Implantable medical device with high bonding strength, preparation method and application thereof

By preparing micron concave holes and nano-round wells on the surface of the medical metal substrate of the implantable medical device, a mechanical interlocking structure is formed, which solves the problem of low bonding strength and improves the stability and durability of the implantable medical device. , reducing the risk of inflammation and immune response.

CN118542969BActive Publication Date: 2024-10-18QIYUAN FUTURE (GUANGZHOU) CELL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410994480.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-18
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The bonding strength between the medical metal substrate and the medical polymer coating in existing implantable medical devices is not high, which may cause the coating to fall off under the action of external forces, increasing the risk of inflammation and immune rejection.

Method used

By preparing micron concave holes and nano-circular wells on the surface of medical metal substrates, and using femtosecond laser and anodizing processes to form a mechanical interlocking structure, the medical polymer coating is embedded into the surface of the substrate to enhance the bonding strength.

Benefits of technology

Significantly improves the bonding strength between medical metal substrates and medical polymer coatings, enhances the stability and durability of implantable medical devices, reduces the risk of coating shedding, and reduces inflammation and immune responses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118542969B_ABST
    Figure CN118542969B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of medical device technology, and in particular, relates to an implantable medical device with high bonding strength, a preparation method and an application thereof. The implantable medical device provided by the present application comprises a medical metal substrate and a medical polymer coating on its surface. By improving the surface structure of the medical metal substrate, the surface of the medical metal substrate is micron-shaped recessed holes with nano-circular wells, and the bottom surface of the medical polymer coating is embedded in the micron-shaped recessed holes with nano-circular wells, so that the bonding is tighter, resulting in mechanical interlocking, which greatly improves the bonding strength. The medical polymer coating is difficult to fall off from the surface of the medical metal substrate, thereby improving the stability and durability of the implantable medical device. Thus, the technical problem of low bonding strength between the medical metal substrate and the medical polymer coating in the implantable medical device in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of medical device technology, and in particular relates to an implantable medical device with high bonding strength, a preparation method and an application thereof. Background Art

[0002] Medical metals used as implantable medical devices may loosen from the surrounding bone tissue after implantation, while medical polymer implants do not have sufficient mechanical strength. Therefore, the implantable medical devices currently used are usually composed of a medical metal substrate and a medical polymer coating. Implantable medical devices can combine the excellent mechanical properties and corrosion resistance of medical metals with the good biocompatibility and degradability of medical polymers, becoming a research direction with great development potential in the field of medical enterprises.

[0003] In the actual application of implantable medical devices, on the one hand, it is necessary to improve the biocompatibility of medical polymer coatings and promote the attachment, proliferation and differentiation of cells such as bone cells on their surfaces. On the other hand, it is necessary to improve the friction between medical metal substrates and medical polymer coatings and improve the interface bonding strength. For metal-polymer implantable medical devices, improving the bonding strength between the medical metal substrate and the medical polymer coating interface and the biocompatibility of the medical polymer coating are of great significance to further broaden the application scope of medical implantable devices. The bonding force between medical metal substrates and medical polymer coatings can be improved by adhesives. However, after the implantable medical device is implanted in the human body, the use of adhesives will increase the risk of various inflammations and immune rejection. At the same time, the bonding strength of the adhesive may also decay over time. The use of pure physical bonding methods will be more suitable for implantable medical devices. At present, medical polymer coatings can also be bonded to the surface of medical metal substrates by molding and other processes. However, molding and other processes do not improve the bonding strength between medical metal substrates and medical polymer coatings. When subjected to external forces, the medical polymer coating may fall off from the surface of the medical metal substrate. Summary of the invention

[0004] In view of this, the present application provides an implantable medical device with high bonding strength, and a preparation method and application thereof, which are used to solve the technical problem of low bonding strength between a medical metal substrate and a medical polymer coating in implantable medical devices in the prior art.

[0005] In a first aspect, the present application provides an implantable medical device with high bonding strength, comprising a medical metal substrate and a medical polymer coating;

[0006] The surface of the medical metal substrate is distributed with micron-sized concave pores;

[0007] The surface of the micron-shaped recessed holes is distributed with nano-circular wells;

[0008] The bottom surface of the medical polymer coating is embedded in the surface of the medical metal substrate to form a mechanical interlock.

[0009] Preferably, the shape of the micron recessed hole is hemispherical and / or spherical.

[0010] Preferably, the radius of the spherical segment is 20-200 μm, and the height is 30-300 μm;

[0011] The height of the nano-circular well is 10-100 μm, and the bottom radius is 50-500 nm.

[0012] Preferably, the surface of the medical metal substrate has micron-shaped recessed holes distributed in an array with equal spacing;

[0013] The surface of the micron-concave holes is arrayed with nano-circular wells at equal intervals.

[0014] Preferably, the distance between adjacent micron recessed holes is 10-100 μm.

[0015] The spacing between adjacent nano-circular wells is 10-500 nm.

