A high thermal conductivity polymer composite material and preparation method thereof
By introducing directional layered SiO2-BN composite materials and graphite nanosheets into polymer materials, a heat conduction channel is formed to improve thermal conductivity, which solves the problem of insufficient thermal conductivity of existing polymer materials and achieves efficient heat dissipation.
Patent Information
- Application Number
- CN202410593289.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The thermal conductivity of existing polymer materials is insufficient, making it difficult to meet the demand for efficient heat dissipation in high-tech fields such as microelectronics, motors and electrical appliances.
A highly thermally conductive polymer composite composed of directional layered SiO2-BN composite material and graphite nanosheets is used to transport heat to the heat dissipation layer through the heat conduction channel, improving the heat conduction and heat dissipation performance of the material.
It achieves efficient heat derivation, significantly improves the thermal conductivity of polymer composite materials, and is suitable for heat dissipation needs in high-tech fields.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymers, and in particular to a high thermal conductivity polymer composite material and a preparation method thereof. Background Art
[0002] With the rapid development of microelectronics integration and assembly technology, the increasing requirements for high voltage in the field of power electrical insulation, and the rapid development of other related fields, the volume of electronic components and logic circuits has shrunk by tens of millions of times, while the operating frequency has increased dramatically. At this time, the heat generated by electronic equipment has accumulated and increased rapidly, and the working environment temperature has also changed rapidly towards high temperature. In order to ensure that electronic components can work normally and reliably for a long time, it is necessary to prevent the continuous increase in working temperature. Therefore, timely heat dissipation capacity has become an important factor affecting its service life. It is urgent to develop polymer materials with high thermal conductivity. The application field of polymer materials is constantly expanding because polymer materials with different characteristics can be obtained by controlling and modifying their structure. Moreover, the unique structure and easy modification and processing characteristics of polymer insulation materials make them have excellent properties that are incomparable and irreplaceable to other materials, so they are widely used in various fields of science and technology, national defense construction and national economy, and have become indispensable materials in all aspects of food, clothing, housing and transportation in modern social life. However, general polymer materials are poor conductors of heat, and their thermal conductivity is generally lower than 0.5Wm -1 K -1 In order to meet the development needs of many manufacturing and high-tech fields such as microelectronics, electrical machinery and appliances, aerospace, and military equipment, the preparation of high thermal conductivity polymer insulation materials with excellent comprehensive performance is becoming a research hotspot in this field and is attracting more and more attention from domestic and foreign research peers. Summary of the invention
[0003] Technical problem to be solved: The purpose of the present invention is to provide a high thermal conductivity polymer composite material and a preparation method thereof, to prepare a oriented layered SiO2-BN composite material, so that the polymer material has interconnected heat conduction channels, and heat is transported to the heat dissipation layer containing graphite nanosheets through the heat conduction channels, thereby improving the thermal conductivity and heat dissipation performance of the polymer composite material.
[0004] Technical solution: A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of a oriented layered SiO2-BN composite material and ABS material, the heat dissipation layer consists of graphite nanosheets and ABS material, the thermal conductive layer has a thickness of 0.5-2mm, and the heat dissipation layer has a thickness of 50-200μm.
[0005] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0006] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material, and drying it to obtain a thermal conductive layer;
[0007] S2. The surface of the thermal conductive layer is subjected to plasma surface modification to obtain a surface-modified thermal conductive layer;
[0008] S3. Adding the graphite nanosheets to N, N-dimethylformamide and stirring to mix evenly to obtain a graphite solution;
[0009] S4. Add ABS to N,N-dimethylformamide and stir to dissolve under heating to obtain an ABS solution;
[0010] S5. The graphite solution prepared in step S3 is added to the ABS solution prepared in step S4, and after stirring, ultrasonic treatment is performed to obtain a suspension, the suspension is ball-milled to obtain a viscous slurry, and then vacuum-degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0011] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0012] Preferably, the preparation method of the oriented layered SiO2-BN composite material is:
[0013] S11. TEOS, ethanol and deionized water are mixed in a molar ratio of 1:10-14:3-5, 0.6-1.5 mol / L nitric acid solution is added dropwise to adjust the pH value to 2-3, and the mixture is stirred at a constant temperature of 45-55° C. for 45-80 min to fully hydrolyze the mixture to obtain a hydrolyzed solution;
[0014] S12. Hydroxyethyl cellulose was added to the hydrolysis solution and mixed, the concentration of hydroxyethyl cellulose in the hydrolysis solution was 4-6wt%, and stirred at a constant temperature of 40-50 ℃ for 1-2h to obtain a composite hydrolysis solution;
[0015] S13. Slowly adding 0.1 mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to about 7, to obtain a composite gel;
[0016] S14. The composite gel is added to a mold for unidirectional freeze drying at a temperature of -40 to -60°C for 20 to 40 hours to obtain a layered aerogel;
[0017] S15. Boric acid and urea are uniformly mixed in a molar ratio of 2:3 and dissolved in ethanol to prepare a solution; then the layered aerogel is immersed in the above solution at 60-70°C under vacuum conditions, and finally the aerogel is sintered in a N2 atmosphere at 850-920°C. The above steps are repeated several times to obtain a directional layered SiO2-BN composite material.
