A kind of iron phosphate material and its preparation method and application

By controlling the particle structure and hardness index of iron phosphate materials, the problems of low grinding efficiency and poor electrochemical performance of lithium iron phosphate materials are solved, and the efficient preparation of positive electrode materials with good electrochemical performance is achieved.

CN118545688BActive Publication Date: 2024-11-12GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410994099.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

During the grinding process, the existing lithium iron phosphate materials have large wear and low efficiency due to the high hardness of anhydrous iron phosphate, making it difficult to prepare a positive electrode material with good electrochemical properties.

Method used

By controlling the equivalent particle size of the primary particles of iron phosphate material to be 20nm~600nm, the D50 of the secondary particles is 5μm~20μm, and the hardness index is ≤5, the micro bubble generator and surfactant in the synthesis reaction are regulated to form Loose structure of iron phosphate material to improve grinding efficiency with lithium source.

Benefits of technology

It realizes reducing machine wear and improving the electrochemical performance of the positive electrode material, and is suitable for the preparation of high-efficiency batteries and electrical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118545688B_ABST
    Figure CN118545688B_ABST
Patent Text Reader

Abstract

The present invention discloses an iron phosphate material and a preparation method and application thereof, belonging to the technical field of battery materials. The iron phosphate material is a secondary particle formed by agglomeration of primary particles, the equivalent particle size of the primary particles is 20nm~600nm, and the D 50 5μm~20μm; the hardness index of the iron phosphate material is ≤5; hardness index = #imgabs0#, #imgabs1# is the average major-minor axis ratio of the primary particles, and the average major-minor axis ratio refers to the ratio of the average length of the longest axis to the average length of the shortest axis of the primary particles; #imgabs2# is the specific pore volume of the iron phosphate material, in cm 3 / g. The iron phosphate material meeting the above characteristics has a loose structure and a low overall hardness. When used to prepare positive electrode materials, it can improve the efficiency of grinding with lithium sources, cause less wear on the machine, and the prepared positive electrode material has good electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to an iron phosphate material and a preparation method and application thereof. Background Art

[0002] Lithium iron phosphate is one of the most competitive cathode active materials for lithium-ion batteries on the market. Compared with lithium cobalt oxide and ternary cathode materials, lithium iron phosphate has the advantages of long life and good safety performance. In addition, lithium iron phosphate also has considerable energy density.

[0003] At present, lithium iron phosphate is mostly prepared by solid phase method, which is specifically made by sintering anhydrous iron phosphate and lithium salt. Anhydrous iron phosphate needs to be ground before sintering, but because anhydrous iron phosphate is in a crystalline state and has a strong lattice strength, the macroscopic hardness of the material is relatively large, which makes the anhydrous iron phosphate cause greater wear on the machine during the grinding process and the grinding efficiency is low.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide an iron phosphate material and a preparation method and application thereof, so as to solve or improve the above-mentioned technical problems.

[0006] The present invention can be implemented like this:

[0007] In a first aspect, the present invention provides an iron phosphate material, which is a secondary particle formed by agglomeration of primary particles, wherein the equivalent particle size of the primary particles is 20 nm to 600 nm, and the equivalent particle size is the diameter of a standard sphere having the same volume as the primary particles; the D 50 5μm~20μm;

[0008] The hardness index of the iron phosphate material is ≤5; hardness index = ,in, The average length-to-short axis ratio of the primary particles refers to the ratio of the average length of the longest axis to the average length of the shortest axis of the primary particles; is the specific pore volume of the iron phosphate material, in cm 3 / g.

[0009] In an alternative embodiment, The results were obtained by scanning electron microscopy (SEM) test and calculation.

[0010] It was calculated from the nitrogen adsorption-desorption isotherm.