[0016] Preferably, the surface of the medical polymer coating is combined with a medical polymer with a composite micro-nano structure;

[0017] The composite micro-nano structured medical polymer comprises a micron structured medical polymer and a nano structured medical polymer;

[0018] The medical polymer coating surface is combined with the medical polymer with micron structure, and the medical polymer with micron structure is combined with the medical polymer with nanometer structure on its surface.

[0019] Preferably, the microstructured medical polymer is hemispherical in shape with a radius of 20 to 200 μm;

[0020] The nanostructured medical polymer is hemispherical in shape, with a radius of 100-500 nm.

[0021] Preferably, the surface of the medical polymer coating is integrally combined with a medical polymer having a micron structure;

[0022] The surface of the medical polymer coating is integrally combined with a medical polymer with a nanostructure.

[0023] Preferably, the micron-structured medical polymer is distributed on the surface of the medical polymer coating in an equidistant array manner;

[0024] The spacing between adjacent microstructured medical polymers is 10-100 μm;

[0025] Preferably, the nanostructured medical polymer is distributed on the surface of the microstructured medical polymer in an equidistant array;

[0026] The distance between adjacent nanostructured medical polymers is 10-200 nm.

[0027] The second aspect of the present application provides a method for preparing an implantable medical device with high bonding strength, the method comprising the steps of:

[0028] Step S1, using a femtosecond laser to prepare hemispherical micron-shaped concave holes on the surface of medical metal;

[0029] Step S2, etching the hemispherical micron-shaped concave holes with acid to obtain spherical micron-shaped concave holes;

[0030] Step S3, preparing nano-circular wells on the inner surface of the spherical micron-shaped concave holes by anodic oxidation to obtain a medical metal substrate;

[0031] Step S4: Pressing the medical polymer onto the surface of the medical metal substrate to obtain an implantable medical device with high bonding strength.

[0032] Preferably, step S4 specifically includes:

[0033] Step S41, using a femtosecond laser to prepare hemispherical micron-shaped concave holes on the surface of a metal mold substrate;

[0034] Step S42, preparing hemispherical nano-concave holes on the inner surface of the hemispherical micro-concave holes by anodizing to obtain a micro-nano structure metal mold;

[0035] Step S43: Using a micro-nano structure mold to press the medical polymer onto the surface of the medical metal substrate to obtain an implantable medical device with high bonding strength.

[0036] Preferably, in step S1, the power of the femtosecond laser is 20-60W, and the wavelength is 900-1100nm;

[0037] In step S2, the acid is hydrochloric acid with a concentration of 1-3 mol / L;

[0038] In step S3, the electrolyte used for the anodization is ammonium fluoride / ethylene glycol electrolyte, the concentration of ammonium fluoride is 0.1 ~ 0.3 mol / L, the oxidation voltage is 20 ~ 40V, the oxidation temperature is 20 ~ 30 ℃, and the oxidation time is 10 ~ 30min;

[0039] In step S41, the power of the femtosecond laser is 20-60W, and the wavelength is 900-1100nm;

[0040] In step S42, the electrolyte used for anodization is oxalic acid / ethanol electrolyte, the oxalic acid concentration is 0.1-0.3 mol / L, the oxidation voltage is 40-80 V, the oxidation temperature is -10-0° C., and the oxidation time is 10-30 min;

[0041] In step S43, the medical polymer is pressed by injection molding or compression molding;

[0042] The temperature of medical polymer molding was 230°C, the pressure was 2 MPa, and the time was 3 min.

[0043] A third aspect of the present application provides the use of an implantable medical device with high bonding strength in the preparation of an orthopedic implantable medical device.

[0044] In summary, the present application provides an implantable medical device with high bonding strength, a preparation method and an application. The implantable medical device provided by the present application includes a medical metal substrate and a medical polymer coating on its surface; wherein, the surface of the medical metal substrate is distributed with micron-shaped recessed holes, and the surface of the micron-shaped recessed holes is distributed with nano-shaped circular wells, so that when the bottom of the medical polymer coating is embedded in the surface of the medical metal substrate, it will form a mechanical interlocking effect with the micron-shaped recessed holes with nano-shaped circular wells. At the same time, the micron-shaped recessed holes with nano-shaped circular wells also greatly increase the bonding area between the medical metal substrate and the medical polymer coating, making the bonding tighter, and the medical polymer coating is difficult to fall off from the surface of the medical metal substrate. The bonding strength is greatly improved, thereby improving the stability and durability of the implantable medical device; thereby solving the technical problem of low bonding strength between the medical metal substrate and the medical polymer coating in the prior art of implantable medical devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0046] Figure 1 A schematic diagram of the structure of an implantable medical device with high bonding strength provided in Example 2 of the present application;

[0047] Figure 2 A schematic diagram of preparing nano-circular wells on the inner surface of micron-shaped recessed holes by anodic oxidation in an implantable medical device with high bonding strength provided in Example 2 of the present application;

[0048] Figure 3A schematic diagram of preparing micron-sized recessed holes on the surface of an aluminum sheet using a femtosecond laser process in an implantable medical device with high bonding strength provided in Example 2 of the present application;