[0018] Preferably, in step S1, the drying temperature is 70-80° C. and the drying time is 2-6 hours.
[0019] Preferably, the current density of the plasma modification in step S2 is 2-5 mA / cm 2 The processing time is 2-5min, the background pressure is 50-120Pa, and the working gas is air.
[0020] Preferably, the concentration of the graphite solution in step S3 is 3.2-6wt%.
[0021] Preferably, the concentration of the ABS solution in step S4 is 15-25wt%, and the stirring temperature is 35-45°C.
[0022] Preferably, in step S5, the volume ratio of the graphite solution to the ABS solution is 1:2-3, the stirring time is 60-120 min, the ultrasonic time is 30-70 min, and the ball milling time is 60-100 min.
[0023] Beneficial effects: The high thermal conductivity polymer composite material of the present invention has the following advantages:
[0024] 1. The high thermal conductivity polymer composite material of the present invention has a directional layered structure prepared by a unidirectional freeze-drying method, and the layered structure is arranged in parallel to form a relatively regular heat conduction channel;
[0025] 2. In the present invention, a directional layered structure is first obtained by using tetraethyl orthosilicate and hydroxyethyl cellulose. The thermal conductivity of silicon dioxide is higher than that of ABS, which can improve the thermal conductivity effect to a certain extent. In order to achieve the effect of high thermal conductivity, boron nitride is generated on the surface of silicon dioxide. The thermal conductivity of boron nitride is 290Wm -1 K -1 , Boron nitride has a high thermal conductivity, which can greatly improve the thermal conductivity;
[0026] 3. In order to further improve the thermal conductivity in the present invention, a heat dissipation layer is cast outside the thermal conductive layer composed of oriented layered SiO2-BN composite material and ABS material. The heat dissipation layer contains graphite nanosheets with better thermal conductivity. Therefore, heat is output to the surface through the thermal conductive channel, absorbed by the graphite on the surface, and then dissipated to obtain a high thermal conductivity polymer composite material. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with embodiments, which are explanations of the present invention and are not limited to the following embodiments:
[0028] Example 1
[0029] The preparation method of the oriented layered SiO2-BN composite material is as follows:
[0030] S11. TEOS, ethanol and deionized water were mixed in a molar ratio of 1:10:3, 0.6 mol / L nitric acid solution was added dropwise to adjust the pH value to 2, and the mixture was stirred at a constant temperature of 55° C. for 45 min to fully hydrolyze the mixture to obtain a hydrolyzed solution;
[0031] S12. Hydroxyethyl cellulose was added to the hydrolysis solution and mixed, the concentration of hydroxyethyl cellulose in the hydrolysis solution was 4wt%, and stirred at a constant temperature of 40 ° C for 2h to obtain a composite hydrolysis solution;
[0032] S13. Slowly adding 0.1 mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to about 7, to obtain a composite gel;
[0033] S14. The composite gel was added to a mold for unidirectional freeze drying at a temperature of -40°C for 20 h to obtain a layered aerogel;
[0034] S15. Boric acid and urea are uniformly mixed in a molar ratio of 2:3 and dissolved in ethanol to prepare a solution; then the layered aerogel is immersed in the above solution at 60°C under vacuum conditions, and finally the aerogel is sintered in a N2 atmosphere at 850°C for 2 hours. The above steps are repeated twice to obtain a directional layered SiO2-BN composite material.