[0011] In an optional embodiment, the iron phosphate material further has at least one of the following characteristics:

[0012] Feature 1: The iron phosphate material is anhydrous iron phosphate material;

[0013] Feature 2: Iron phosphate material 0.3cm 3 / g~1.3cm 3 / g, preferably 0.72cm 3 / g~1.28cm 3 / g;

[0014] Feature 3: The average major-minor axis ratio of the primary particles does not exceed 3.5, preferably 1.11 to 3.14;

[0015] Feature 4: The hardness index of the iron phosphate material is 0.98~3.57;

[0016] Feature 5: The equivalent particle size of primary particles is 254nm~411nm;

[0017] Feature 6: D of secondary particles 50 It is 8.74μm~10.28μm.

[0018] In a second aspect, the present invention provides a method for preparing an iron phosphate material as described in the aforementioned embodiment, comprising the following steps: mixing an iron source solution with a phosphorus source solution, an oxidant, and a pH adjuster and conducting a synthesis reaction, collecting an amorphous iron phosphate precipitate obtained by the reaction; aging and crystallizing the amorphous iron phosphate precipitate to obtain dihydrate iron phosphate crystals; and calcining the dihydrate iron phosphate crystals to obtain an anhydrous iron phosphate material.

[0019] In an optional embodiment, the synthesis reaction includes at least one of the following features:

[0020] Feature 7: The iron source solution is a soluble ferrous salt solution; preferably, the iron source includes at least one of ferrous sulfate, ferrous chloride, ferrous nitrate, ferrous oxalate and ferrous acetate;

[0021] Feature 8: The oxidant includes at least one of hydrogen peroxide, ozone, sodium persulfate, ammonium persulfate, sodium hypochlorite, sodium ferrate, oxygen and air; preferably, the oxidant includes hydrogen peroxide and air;

[0022] Feature 9: The phosphorus source includes at least one of phosphoric acid, sodium dihydrogen phosphate, sodium monohydrogen phosphate, ammonium dihydrogen phosphate and ammonium monohydrogen phosphate;

[0023] Feature 10: The pH adjuster includes at least one of ammonia water, sodium hydroxide, sulfuric acid, hydrochloric acid and nitric acid;

[0024] Feature 11: The concentration of the iron source solution is 0.8 mol / L~1.5 mol / L;

[0025] Feature 12: The concentration of the phosphorus source solution is 0.85 mol / L~3 mol / L;

[0026] Feature 13: The iron source and the phosphorus source are added in a ratio of the amount of P to the amount of Fe of 1.05:1 to 1.5:1;

[0027] Feature 14: The amount of oxidant used is not less than the theoretical amount of Fe in the iron source. 2+ All oxidized to Fe 3+ The amount of

[0028] Feature 15: The pH value of the synthesis reaction is 1~2.5;

[0029] Feature 16: The temperature of the synthesis reaction is 50°C~70°C;

[0030] Feature 17: The synthesis reaction time is 1h~4h;

[0031] Feature 18: The stirring speed of the synthesis reaction is 400 rpm to 800 rpm.

[0032] In an optional embodiment, when the oxidant includes both gaseous oxidants and liquid oxidants, a mixed solution consisting of an iron source solution and a phosphorus source solution is reacted with the gaseous oxidants through a microbubble generator and then mixed with the liquid oxidants and a pH regulator.

[0033] In an optional embodiment, the bubble particle size generated by the micro-nano bubble generator is 200 nm to 4.0 μm.

[0034] In an optional embodiment, the bubble content of the micro-nano bubble generator is 10% to 30% by volume.

[0035] In an optional embodiment, the aging and crystallization comprises: dispersing the amorphous iron phosphate precipitate in an aging solution to perform a crystallization reaction;

[0036] Wherein, the aging solution is a phosphoric acid solution containing a surfactant.

[0037] In an optional embodiment, the crystal transformation reaction includes at least one of the following features:

[0038] Feature 19: The pH value of the aging solution is 1 to 2.5;

[0039] Feature 20: The concentration of the surfactant contained in the aging solution is 1wt%~5wt%;

[0040] Feature 21: The feed ratio of amorphous iron phosphate precipitate to aged solution is 1 g:100 mL to 1 g:300 mL;