[0049] Figure 4 A schematic diagram of preparing nano-recessed holes on the inner surface of micro-recessed holes by anodic oxidation in an implantable medical device with high bonding strength provided in Example 2 of the present application;

[0050] Figure 5 This is a scanning electron microscope photograph of nano-holes prepared on the surface of an aluminum sheet using a femtosecond laser process in an implantable medical device with high bonding strength provided in Example 2 of the present application. DETAILED DESCRIPTION

[0051] The present application provides an implantable medical device with high bonding strength, a preparation method and an application thereof, which are used to solve the technical problem of low bonding strength between a medical metal substrate and a medical polymer coating in implantable medical devices in the prior art.

[0052] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0053] In view of the low bonding strength of the current medical polymer coating, the medical polymer coating may fall off from the surface of the medical metal substrate when impacted by external force; in view of this, the present application provides a technical solution for improving the surface structure of the medical metal substrate in an implantable medical device; the implantable medical device provided by the present application includes a medical metal substrate and a medical polymer coating covering its surface; and the surface of the medical metal substrate is distributed with micron-shaped recessed holes, and the surface of the micron-shaped recessed holes is distributed with nano-circular wells; wherein, the micron-shaped recessed holes are obtained by introducing femtosecond laser technology and other processes to process the medical metal substrate. Femtosecond laser technology can be used to process metals, ceramics, plastics, glass and other materials. It has a wide range of applicability in material processing and has extremely high precision. It can be used on the surface of medical metals. The processing obtains micron-shaped concave holes with a depth and width of tens to hundreds of microns. The micron-shaped concave holes obtained by femtosecond laser technology are deeper and wider, which is beneficial to increase the contact area with the medical polymer coating and improve the bonding strength. At the same time, the anodic oxidation process is also used to prepare nano-circular wells on the inner surface of the micron-shaped concave holes. The present application improves the surface structure of the medical metal substrate so that the surface of the medical metal substrate is micron-shaped concave holes with nano-circular wells. When the medical polymer coating such as polylactic acid (PLA) is pressed onto the surface of the medical metal substrate such as titanium alloy, the polylactic acid (PLA) will be embedded in the micron-shaped concave holes with nano-circular wells, forming a mechanical interlocking effect. At the same time, the nano-circular wells also greatly increase the bonding area between the medical metal substrate and the medical polymer coating, making the bonding tighter.

[0054] Specifically, when the medical polymer coating is subjected to peeling force, the micron-shaped concave holes with nano-circular wells produce compressive stress on the medical polymer coating, and the coating is subjected to the friction between the micron-shaped concave holes and the polymer, and the friction between the nano-circular wells and the polymer. The mechanical interlocking effect formed by the micron-shaped concave holes with nano-circular wells and the polymer doubles the contact area and friction with the polymer coating. Therefore, when the coating is subjected to an upward peeling force F 1 When the nano-wells in the micron pits produce compressive stress on the polymer coating, the friction between the nanotube structure and the polymer coating can be enhanced. The direction of the resultant friction force is opposite to the peeling force, which can prevent the polymer coating from peeling off and greatly improve its bonding strength. The medical polymer coating is difficult to fall off from the surface of the medical metal substrate, thereby improving the stability and durability of implantable medical devices.

[0055] Preferably, the shape of the micron recessed hole can be a hemisphere or a spherical segment; when the micron recessed hole is in the shape of a spherical segment, on the basis of obtaining the hemisphere by femtosecond laser processing, it is necessary to further expand it inward by hydrochloric acid corrosion to obtain a micron recessed hole in the shape of a spherical segment; the spherical segment is a geometric body, which refers to the remaining part of a sphere after being cut by a plane, the cross section is used as the bottom surface of the spherical segment, the bottom surface of the spherical segment faces the medical polymer coating, and the length of the line segment remaining after the diameter perpendicular to the cross section is cut is used as the height of the spherical segment; since the micron recessed hole in the shape of a spherical segment is narrow at the top and wide at the bottom, it cooperates with the nano-circular well prepared on the inner surface to form a mechanically interlocked micro-nano structure connection, which greatly improves the bonding strength and connection stability between the medical metal substrate and the medical polymer in the implantable medical device.

[0056] Preferably, for the size of the micron recessed hole, the radius of the hemispherical or spherical micron recessed hole is 20-200 μm, and the height of the spherical cavity is greater than the radius, which is 30-300 μm; while the height of the nano-circular well is 10-100 μm, and the bottom radius is 50-500 nm.

[0057] Preferably, for the distribution of micron-pitted holes, the micron-pitted holes on the surface of the medical metal substrate in the present application are distributed in an equally spaced array with a spacing of 10~100μm; an equally spaced array means that the spacing between any adjacent micron-pitted holes is equal. After the implantable medical device is implanted in the human body and subjected to mechanical shock, the occurrence of excessive local force is reduced, the implantable medical device is subjected to more uniform force, and the stability and durability of the implantable medical device are improved; at the same time, the nano-circular wells can also be set to be distributed in an equally spaced array with a spacing of 10~500nm.

