the second lithium iron phosphate is 1.97 microns; the Dmo of the third lithium iron phosphate in the bag collector is 0.58 microns;

[0140] In step (e), the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate collected by classification were mixed in a drum mill at a mass ratio of 4:4:2 until the sphericity reached 0.81.

[0141] The sphericity of the positive electrode material and the thickness of the carbon coating layer of each embodiment were tested, and the test data are shown in Table 1.

[0142] The batteries prepared in each embodiment were subjected to compaction density test, first charge gram capacity test, energy density test and rate performance test. The test data are shown in Table 2.

[0143] Table 1

[0144]

[0145] In Table 1, z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, where n refers to the mass ratio between the second lithium iron phosphate and the third lithium iron phosphate.

[0146] Table 2

[0147]

[0148] According to the above data, by optimizing the particle size, the particle size distribution of the positive electrode material is limited to meet: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.3≤z≤2.79, is beneficial to the grading of large and small particles and filling the pores between the particles, which can significantly improve the compaction density, thereby solving the problem that there are many pores between the particles of the existing lithium iron phosphate positive electrode material, which makes the compaction density of the electrode sheet small, resulting in low battery energy density and poor rate performance.

[0149] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0150] The above is a detailed introduction to a positive electrode material and a preparation method thereof, a secondary battery and an electrical device provided by the present invention. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for a general technician in this field, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A positive electrode material, characterized in that: The positive electrode material includes a first lithium iron phosphate, a second lithium iron phosphate, and a third lithium iron phosphate, wherein the mass ratio of the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate is (4-5):4:(1-2), and the particle size and morphology distribution of the positive electrode material satisfy: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.6≤z≤2.78; Among them, D 1 50 refers to the D50 of the first lithium iron phosphate, D 2 50 refers to the D50 of the second lithium iron phosphate, D 3 mo refers to the particle size corresponding to the maximum volume fraction of the third lithium iron phosphate, S refers to the sphericity of the positive electrode material, and n refers to the mass ratio of the second lithium iron phosphate to the third lithium iron phosphate; 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3 mo≤0.6μm, 0.6≤S≤1.0, 2≤n≤4.

2. The positive electrode material according to claim 1, characterized in that The sphericity of the first lithium iron phosphate is S1, the sphericity of the second lithium iron phosphate is S2, and the sphericity of the third lithium iron phosphate is S3, and S1, S2, and S3 satisfy: 0.6≤S1≤1.0, and / or, 0.6≤S2≤1.0, and / or, 0.6≤S3≤1.

0.

3. The positive electrode material according to claim 1, characterized in that At least one of the first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate has a carbon coating layer.

4. The positive electrode material according to claim 3, characterized in that The thickness of the carbon coating layer is 2nm~5nm.

5. A method for preparing a positive electrode material according to any one of claims 1 to 4, characterized in that: include: Obtaining lithium iron phosphate, wherein the lithium iron phosphate has a sphericity of 0.6 to 1.0; The lithium iron phosphate is graded to obtain a first lithium iron phosphate, a second lithium iron phosphate, and a third lithium iron phosphate, wherein the D 1 50. D 2 50. D 3 Mo meets: 2μm≤D 1 50≤4μm, 0.8μm≤D 2 50<2μm,0.35μm≤D 3 mo≤0.6μm; The first lithium iron phosphate, the second lithium iron phosphate, and the third lithium iron phosphate are mixed in a mass ratio of (4-5):4:(1-2) to obtain the positive electrode material, the mass ratio n of the second lithium iron phosphate to the third lithium iron phosphate satisfies: 2≤n≤4, the sphericity S of the positive electrode material satisfies: 0.6≤S≤1.0; the positive electrode material satisfies: z=2.35+0.258*D 1 50-0.121*D 2 50-0.639*D 3 mo+0.3125*S+0.0142*n, 2.6≤z≤2.

78.

6. The method for preparing the positive electrode material according to claim 5, characterized in that: Obtaining lithium iron phosphate includes: Mixing iron phosphate and a lithium source to obtain a lithium iron phosphate precursor, grinding the lithium iron phosphate precursor, wherein the particle size D50 of the ground lithium iron phosphate precursor satisfies: 400nm≤D50≤800nm; The ground lithium iron phosphate precursor is dried, sintered and crushed to obtain the lithium iron phosphate, and the sphericity of the lithium iron phosphate is 0.6-1.

0.

7. The method for preparing the positive electrode material according to claim 6, characterized in that: The lithium source includes one or more of Li2CO3 and LiOH.

8. The method for preparing the positive electrode material according to claim 6, characterized in that: Mixing iron phosphate and a lithium source to obtain a lithium iron phosphate precursor further includes: adding a carbon source to the mixture, wherein the carbon source includes one or more of glucose, starch, and phenolic resin.

9. The method for preparing the positive electrode material according to claim 8, characterized in that: The molar ratio of the iron phosphate, the carbon source, and the lithium source is 1:(0.15-0.2):(1-1.04).

10. A secondary battery, characterized in that: The invention comprises a positive electrode plate, wherein the positive electrode plate comprises a positive electrode current collector and a positive electrode active material layer arranged on the positive electrode current collector, wherein the positive electrode active material layer comprises the positive electrode material as described in any one of claims 1 to 4 or the positive electrode material prepared by the method for preparing the positive electrode material as described in any one of claims 5 to 9.

11. An electrical device, characterized in that: The secondary battery according to claim 10 is included, and the secondary battery is used as a power supply for the electrical device.

Citation Information

Patent Citations

  • Lithium iron phosphate positive electrode active material, preparation method thereof, positive electrode plate and battery

    CN114068920A

  • Lithium iron phosphate positive electrode active material, preparation method thereof, positive electrode plate and battery

    CN114068921A

  • Positive electrode active material, positive plate and lithium ion battery

    CN115312763A

  • Positive electrode active material composition, aqueous positive electrode slurry, positive electrode sheet, secondary battery, and electric device

    CN116565153A

  • Lithium iron phosphate positive active material and preparation method thereof, positive pole piece and lithium ion battery

    CN116779777A