[0041] Feature 22: The surfactant includes at least one of lignin sulfonate and naphthalene sulfonate formaldehyde condensate; wherein the lignin sulfonate includes at least one of sodium lignin sulfonate and ammonium lignin sulfonate; and the naphthalene sulfonate formaldehyde condensate includes at least one of β-naphthalene sulfonate sodium formaldehyde condensate, benzyl naphthalene sulfonate sodium formaldehyde condensate, α-methyl naphthalene sulfonate sodium formaldehyde condensate and alkyl benzene sulfonate sodium formaldehyde condensate;

[0042] Feature 23: The temperature of the crystallization reaction is 80℃~90℃;

[0043] Feature 24: The crystal transformation reaction time is 1h~3h;

[0044] Feature 25: The stirring rate of the crystallization reaction is 100 rpm~300 rpm.

[0045] In an alternative embodiment, calcination includes at least one of the following features:

[0046] Feature 26: The calcination temperature is 600°C to 750°C;

[0047] Feature 27: Calcination time is 2h~3h;

[0048] Feature 28: The heating rate during the calcination process is 3℃ / min~5℃ / min.

[0049] In a third aspect, the present invention provides a positive electrode material, which is prepared by mixing and sintering the above-mentioned iron phosphate material with a lithium source and a carbon source.

[0050] In an optional embodiment, the positive electrode material has at least one of the following characteristics:

[0051] Feature 29: D of positive electrode material 50 0.87μm~1.17μm;

[0052] Feature 30: The specific surface area of ​​the positive electrode material is 12.13 cm 2 / g~12.85cm 2 / g;

[0053] Feature 31: The 0.1C charge capacity of the positive electrode material is not less than 161.5 mAh / g, preferably 161.7 mAh / g to 163.5 mAh / g;

[0054] Feature 32: The 0.1C discharge specific capacity of the positive electrode material is not less than 158.5 mAh / g, preferably 158.8 mAh / g to 161.6 mAh / g;

[0055] Feature 33: The 1C discharge specific capacity of the positive electrode material is not less than 143.0 mAh / g, preferably 143.3 mAh / g~149.0 mAh / g.

[0056] In a fourth aspect, the present invention provides a positive electrode plate, wherein the active material in the positive electrode plate includes the positive electrode material of the aforementioned embodiment.

[0057] In a fifth aspect, the present invention provides a battery comprising the positive electrode sheet of the aforementioned embodiment.

[0058] The beneficial effects of the present invention include:

[0059] The present invention is to adjust the primary particle equivalent particle size and secondary particle D 50 And the hardness index of the iron phosphate material is limited to a specific range, so that the iron phosphate material meeting the above characteristics has a loose structure and a lower overall hardness. When used to prepare positive electrode materials, it can improve the efficiency of grinding with the lithium source and cause less wear on the machine. The prepared positive electrode material has good electrochemical properties, which is conducive to the further preparation of batteries and electrical devices with excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0061] Figure 1 This is a SEM image of the anhydrous ferric phosphate prepared in Example 1;

[0062] Figure 2 This is a SEM image of anhydrous ferric phosphate prepared in Comparative Example 1;

[0063] Figure 3 This is a SEM image of anhydrous ferric phosphate prepared in Comparative Example 2;

[0064] Figure 4 This is a SEM image of anhydrous ferric phosphate prepared in Comparative Example 3;

[0065] Figure 5 This is a SEM image of anhydrous ferric phosphate prepared in Comparative Example 4;

[0066] Figure 6 The XRD diagrams of the anhydrous ferric phosphate prepared in Example 1 and Comparative Examples 1-4 are shown. DETAILED DESCRIPTION

[0067] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0068] The iron phosphate material provided by the present invention and its preparation method and application are described in detail below.

[0069] The present invention provides an iron phosphate material, the general formula of which is FePO4.

[0070] The iron phosphate material is a secondary particle formed by agglomeration of primary particles. The equivalent particle size of the primary particles is 20nm~600nm, and the equivalent particle size is the diameter of a standard sphere with the same volume as the primary particles. 50 5μm~20μm;

[0071] The hardness index of the iron phosphate material is ≤5; hardness index = ,in, The average length-to-short axis ratio of primary particles is the ratio of the average length of the longest axis to the average length of the shortest axis of primary particles. is the specific pore volume of the iron phosphate material, in cm 3 / g.