[0058] Preferably, the present application also improves the surface structure of the medical polymer coating in the implantable medical device, and sets a micro-nano structure on the surface of the medical polymer coating; the medical polymer with the micro-nano structure increases the roughness and surface area of ​​the implantable medical device, thereby increasing the contact area between the implantable medical device and the cells, thereby forming a more stable large-area adhesion spot, making the adhesion between the cells and the implantable medical device stronger, and promoting the proliferation and differentiation of cells on the surface of the implantable medical device.

[0059] For the micro-nano structure, the micro-nano structure can be a single hemispherical micron structure with a radius of 20~200 μm. The micro-nano structure can also be a composite micro-nano structure. The medical polymer of the composite micro-nano structure includes a medical polymer of micron structure and a medical polymer of nanostructure. The surface of the medical polymer coating is combined with the medical polymer of micron structure, and the surface of the medical polymer of micron structure is combined with the medical polymer of nanostructure. The micro-nano structure can also be a multi-level micro-nano structure, that is, a second nanostructure is prepared on the surface of the nanostructure. Among them, the single micron structure can be obtained by preparing micron concave holes on the mold surface by femtosecond laser and then pressing the medical polymer, while the composite micro-nano structure needs to be anodized on the micron concave holes on the basis of femtosecond laser, and then pressed with the medical polymer to obtain it; the multi-level micro-nano structure needs to be anodized again and then pressed with the medical polymer to obtain it; compared with the single micro-nano structure, the composite micro-nano structure has a higher contact area with cells, and compared with the composite micro-nano structure, the multi-level micro-nano structure has a higher contact area with cells, which can better promote the proliferation and differentiation of cells on the surface of implantable medical devices.

[0060] Regarding the shape and size of the microstructure, the shape of the microstructured medical polymer in the present application is a hemispherical microstructure with a radius of 20-200 μm; and the shape of the nanostructured medical polymer is also a hemispherical nanostructure with a radius of 100-500 nm.

[0061] Preferably, in implantable medical devices, the present application also optimizes the positional distribution of micron-structured medical polymers and nano-structured medical polymers, so that the micron-structured medical polymers are distributed in an equidistant array on the upper surface of the medical polymer. The equidistant array means that any adjacent micro-nano-structured medical polymers have the same spacing, which is 10 to 100 μm; and the nano-structured medical polymers are also distributed in an equidistant array on the upper surface of the micron-structured medical polymer, with a smaller spacing of 10 to 200 nm; the distribution of the equidistant array is beneficial to reduce the occurrence of excessive local force after the implantable medical device is implanted in the human body and is subjected to mechanical shock, so that the implantable medical device is subjected to more uniform force, thereby improving the stability and durability of the implantable medical device.

[0062] Example 1

[0063] Example 1 of the present application provides a method for preparing an implantable medical device with high bonding strength, the preparation method comprising: a step of preparing a medical metal substrate, a step of preparing a micro-nanostructure mold, and a step of preparing a micro-nanostructure medical polymer on the surface of the medical metal substrate.

[0064] The steps of preparing the medical metal substrate include:

[0065] Step I: using a femtosecond laser to prepare hemispherical micron-shaped recessed holes on the surface of titanium alloy medical metal.

[0066] The titanium alloy is first polished with sandpaper, cleaned and dried, and then placed horizontally on a laser processing table for femtosecond laser processing; the laser center wavelength of the femtosecond laser processing is set to 1035nm, and the power is 40W, and then the titanium alloy material is laser ablated to obtain an array of micron-shaped concave holes on the surface of the sealed titanium alloy; the shape of the micron-shaped concave holes is hemispherical, with a radius of 20μm, and they are distributed in an equidistant array with a spacing of 10μm.

[0067] Step II: preparing nano-circular wells on the inner surface of the micron-concave hole by anodizing.

[0068] The titanium alloy obtained in step I is ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each to remove oil stains adhering to the surface, and then polished in an electrochemical polishing solution with a volume ratio of V hydrofluoric acid: V nitric acid: V deionized water = 1:1:8, and then ultrasonically cleaned with deionized water, blown dry with cold air, and used as an anode, a graphite sheet as a cathode, and an ammonium fluoride / ethylene glycol electrolyte system is selected, the ammonium fluoride concentration is 0.2 mol / L, the oxidation voltage is 30 V, the oxidation temperature is 25°C, and the oxidation time is 20 min. Nano-circular wells are prepared on the inner surface of the micron-shaped concave hole; the nano-circular well height is 50 μm, the bottom radius is 100 nm, and the nano-circular wells are evenly spaced in an array with a spacing of 200 nm.

[0069] Step III: annealing the titanium alloy medical metal substrate.

[0070] The titanium alloy obtained in step II is placed in ethanol, cleaned with low-power ultrasonic waves, and dried; then placed in a micro-box furnace for annealing at a temperature of 450°C, an annealing holding time of 60 minutes, and a heating rate of 5°C / min. After annealing, the structure of the titanium alloy medical metal substrate is stable.