[0035] Example 2
[0036] The preparation method of the oriented layered SiO2-BN composite material is as follows:
[0037] S11. TEOS, ethanol and deionized water were mixed in a molar ratio of 1:14:5, 1.5 mol / L nitric acid solution was added dropwise to adjust the pH value to 3, and the mixture was stirred at a constant temperature of 55° C. for 80 min for full hydrolysis to obtain a hydrolyzed solution;
[0038] S12. Hydroxyethyl cellulose was added to the hydrolysis solution and mixed, the concentration of hydroxyethyl cellulose in the hydrolysis solution was 6wt%, and stirred at a constant temperature of 50 ° C for 1h to obtain a composite hydrolysis solution;
[0039] S13. Slowly adding 0.1 mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to about 7, to obtain a composite gel;
[0040] S14. The composite gel was added to a mold for unidirectional freeze drying at a temperature of -60°C for 40 h to obtain a layered aerogel;
[0041] S15. Boric acid and urea are uniformly mixed in a molar ratio of 2:3 and dissolved in ethanol to prepare a solution; then the layered aerogel is immersed in the above solution at 70°C under vacuum conditions, and finally the aerogel is sintered in a N2 atmosphere at 920°C for 4 hours. The above steps are repeated twice to obtain a directional layered SiO2-BN composite material.
[0042] Example 3
[0043] The preparation method of the oriented layered SiO2-BN composite material is as follows:
[0044] S11. TEOS, ethanol and deionized water were mixed in a molar ratio of 1:11:3.5, 0.9 mol / L nitric acid solution was added dropwise to adjust the pH value to 2, and the mixture was stirred at a constant temperature of 50° C. for 55 min to fully hydrolyze the mixture to obtain a hydrolyzed solution;
[0045] S12. Hydroxyethyl cellulose was added to the hydrolysis solution and mixed, the concentration of hydroxyethyl cellulose in the hydrolysis solution was 4.5wt%, and stirred at a constant temperature of 50 ° C for 1h to obtain a composite hydrolysis solution;
[0046] S13. Slowly adding 0.1 mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to about 7, to obtain a composite gel;
[0047] S14. The composite gel was added to a mold for unidirectional freeze drying at a temperature of -45°C for 35 hours to obtain a layered aerogel;
[0048] S15. Boric acid and urea are uniformly mixed in a molar ratio of 2:3 and dissolved in ethanol to prepare a solution; then the layered aerogel is immersed in the above solution at 65°C under vacuum conditions, and finally the aerogel is sintered in a N2 atmosphere at 870°C for 3 hours. The above steps are repeated once to obtain a directional layered SiO2-BN composite material.
[0049] Example 4
[0050] The preparation method of the oriented layered SiO2-BN composite material is as follows:
[0051] S11. TEOS, ethanol and deionized water were mixed in a molar ratio of 1:13:4.5, 1.2 mol / L nitric acid solution was added dropwise to adjust the pH value to 3, and the mixture was stirred at a constant temperature of 50°C for 70 min for full hydrolysis to obtain a hydrolyzed solution;
[0052] S12. Hydroxyethyl cellulose was added to the hydrolysis solution and mixed, the concentration of hydroxyethyl cellulose in the hydrolysis solution was 5.5wt%, and stirred at a constant temperature of 40 ° C for 2h to obtain a composite hydrolysis solution;
[0053] S13. Slowly adding 0.1 mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to about 7, to obtain a composite gel;
[0054] S14. The composite gel was added to a mold for unidirectional freeze drying at a temperature of -55°C for 25 h to obtain a layered aerogel;
[0055] S15. Boric acid and urea are uniformly mixed in a molar ratio of 2:3 and dissolved in ethanol to prepare a solution; then the layered aerogel is immersed in the above solution at 70°C under vacuum conditions, and finally the aerogel is sintered in a N2 atmosphere at 910°C for 3 hours. The above steps are repeated once to obtain a directional layered SiO2-BN composite material.