[0072] The equivalent diameter of the primary particles can be measured and calculated by scanning electron microscopy (SEM). Specifically, the volume V is calculated by measuring the morphological parameters of the primary particles in the SEM test image of the iron phosphate material, and then the volume V is calculated according to the volume formula of the standard sphere V=4 / 3. (d / 2) 3 , calculate the equivalent particle size d.

[0073] Among them, D 50 It refers to the size of secondary particles corresponding to 50% of the cumulative distribution.

[0074] in, It refers to the ratio of the average length of the longest axis of the primary particles to the average length of the shortest axis. The average length of the longest axis refers to the sum of the lengths of the longest axes of the primary particles divided by the number of primary particles; the average length of the shortest axis refers to the sum of the lengths of the shortest axes of the primary particles divided by the number of primary particles. It can be tested and calculated by scanning electron microscope (SEM).

[0075] Among them, the hardness index does not consider the dimension and the value is ≤5.

[0076] in, It can be understood as the pore volume per unit mass, in cm 3 / g. It can be calculated through the nitrogen adsorption-desorption isotherm curve.

[0077] The iron phosphate material of the present invention is anhydrous iron phosphate after calcination and drying. Since the chemical composition is fixed and the surface properties of the crystalline anhydrous iron phosphate after calcination and drying are almost the same, the difficulty of grinding the iron phosphate material is related to the properties of its primary particles and secondary particles formed by agglomeration of the primary particles.

[0078] As for the effect of the primary particle size on the grinding difficulty: on the one hand, the smaller the primary particle size, the larger the specific surface area of ​​the material, the higher the specific surface energy of the material, the easier it is to agglomerate, which is not conducive to crushing; on the other hand, if the primary particles are too large, it is not conducive to the preparation of positive electrode materials with a large specific surface area, and it is also difficult to grind oversized iron phosphate particles into small particles. Therefore, the particle size of the primary particles needs to be controlled within an appropriate range.

[0079] As for the influence of the morphology of primary particles on the difficulty of grinding: the more spherical the primary particles are, the smaller their specific surface area, the lower their surface energy, and the lower their tendency to agglomerate; in addition, the more spherical the primary particles are, the smaller the contact area between the particles, and the easier it is to break.

[0080] As for the effect of the pore structure of secondary particles on the difficulty of grinding: the larger the volume of the pores of the secondary particles, the looser the material, and the easier it is to crush.

[0081] Although the size and morphology of primary particles will affect the specific pore volume of the material, the specific pore volume of the material is also affected by the width of the primary particle size distribution and the preparation method. Specifically, the wider the particle size distribution, the easier it is for the material to be combined more tightly according to the stacking principle (small particles fill the pores formed by large particles); the preparation method affects the intensity and probability of collisions between particles. For example, increased temperature and increased stirring speed intensify the collisions between particles, thereby improving the agglomeration and contact tightness of primary particles.

[0082] That is, the specific pore volume, specific surface area or porosity of the material cannot comprehensively evaluate the difficulty of grinding the material. For example, porosity is the ratio of pore volume to material volume, and specific pore volume is the ratio of pore volume to material mass, and the two are similar. On the one hand, the mass of the material is more accurately measured than the volume of the material. The prior art generally calculates the porosity by the pore area in the SEM of the material section to the solid area; on the other hand, to take an extreme case, spherical primary particles (which can be regarded as single crystals) and disc-shaped primary particles (which can be regarded as single crystals) of the same mass (or volume) are used as shell materials to assemble a hollow material with the same cavity area, that is, the surface area of ​​the spherical cavity is fixed. Since the total surface area of ​​the disc-shaped particles is larger than the total surface area of ​​the spherical particles, the disc-shaped particles overlap with each other more, and are therefore more difficult to crush. In addition, the specific surface area of ​​secondary particles, that is, the sum of the surface areas per unit mass of materials, such as iron phosphate materials with equal mass (or volume), disc-shaped particles have a larger specific surface area than spherical particles, but disc-shaped particles are more difficult to crush.