[0071] The steps of preparing the micro-nano structure mold include:

[0072] Step I: prepare micron-sized recessed holes on the surface of the aluminum sheet using a femtosecond laser process.

[0073] The pretreated aluminum sheet surface is placed horizontally with the horizontal plane of the laser processing workbench. Micron-shaped recessed holes can be obtained on the aluminum sheet surface by laser femtosecond etching. Repeating the process many times, an aluminum sheet with an array of micron-shaped recessed holes distributed on the surface can be obtained. The micron-shaped recessed holes are hemispherical in shape, semicircular in cross section, with a radius of 40μm, and are evenly spaced in an array with a spacing of 10μm.

[0074] Step II: preparing nano-concave holes on the inner surface of the micro-concave holes by anodizing.

[0075] The aluminum sheet obtained in step I is cleaned, and ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each to remove oil stains adhering to the surface, and polished in an electrochemical polishing solution with a volume ratio of V perchloric acid: V ethanol = 1:9, and then ultrasonically cleaned with deionized water, dried with cold wind, and used as an anode, and a graphite sheet as a cathode. An oxalic acid / ethanol electrolyte system is selected, and the oxalic acid concentration is 0.2 mol / L. An anodizing treatment is performed once. The oxidation voltage of the anodizing treatment is 60 V, the oxidation temperature is -5°C, and the oxidation time is 20 min. Nano-concave holes are prepared to obtain a micro-nano structure mold; the shape of the nano-concave holes is hemispherical, the cross section is semicircular, the radius is 200 nm, and the array distribution is equidistant with a spacing of 100 nm.

[0076] The steps of preparing a micro-nanostructured medical polymer on the surface of a medical metal substrate include:

[0077] After placing the anodized micro-nanostructure mold, polylactic acid (PLA) and the treated titanium alloy medical metal substrate in order, the molding process is maintained at a temperature of 230°C and a pressure of 2MPa for 3 minutes. After the aluminum sheet is demolded, a coating with a micro-nanostructure medical polymer can be prepared on the surface of the titanium alloy medical metal substrate. The coating is 15*60mm*3mm PLA, and the shape and size of the micro-nanostructure medical polymer are the same as the micron-shaped pores and nano-shaped pores in the micro-nanostructure mold.

[0078] Example 2

[0079] Example 2 of the present application provides a method for preparing an implantable medical device with high bonding strength, the structure of which is as follows: Figure 1 As shown, the difference between the preparation method and Example 1 is that hydrochloric acid is used to expand the micron-concave holes on the surface of the titanium alloy as quickly as possible; it includes: the steps of preparing a medical metal substrate, the steps of preparing a micro-nano structure mold, and the steps of preparing a micro-nano structure medical polymer on the surface of the medical metal substrate.

[0080] The steps of preparing the medical metal substrate include:

[0081] Step I: using a femtosecond laser to prepare hemispherical micron-shaped recessed holes on the surface of titanium alloy medical metal.

[0082] The titanium alloy is first polished with sandpaper, cleaned and dried, and the entire titanium alloy is sealed with polyethylene terephthalate glue (PET glue). The sealed titanium alloy is placed horizontally on a laser processing table for femtosecond laser processing; the laser center wavelength of the femtosecond laser processing is set to 1035nm, and the power is 40W. Then the titanium alloy material is laser ablated to obtain an array of micron-shaped concave holes on the surface of the sealed titanium alloy; the shape of the micron-shaped concave holes is hemispherical, with a radius of 20μm, and they are evenly spaced in an array with a spacing of 10μm.

[0083] Step II: using hydrochloric acid corrosion to expand the micron-shaped concave hole to prepare a spherical micron-shaped concave hole.

[0084] The titanium alloy surface obtained in step I is ultrasonically cleaned to remove residual debris on the surface, and then dried with cold air to retain the polyethylene terephthalate glue on the titanium alloy surface; then it is placed in dilute hydrochloric acid with a concentration of 2 mol / L for corrosion. Since the polyethylene terephthalate glue protects the titanium alloy surface from acid corrosion, the hemispherical micron-shaped concave holes are expanded inward to obtain spherical micron-shaped concave holes with a radius of 40 μm and a height of 60 μm, which are evenly spaced in an array with a spacing of 10 μm.

[0085] Step III: preparing nano-circular wells on the inner surface of the micron-concave hole by anodizing.

[0086] The PET glue on the surface of the titanium alloy obtained in step II was torn off, and the alloy was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 minutes each to remove the oil stains adhering to the surface, and the alloy was polished in an electrochemical polishing solution with a volume ratio of V hydrofluoric acid: V nitric acid: V deionized water = 1:1:8, and then ultrasonically cleaned with deionized water, dried with cold air, and used as an anode, a graphite sheet as a cathode, and an ammonium fluoride / ethylene glycol electrolyte system with an ammonium fluoride concentration of 0.2 mol / L, an oxidation voltage of 30 V, an oxidation temperature of 25°C, and an oxidation time of 20 minutes to prepare nano-circular wells on the inner surface of the micron-shaped recessed holes; the nano-circular wells had a height of 50 μm and a bottom radius of 100 nm.