[0056] Example 5
[0057] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of graphite nanosheets and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0058] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0059] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 1, and drying to obtain a thermal conductive layer, wherein the drying temperature is 70° C. and the drying time is 6 h;
[0060] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 2 mA / cm 2 , the treatment time is 5min, the background pressure is 50Pa, the working gas is air, and the surface modified thermal conductive layer is obtained;
[0061] S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to mix well to obtain a graphite solution having a concentration of 3.2wt%;
[0062] S4. Add ABS to N,N-dimethylformamide, heat to 35°C, stir and dissolve, and obtain a 15wt% ABS solution; S5. Add the graphite solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the graphite solution to the ABS solution is 1:2, and stir and ultrasonicate to obtain a suspension, the stirring time is 60min, the ultrasonic time is 30min, and the ball milling time is 100min. The suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0063] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0064] Example 6
[0065] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of graphite nanosheets and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0066] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0067] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 2, and drying it to obtain a thermal conductive layer, wherein the drying temperature is 80°C and the drying time is 2h;
[0068] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 5 mA / cm 2 , the treatment time is 2min, the base pressure is 120Pa, the working gas is air, and a surface-modified thermal conductive layer is obtained;
[0069] S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to mix well to obtain a graphite solution having a concentration of 6 wt%;
[0070] S4. ABS was added to N, N-dimethylformamide and heated to 45 ° C with stirring to dissolve to obtain a concentration of 25wt% ABS solution;
[0071] S5. Add the graphite solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the graphite solution to the ABS solution is 1:3, and stir and ultrasonicate to obtain a suspension, the stirring time is 120 min, the ultrasonication time is 70 min, the ball milling time is 60 min, the suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0072] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0073] Example 7
[0074] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of graphite nanosheets and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0075] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0076] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 3, and drying it to obtain a thermal conductive layer, wherein the drying temperature is 75° C. and the drying time is 3 h;
[0077] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 3 mA / cm 2 , the treatment time is 3min, the base pressure is 100Pa, the working gas is air, and a surface-modified thermal conductive layer is obtained;
[0078] S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to mix well to obtain a graphite solution having a concentration of 4.5wt%;
[0079] S4. ABS was added to N, N-dimethylformamide and heated to 40 ° C with stirring to dissolve to obtain a concentration of 18wt% ABS solution;
[0080] S5. Add the graphite solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the graphite solution to the ABS solution is 1:2, and stir and ultrasonicate to obtain a suspension, the stirring time is 80 min, the ultrasonication time is 45 min, the ball milling time is 70 min, the suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0081] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0082] Example 8
[0083] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of graphite nanosheets and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0084] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0085] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 4, and drying it to obtain a thermal conductive layer, wherein the drying temperature is 75° C. and the drying time is 5 h;
[0086] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 4 mA / cm 2 , the treatment time is 4min, the background pressure is 70Pa, the working gas is air, and the surface modified thermal conductive layer is obtained;
[0087] S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to mix well to obtain a graphite solution having a concentration of 5.5wt%;
[0088] S4. ABS was added to N, N-dimethylformamide and heated to 45 ° C with stirring to dissolve to obtain a concentration of 22wt% ABS solution;
[0089] S5. Add the graphite solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the graphite solution to the ABS solution is 1:3, and stir and ultrasonicate to obtain a suspension, the stirring time is 100 min, the ultrasonication time is 55 min, the ball milling time is 90 min, the suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0090] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0091] Example 9
[0092] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of graphite nanosheets and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0093] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0094] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 4, and drying it to obtain a thermal conductive layer, wherein the drying temperature is 75° C. and the drying time is 4 h;
[0095] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 3.5 mA / cm 2 , the treatment time is 3min, the base pressure is 80Pa, the working gas is air, and the surface modified thermal conductive layer is obtained;
[0096] S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to obtain a graphite solution having a concentration of 5 wt%;
[0097] S4. ABS was added to N, N-dimethylformamide and heated to 45 ° C with stirring to dissolve to obtain a concentration of 20wt% ABS solution;
[0098] S5. Add the graphite solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the graphite solution to the ABS solution is 1:2, and stir and ultrasonicate to obtain a suspension, the stirring time is 90 min, the ultrasonication time is 50 min, and the ball milling time is 80 min. The suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0099] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0100] Comparative Example 1
[0101] A high thermal conductivity polymer composite material, the polymer composite material comprising a thermal conductive layer, the thermal conductive layer consisting of an oriented layered SiO2-BN composite material and an ABS material, the thermal conductive layer having a thickness of 1 mm;
[0102] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0103] After ABS was melted, it was poured into the oriented layered SiO2-BN composite material prepared in Example 3 and dried to obtain a thermal conductive layer. The drying temperature was 75° C. and the drying time was 4 h to obtain a high thermal conductive polymer composite material.