[0083] The present invention creatively proposes to use the equivalent particle size of primary particles and the D 50 The hardness index of the iron phosphate material is combined to characterize the difficulty of grinding the material, and the characterization result is consistent with the actual grinding difficulty of the material.

[0084] Specifically, by controlling the equivalent particle size of the primary particles of the iron phosphate material to 20nm~600nm and the D 50 The particle size is controlled to be 5μm~20μm and the hardness index of the iron phosphate material is controlled to be ≤5, so that the iron phosphate material meeting the above characteristics has a loose structure and a lower overall hardness. When used to prepare positive electrode materials, the efficiency of grinding with the lithium source can be improved, and the wear on the machine is small. The prepared positive electrode material has good electrochemical properties, which is conducive to the further preparation of batteries and electrical devices with excellent electrochemical properties.

[0085] In some optional embodiments, the iron phosphate material 0.3cm 3 / g~1.3cm 3 / g, for example, 0.72 cm 3 / g~1.28cm 3 / g, such as 0.72cm 3 / g, 0.84cm 3 / g, 0.88cm 3 / g, 0.91cm 3 / g, 1.05cm 3 / g, 1.19cm 3 / g or 1.28cm 3 / g, etc., can also be 0.72cm3 / g~1.28cm 3 / Other values ​​within the range of g.

[0086] In some optional embodiments, the average aspect ratio of the primary particles of the ferric phosphate material does not exceed 3.5, for example, it can be 1.11 to 3.14, such as 1.11, 1.25, 1.28, 1.31, 1.33, 2.34 or 3.14, or other values ​​within the range of 1.11 to 3.14. The average aspect ratio of the primary particles can reflect their morphology. The closer the average aspect ratio is to 1, the more the primary particles are similar to a standard sphere; the larger the average aspect ratio is, the more the primary particles are similar to a flake.

[0087] In some optional embodiments, the hardness index of the ferrous phosphate material may have a value of 0.98 to 3.57, such as 0.98, 1.08, 1.22, 1.27, 1.82, 2.79 or 3.57, or other values ​​within the range of 0.98 to 3.57.

[0088] In some optional embodiments, the equivalent particle size of the primary particles of the iron phosphate material can be 254nm~411nm, such as 254nm, 327nm, 372nm, 395nm, 396nm, 405nm or 411nm, or other values ​​within the range of 254nm~411nm.

[0089] In some optional embodiments, the D of the secondary particles 50 It can be 8.74 μm to 10.28 μm, such as 8.74 μm, 9.84 μm, 10.06 μm, 10.11 μm, 10.12 μm, 10.28 μm or 11.2 μm, or other values ​​within the range of 8.74 μm to 10.28 μm.

[0090] As mentioned above, the iron phosphate material provided by the present invention is a secondary particle formed by agglomeration of primary particles. The primary particles are approximately spherical and have uniform particle size distribution. The secondary particles obtained by agglomeration have a relatively loose structure, high crystallinity, and low overall hardness. They are suitable for mixing and grinding with raw materials such as lithium sources to prepare positive electrode materials such as lithium iron phosphate.

[0091] Accordingly, the present invention also provides a method for preparing the above-mentioned iron phosphate material, comprising the following steps: mixing an iron source solution with a phosphorus source solution, an oxidant and a pH regulator and performing a synthesis reaction, collecting an amorphous iron phosphate precipitate obtained by the reaction; aging and crystallizing the amorphous iron phosphate precipitate to obtain dihydrate iron phosphate crystals; calcining the dihydrate iron phosphate crystals to obtain anhydrous iron phosphate material;

[0092] In some optional embodiments, the iron source solution is a soluble ferrous salt solution, wherein the iron source may illustratively but not limitatively include at least one of ferrous sulfate, ferrous chloride, ferrous nitrate, ferrous oxalate and ferrous acetate.

[0093] In some optional embodiments, the concentration of the iron source solution can be 0.8mol / L~1.5mol / L, such as 0.8mol / L, 0.9mol / L, 1.0mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L or 1.5mol / L, etc., or it can be other values ​​within the range of 0.8mol / L~1.5mol / L.