[0087] Step IV: annealing the titanium alloy medical metal substrate.

[0088] The titanium alloy obtained in step III is placed in ethanol, cleaned with low-power ultrasonic waves, and dried; then placed in a micro-box furnace for annealing at a temperature of 450°C, an annealing holding time of 60 minutes, and a heating rate of 5°C / min. After annealing, the structure of the titanium alloy medical metal substrate is stable.

[0089] The steps of preparing the micro-nano structure mold include:

[0090] Step I: prepare micron-sized recessed holes on the surface of the aluminum sheet using a femtosecond laser process.

[0091] The pretreated aluminum sheet surface is placed horizontally with the horizontal plane of the laser processing workbench. Micron-shaped recessed holes can be obtained on the aluminum sheet surface by laser femtosecond etching. Repeating the process many times, an aluminum sheet with an array of micron-shaped recessed holes distributed on the surface can be obtained. The micron-shaped recessed holes are hemispherical in shape, semicircular in cross section, with a radius of 40μm, and are evenly spaced in an array with a spacing of 10μm.

[0092] Step II: preparing nano-concave holes on the inner surface of the micro-concave holes by anodizing.

[0093] The aluminum sheet obtained in step I is cleaned, ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 minutes each to remove oil stains adhering to the surface, and polished in an electrochemical polishing solution with a volume ratio of V perchloric acid: V ethanol = 1:9, and then ultrasonically cleaned with deionized water, dried with cold wind, and used as an anode, and a graphite sheet as a cathode. An oxalic acid / ethanol electrolyte system is selected, and the oxalic acid concentration is slightly 0.2 mol / L. An anodizing treatment is performed once. The oxidation voltage of the anodizing treatment is 60 V, the oxidation temperature is -5°C, and the oxidation time is 20 minutes. Nano-concave holes are prepared to obtain a composite micro-nano structure mold; the shape of the nano-concave hole is hemispherical, the cross section is semicircular, and the radius is 200 nm.

[0094] The steps of preparing a micro-nanostructured medical polymer on the surface of a medical metal substrate include:

[0095] After placing the anodized micro-nanostructure mold, polylactic acid (PLA) and untreated titanium alloy medical metal substrate in order, the molding process is maintained at a temperature of 230°C and a pressure of 2MPa for 3 minutes. After the aluminum sheet is demolded, a coating with a micro-nanostructure medical polymer can be prepared on the surface of the titanium alloy medical metal substrate. The coating is 15*60mm*3mm PLA, and the shape and size of the micro-nanostructure medical polymer are the same as the micron-shaped pores and nano-shaped pores in the micro-nanostructure mold.

[0096] Example 3

[0097] Example 3 of the present application provides a method for preparing an implantable medical device with high bonding strength. The difference between the preparation method and Example 2 is that, on the basis of preparing nano-recesses on the inner surface of micro-recesses by anodizing, a secondary anodizing treatment can be performed to prepare a second nano-recesses to obtain a multi-level micro-nano structure.

[0098] Example 4

[0099] Example 4 of the present application provides a method for preparing an implantable medical device with high bonding strength. The difference between the preparation method and Example 2 is that, based on the preparation of nano-recesses on the inner surface of micro-recesses by anodizing, after the titanium alloy is wrapped with polyethylene terephthalate glue, it is immersed in a 5wt% phosphoric acid solution for pore expansion to obtain a spherical micro-nano structure.

[0100] Comparative Example 1

[0101] Comparative Example 1 of the present application provides a method for preparing an implantable medical device. The difference between the preparation method and Example 2 is that the preparation method does not include the step of preparing a medical metal substrate, and the preparation method includes the steps of preparing a micro-nanostructure mold and preparing a micro-nanostructure medical polymer on the surface of a titanium alloy.

[0102] The steps of preparing the micro-nano structure mold include:

[0103] Step I: prepare micron-sized recessed holes on the surface of the aluminum sheet using a femtosecond laser process.

[0104] The pretreated aluminum sheet surface is placed horizontally with the horizontal plane of the laser processing workbench. Micron-shaped recessed holes can be obtained on the aluminum sheet surface by laser femtosecond etching. Repeating the process many times, an aluminum sheet with an array of micron-shaped recessed holes distributed on the surface can be obtained. The micron-shaped recessed holes are hemispherical in shape, semicircular in cross section, with a radius of 40μm, and are evenly spaced in an array with a spacing of 10μm.

[0105] Step II: preparing nano-concave holes on the inner surface of the micro-concave holes by anodizing.