[0104] Comparative Example 2
[0105] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of oriented layered SiO2 material and ABS material, the heat dissipation layer consists of graphite nanosheets and ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0106] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0107] S1. After melting ABS, pouring it into the oriented layered SiO2 material, and drying it to obtain a thermal conductive layer, wherein the drying temperature is 80°C and the drying time is 2h;
[0108] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 5 mA / cm 2 , the treatment time is 2min, the base pressure is 120Pa, the working gas is air, and a surface-modified thermal conductive layer is obtained;
[0109] S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to mix well to obtain a graphite solution having a concentration of 6 wt%;
[0110] S4. ABS was added to N, N-dimethylformamide and heated to 45 ° C with stirring to dissolve to obtain a concentration of 25wt% ABS solution;
[0111] S5. Add the graphite solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the graphite solution to the ABS solution is 1:3, and stir and ultrasonicate to obtain a suspension, the stirring time is 120 min, the ultrasonication time is 70 min, the ball milling time is 60 min, the suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0112] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the side of the surface-modified heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material;
[0113] Wherein, the preparation method of oriented layered SiO2 material is:
[0114] S11. TEOS, ethanol and deionized water were mixed in a molar ratio of 1:10:3, 0.6 mol / L nitric acid solution was added dropwise to adjust the pH value to 2, and the mixture was stirred at a constant temperature of 55° C. for 45 min to fully hydrolyze the mixture to obtain a hydrolyzed solution;
[0115] S12. Hydroxyethyl cellulose was added to the hydrolysis solution and mixed, the concentration of hydroxyethyl cellulose in the hydrolysis solution was 4wt%, and stirred at a constant temperature of 40 ° C for 2h to obtain a composite hydrolysis solution;
[0116] S13. Slowly adding 0.1 mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to about 7, to obtain a composite gel;
[0117] S14. The composite gel is added into a mold for unidirectional freeze drying at a temperature of -40°C for 20 hours to obtain a layered aerogel. The aerogel is sintered in a N2 atmosphere at 550°C for 2 hours to obtain a directional layered SiO2 material.
[0118] Comparative Example 3
[0119] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of graphite nanosheets and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0120] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0121] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 4, and drying it to obtain a thermal conductive layer, wherein the drying temperature is 75° C. and the drying time is 5 h;
[0122] S2. The graphite nanosheets were added to N, N-dimethylformamide and stirred to obtain a graphite solution having a concentration of 5.5 wt%;
[0123] S3. ABS was added to N, N-dimethylformamide and heated to 40 ° C with stirring to dissolve to obtain a concentration of 22wt% ABS solution;
[0124] S4. Add the graphite solution prepared in step S2 to the ABS solution prepared in step S3, the volume ratio of the graphite solution to the ABS solution is 1:3, and stir and ultrasonicate to obtain a suspension, the stirring time is 100 min, the ultrasonication time is 55 min, the ball milling time is 90 min, the suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0125] S6. The heat dissipation layer polymer prepared in step S4 is tape-cast and hot-pressed on one side of the surface of the heat conductive layer prepared in step S1 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0126] Comparative Example 4
[0127] A high thermal conductivity polymer composite material, the polymer composite material consists of a thermal conductive layer and a heat dissipation layer, the thermal conductive layer consists of an oriented layered SiO2-BN composite material and an ABS material, the heat dissipation layer consists of nano BN particles and an ABS material, the thermal conductive layer has a thickness of 1 mm, and the heat dissipation layer has a thickness of 100 μm;
[0128] The method for preparing the above-mentioned high thermal conductivity polymer composite material comprises the following steps:
[0129] S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material prepared in Example 3, and drying to obtain a thermal conductive layer, wherein the drying temperature is 75° C. and the drying time is 4 h;
[0130] S2. The surface of the thermal conductive layer is subjected to plasma surface modification, and the current density of the plasma modification is 3.5 mA / cm 2 , the treatment time is 3min, the base pressure is 80Pa, the working gas is air, and the surface modified thermal conductive layer is obtained;
[0131] S3. The nano BN particles were added to N, N-dimethylformamide and stirred to mix evenly to obtain a 10wt% nano BN solution;
[0132] S4. ABS was added to N, N-dimethylformamide and heated to 40 ° C with stirring to dissolve to obtain a concentration of 20wt% ABS solution;