[0094] The oxidant may illustratively but not limitatively include at least one of hydrogen peroxide, ozone, sodium persulfate, ammonium persulfate, sodium hypochlorite, sodium ferrate, oxygen and air.

[0095] The amount of oxidant used should not be less than the theoretical amount of Fe in the iron source. 2+ All oxidized to Fe 3+ The amount.

[0096] In some embodiments, the oxidant includes both gaseous oxidants and liquid oxidants, for example, the oxidant contains both hydrogen peroxide and air. In this manner, the mixed solution consisting of the iron source solution and the phosphorus source solution can be mixed with hydrogen peroxide and a pH regulator after being acted on by a microbubble generator and air, which is beneficial to greatly increase the contact area and time between the air and the liquid phase and improve the oxidation efficiency. In this manner, the gas-liquid interface of the bubble has a higher surface energy, which is more conducive to adsorption on the surface of the agglomerate, making the agglomerate more loose.

[0097] For example, the bubble particle size generated by the micro-nano bubble generator may be 200 nm to 4.0 μm. In terms of volume percentage, the bubble content generated by the micro-nano bubble generator may be 10% to 30%, such as 10%, 15%, 20%, 25% or 30%.

[0098] The phosphorus source may illustratively but not limitatively include at least one of phosphoric acid, sodium dihydrogen phosphate, sodium monohydrogen phosphate, ammonium dihydrogen phosphate, and ammonium monohydrogen phosphate.

[0099] The concentration of the phosphorus source solution can be 0.85mol / L~3mol / L, such as 0.85mol / L, 1mol / L, 1.5mol / L, 2mol / L, 2.5mol / L or 3mol / L, etc., or other values ​​within the range of 0.85mol / L~3mol / L.

[0100] The iron source and the phosphorus source can be added in a ratio of the amount of P to the amount of Fe of 1.05:1 to 1.5:1 (such as 1.05:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1, 1.35:1, 1.4:1, 1.45:1 or 1.5:1, etc.).

[0101] The pH adjuster may illustratively but not limitatively include at least one of aqueous ammonia, sodium hydroxide, sulfuric acid, hydrochloric acid, and nitric acid.

[0102] In the present invention, the mixing order and mixing method of the raw materials are not particularly limited, and the mixing method includes but is not limited to titration mixing, one-pot mixing or parallel flow mixing.

[0103] In some embodiments, the iron source solution is first mixed with the phosphorus source solution to obtain a mixed solution; the mixed solution, the oxidant and the pH regulator are then added to the reaction vessel in parallel using a constant flow pump. The pH regulator is used to control the pH value of the synthesis reaction.

[0104] In some embodiments, the pH value of the synthesis reaction is 1-2.5, such as 1, 1.5, 2 or 2.5, etc., and can also be other values ​​within the range of 1-2.5.

[0105] The temperature of the synthesis reaction can be 50°C to 70°C, such as 50°C, 55°C, 60°C, 65°C or 70°C, etc., or other values ​​within the range of 50°C to 70°C.

[0106] The above-mentioned synthesis reaction temperature is relatively low, which is conducive to the formation of loosely structured agglomerates.

[0107] The time of the synthesis reaction can be 1 h to 4 h, such as 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h or 4 h, etc., or other values ​​within the range of 1 h to 4 h.

[0108] The stirring speed of the synthesis reaction may be 400 rpm to 800 rpm, such as 400 rpm, 500 rpm, 600 rpm, 700 rpm or 800 rpm, or other values ​​within the range of 400 rpm to 800 rpm.

[0109] The above-mentioned faster stirring speed is conducive to making the agglomerate structure more loose and the particle size smaller, which is further conducive to improving the crystallization efficiency in the crystallization stage, obtaining grains with relatively uniform particle size and higher crystallinity, and reducing the agglomeration of primary particles.

[0110] In some embodiments, the aging and crystallization comprises: dispersing amorphous iron phosphate precipitate in an aging solution to perform a crystallization reaction;

[0111] Wherein, the aging solution is a phosphoric acid solution containing a surfactant.