[0106] The aluminum sheet obtained in step I is cleaned, ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each to remove oil stains adhering to the surface, and polished in an electrochemical polishing solution with a volume ratio of V perchloric acid: V ethanol = 1:9, and then ultrasonically cleaned with deionized water, dried with cold wind, and used as an anode, and a graphite sheet as a cathode. An oxalic acid / ethanol electrolyte system is selected, and the oxalic acid concentration is slightly 0.2 mol / L. An anodizing treatment is performed once. The oxidation voltage of the anodizing treatment is 60 V, the oxidation temperature is -5°C, and the oxidation time is 20 min. Nano-concave holes are prepared to obtain a composite micro-nano structure mold; the shape of the nano-concave hole is hemispherical, the cross section is semicircular, and the radius is 200 nm.

[0107] The steps of preparing micro-nanostructured medical polymers on the surface of titanium alloy include:

[0108] After placing the anodized micro-nanostructure mold, polylactic acid (PLA) and untreated titanium alloy in order, the molding process is carried out at a temperature of 230°C and a pressure of 2 MPa for 3 minutes. After the aluminum sheet is demolded, a coating of a micro-nanostructured medical polymer can be prepared on the surface of the titanium alloy. The coating is 15*60mm*3mm PLA.

[0109] Comparative Example 2

[0110] Comparative Example 2 of the present application provides a method for preparing an implantable medical device. The difference between the preparation method and Example 2 is: the step of preparing a medical metal substrate, the preparation method includes: the step of preparing a medical metal substrate, the step of preparing a micro-nano structure mold, and the step of preparing a micro-nano structure medical polymer on the surface of the medical metal substrate.

[0111] The steps of preparing the medical metal substrate include:

[0112] Step I: using a femtosecond laser to prepare hemispherical micron-shaped recessed holes on the surface of titanium alloy medical metal.

[0113] The titanium alloy is first polished with sandpaper, cleaned and dried, and the entire titanium alloy is sealed with polyethylene terephthalate glue (PET glue). The sealed titanium alloy is placed horizontally on a laser processing table for femtosecond laser processing; the laser center wavelength of the femtosecond laser processing is set to 1035nm, and the power is 40W. Then the titanium alloy material is laser ablated to obtain an array of micron-shaped concave holes on the surface of the sealed titanium alloy; the shape of the micron-shaped concave holes is hemispherical, with a radius of 20μm, and they are evenly spaced in an array with a spacing of 10μm.

[0114] Step II: annealing the titanium alloy medical metal substrate.

[0115] The titanium alloy obtained in step I is placed in ethanol, cleaned with low-power ultrasonic waves, and dried; then placed in a micro-box furnace for annealing, the annealing temperature is 450°C, the annealing holding time is 60 minutes, and the heating rate is 5°C / min. After annealing, the structure of the titanium alloy medical metal substrate is stable.

[0116] The steps of preparing the micro-nano structure mold include:

[0117] Step I: prepare micron-sized recessed holes on the surface of the aluminum sheet using a femtosecond laser process.

[0118] The pretreated aluminum sheet surface is placed horizontally with the horizontal plane of the laser processing workbench. Micron-shaped recessed holes can be obtained on the aluminum sheet surface by laser femtosecond etching. Repeating the process many times, an aluminum sheet with an array of micron-shaped recessed holes distributed on the surface can be obtained. The micron-shaped recessed holes are hemispherical in shape, semicircular in cross section, with a radius of 40μm, and are evenly spaced in an array with a spacing of 10μm.

[0119] Step II: preparing nano-concave holes on the inner surface of the micro-concave holes by anodizing.

[0120] The aluminum sheet obtained in step I is cleaned, ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each to remove oil stains adhering to the surface, and polished in an electrochemical polishing solution with a volume ratio of V perchloric acid: V ethanol = 1:9, and then ultrasonically cleaned with deionized water, dried with cold wind, and used as an anode, and a graphite sheet as a cathode. An oxalic acid / ethanol electrolyte system is selected, and the oxalic acid concentration is slightly 0.2 mol / L. An anodizing treatment is performed once. The oxidation voltage of the anodizing treatment is 60 V, the oxidation temperature is -5°C, and the oxidation time is 20 min. Nano-concave holes are prepared to obtain a composite micro-nano structure mold; the shape of the nano-concave hole is hemispherical, the cross section is semicircular, and the radius is 200 nm.

[0121] The steps of preparing micro-nanostructured medical polymers on the surface of titanium alloy include:

[0122] After placing the anodized micro-nanostructure mold, polylactic acid (PLA) and untreated titanium alloy in order, the molding process is carried out at a temperature of 230°C and a pressure of 2 MPa for 3 minutes. After the aluminum sheet is demolded, a coating of a micro-nanostructured medical polymer can be prepared on the surface of the titanium alloy. The coating is 15*60mm*3mm PLA.

[0123] Experimental Example 1

[0124] In this Experimental Example 1, the implantable medical devices provided in Examples 1-2 and Comparative Examples 1-2 were subjected to performance testing; the performance testing included: stretching the obtained implantable medical device at a speed of 50 mm / min using a universal testing machine, and calculating the bonding strength thereof. The bonding strength results are shown in Table 1.