[0133] S5. Add the nano BN solution prepared in step S3 to the ABS solution prepared in step S4, the volume ratio of the nano BN solution to the ABS solution is 1:2, and stir and ultrasonicate to obtain a suspension, the stirring time is 90 min, the ultrasonication time is 50 min, and the ball milling time is 80 min. The suspension is ball milled to obtain a viscous slurry, and then vacuum degassing is performed at room temperature to obtain a heat dissipation layer polymer;
[0134] S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
[0135] GB 3399-1982 was used to test thermal conductivity. The test data of the embodiment and the comparative example are shown in the following table:
[0136] <![CDATA[Thermal conductivity / Wm -1 K -1 > Example 5 5.07 Example 6 5.23 Example 7 5.18 Example 8 5.09 Example 9 5.20 Comparative Example 1 4.22 Comparative Example 2 2.31 Comparative Example 3 4.85 Comparative Example 4 4.73
[0137] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A high thermal conductivity polymer composite material, characterized in that: The polymer composite material is composed of a heat-conducting layer and a heat-dissipating layer, the heat-conducting layer is composed of a directional layered SiO2-BN composite material and an ABS material, the heat-dissipating layer is composed of graphite nanosheets and an ABS material, the thickness of the heat-conducting layer is 0.5-2 mm, and the thickness of the heat-dissipating layer is 50-200 μm; Wherein, the preparation method of the oriented layered SiO2-BN composite material is: S11. TEOS, ethanol and deionized water are mixed in a molar ratio of 1:10-14:3-5, 0.6-1.5 mol / L nitric acid solution is added dropwise to adjust the pH value to 2-3, and the mixture is stirred at a constant temperature of 45-55° C. for 45-80 min to fully hydrolyze the mixture to obtain a hydrolyzed solution; S12. Add hydroxyethyl cellulose to the hydrolysis solution and mix, wherein the concentration of hydroxyethyl cellulose in the hydrolysis solution is 4-6wt%, and stir at a constant temperature of 40-50°C for 1-2h to obtain a composite hydrolysis solution; S13. Slowly adding 0. 1mol / L ammonia solution to the composite hydrolysis solution, adjusting the pH value to 7 to obtain a composite gel; S14. The composite gel is added to a mold for unidirectional freeze drying at a temperature of -40 to -60°C for 20 to 40 hours to obtain a layered aerogel; S15. Boric acid and urea are uniformly mixed in a molar ratio of 2:3 and dissolved in ethanol to prepare a solution; then the layered aerogel is immersed in the above solution at 60-70°C under vacuum conditions, and finally the aerogel is sintered in a N2 atmosphere at 850-920°C. The above steps are repeated several times to obtain a directional layered SiO2-BN composite material.
2. The method for preparing a high thermal conductive polymer composite material according to claim 1, characterized in that: The following steps are involved: S1. After melting ABS, pouring it into the oriented layered SiO2-BN composite material, and drying it to obtain a thermal conductive layer; S2. The surface of the thermal conductive layer is subjected to plasma surface modification to obtain a surface-modified thermal conductive layer; S3. The graphite nanosheets were added to N, N-dimethylformamide and stirred to mix well to obtain a graphite solution; S4. ABS was added to N, N-dimethylformamide and heated with stirring to dissolve to obtain an ABS solution; S5. The graphite solution prepared in step S3 is added to the ABS solution prepared in step S4, and after stirring, ultrasonically obtained a suspension, the suspension is ball-milled to obtain a slurry having a viscosity, and then vacuum-degassed at room temperature to obtain a heat dissipation layer polymer; S6. The heat dissipation layer polymer prepared in step S5 is tape-cast and hot-pressed on the surface-modified side of the heat conductive layer prepared in step S2 to obtain a heat dissipation layer, and then vacuum-dried to obtain a high thermal conductive polymer composite material.
3. The method for preparing a high thermal conductivity polymer composite material according to claim 2, characterized in that: In step S1, the drying temperature is 70-80° C. and the drying time is 2-6 hours.
4. The method for preparing a high thermal conductive polymer composite material according to claim 2, characterized in that: The current density of the plasma modification in step S2 is 2-5 mA / cm 2 The processing time is 2-5min, the background pressure is 50-120Pa, and the working gas is air.
5. The method for preparing a high thermal conductive polymer composite material according to claim 2, characterized in that: The concentration of the graphite solution in step S3 is 3.2-6wt%.
6. The method for preparing a high thermal conductive polymer composite material according to claim 2, characterized in that: The concentration of the ABS solution in step S4 is 15-25wt%, and the stirring temperature is 35-45°C.
7. The method for preparing a high thermal conductive polymer composite material according to claim 2, characterized in that: In the step S5, the volume ratio of the graphite solution to the ABS solution is 1:2-3, the stirring time is 60-120 min, the ultrasonic time is 30-70 min, and the ball milling time is 60-100 min.