[0125] Table 1: Bonding strength of implantable medical devices provided by Examples 1-2 and Comparative Examples 1-2

[0126]

[0127] As can be seen from Table 1, the titanium alloy surface provided in Comparative Example 1 does not have any micron or nanostructure, so that the bonding strength between PLA and the titanium alloy is extremely weak, below the detection limit of the universal testing machine, and the bonding strength is 0; while the bonding strength of the medical titanium alloy provided in Comparative Example 2 is about 20MPa after having a micron-concave pore structure on the surface, and after further distributing nano-circular wells inside the micron-concave pores, the bonding strength between PLA and the medical titanium alloy can be increased to about 23MPa, an increase of about 15%, which is a relatively high increase; and after further corroding the shape of the micron-concave pores to form spherical-shaped micron-concave pores, the bonding strength can be further increased by about 10% to 25.5MPa; this shows that the present application can improve the bonding strength between PLA and the medical titanium alloy by improving the microstructure of the surface of the medical titanium alloy and setting micron-concave pores and nano-circular wells, spherical-shaped micron-concave pores and nano-circular wells, which is beneficial to the long-term stability of implantable medical devices.

[0128] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. An implantable medical device with high bonding strength, characterized in that: Including medical metal substrates and medical polymer coatings; The surface of the medical metal substrate is distributed with micron-sized concave pores; The surface of the micron-shaped recessed holes is distributed with nano-circular wells; The bottom surface of the medical polymer coating is embedded in the surface of the medical metal substrate to form a mechanical interlock; The shape of the micron-shaped recessed hole is a spherical segment; The radius of the spherical part is 20-200 μm, and the height is 30-300 μm; The height of the nano-circular well is 10-100 μm, and the bottom radius is 50-500 nm; The bottom surface of the spherical segment faces the medical polymer coating, and the length of the remaining line segment after the diameter perpendicular to the cross section is cut is used as the height of the spherical segment. The micron-shaped concave hole of the spherical segment is narrow at the top and wide at the bottom. The preparation method of the medical metal substrate comprises: Step S1, using a femtosecond laser to prepare hemispherical micron-shaped concave holes on the surface of medical metal; Step S2, etching the hemispherical micron-shaped concave holes with acid to obtain spherical micron-shaped concave holes; Step S3, preparing nano-circular wells on the inner surface of the spherical-shaped micron-shaped recessed holes by anodizing to obtain a medical metal substrate.

2. An implantable medical device with high bonding strength according to claim 1, characterized in that: The surface of the medical metal substrate is provided with micron-concave holes arranged in an array with equal spacing.

3. An implantable medical device with high bonding strength according to claim 1, characterized in that: The surface of the micron-concave holes is arrayed with nano-circular wells at equal intervals.

4. The implantable medical device with high bonding strength according to claim 1, characterized in that: The surface of the medical polymer coating is combined with a medical polymer having a composite micro-nano structure; The composite micro-nano structured medical polymer comprises a micron structured medical polymer and a nano structured medical polymer; The medical polymer coating surface is combined with the medical polymer with micron structure, and the medical polymer with micron structure is combined with the medical polymer with nanometer structure on its surface.

5. A method for preparing an implantable medical device with high bonding strength according to any one of claims 1 to 4, characterized in that: Includes steps: Step S1, using a femtosecond laser to prepare hemispherical micron-shaped concave holes on the surface of medical metal; Step S2, etching the hemispherical micron-shaped concave holes with acid to obtain spherical micron-shaped concave holes; Step S3, preparing nano-circular wells on the inner surface of the spherical micron-shaped concave holes by anodic oxidation to obtain a medical metal substrate; Step S4: Pressing the medical polymer onto the surface of the medical metal substrate to obtain an implantable medical device with high bonding strength.

6. The method for preparing an implantable medical device with high bonding strength according to claim 5, characterized in that: Step S4 specifically includes: Step S41, using a femtosecond laser to prepare hemispherical micron-shaped concave holes on the surface of a metal mold substrate; Step S42, preparing hemispherical nanopores on the inner surface of the hemispherical micron-shaped concave holes by anodizing to obtain a micro-nano structure metal mold; Step S43: Using a micro-nano structure mold to press the medical polymer onto the surface of the medical metal substrate to obtain an implantable medical device with high bonding strength.

7. Use of an implantable medical device with high bonding strength as claimed in any one of claims 1 to 4 in the preparation of an orthopedic implantable medical device.

Citation Information

Patent Citations

  • Medical titanium substrate material and manufacturing method thereof

    CN103520776A

  • Anti-inflammatory polymer material and preparation method and application thereof

    CN110540672A

  • Preparation method of composite coating for improving corrosion resistance and antibacterial property of magnesium alloy

    CN111842086A

  • Metal medical device, preparation method and implantable or interventional medical device

    CN116019983A

  • Bioimplantation metal having nano-patterning groove surface, method for preparing metal, implant, method for manufacturing implant, stent, and method for manufacturing stent

    WO2017047912A1