[0112] The feed ratio of the amorphous ferric phosphate precipitate to the aged solution can be 1g:100mL to 1g:300mL, such as 1g:100mL, 1g:150mL, 1g:200mL, 1g:250mL or 1g:300mL, etc., or other values ​​within the range of 1g:100mL to 1g:300mL. The amorphous ferric phosphate precipitate has a solid content of 80wt% to 90wt% based on wet material.

[0113] The pH value of the aging solution may be 1 to 2.5, such as 1, 1.5, 2 or 2.5, or other values ​​within the range of 1 to 2.5.

[0114] The concentration of the surfactant contained in the aging solution may be 1 wt% to 5 wt%, such as 1 wt%, 2 wt%, 3 wt%, 4 wt% or 5 wt%, etc., or may be other values ​​within the range of 1 wt% to 5 wt%.

[0115] As an example, the surfactant may include at least one of lignin sulfonate and naphthalene sulfonate formaldehyde condensate. Among them, lignin sulfonate may exemplarily but not limitatively include at least one of sodium lignin sulfonate and ammonium lignin sulfonate. Naphthalene sulfonate formaldehyde condensate may exemplarily but not limitatively include at least one of β-naphthalene sulfonate sodium formaldehyde condensate, benzyl naphthalene sulfonate sodium formaldehyde condensate, α-methyl naphthalene sulfonate sodium formaldehyde condensate and alkyl benzene sulfonate sodium formaldehyde condensate.

[0116] By adding anionic polymer surfactants during the crystallization stage, anions are adsorbed on the surface of positively charged iron phosphate particles. The electrostatic effect and steric effect inhibit the agglomeration between particles and induce the primary particles to be spherical crystals, which is beneficial for making the structure of the secondary particles looser. In addition, since the surfactant contains a large amount of rigid benzene ring structure, it can act as a pore-forming agent during calcination to increase the looseness of the iron phosphate material.

[0117] In some embodiments, the temperature of the crystallization reaction may be 80°C to 90°C, such as 80°C, 85°C or 90°C, or other values ​​within the range of 80°C to 90°C.

[0118] The time of the crystal transformation reaction can be 1 h to 3 h, such as 1 h, 1.5 h, 2 h, 2.5 h or 3 h, or other values ​​within the range of 1 h to 3 h.

[0119] The stirring rate of the crystallization reaction can be 100 rpm to 300 rpm, such as 100 rpm, 150 rpm, 200 rpm, 250 rpm or 300 rpm, or other values ​​within the range of 100 rpm to 300 rpm.

[0120] The stirring speed of the aging and crystallization reaction is controlled at a low level to avoid violent collisions between particles and aggravate agglomeration.

[0121] After the crystallization reaction is completed, the product is filtered and washed, and the filter residue is dried.

[0122] The drying may be performed by normal pressure oven drying, vacuum oven drying or spray drying, etc. In some embodiments, spray drying is used to dry the powder, which is beneficial to reduce the degree of agglomeration of the powder.

[0123] In some embodiments, the calcination temperature may be 600°C to 750°C, such as 600°C, 650°C, 700°C or 750°C, or other values ​​within the range of 600°C to 750°C.

[0124] The calcination time can be 2 h to 3 h, such as 2 h, 2.5 h or 3 h, or other values ​​within the range of 2 h to 3 h.

[0125] The heating rate during the calcination process can be 3°C / min~5°C / min, such as 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min or 5°C / min, or other values ​​within the range of 3°C / min~5°C / min.

[0126] In the above, the present invention uses ferrous salt as an iron source and adopts an oxidation precipitation crystallization method to prepare an iron phosphate material. In the preparation process, a variety of means are used to control the morphology, particle size and distribution of the primary particles of the iron phosphate material and the agglomeration structure of the secondary particles, so that the primary particles are approximately spherical, the particle size range is 20nm~600nm and the distribution is relatively uniform, and the secondary particles are loose in structure and D 50 The hardness index of iron phosphate material is ≤5.

[0127] In addition, the present invention also provides a positive electrode material, which is prepared by mixing and sintering the above-mentioned iron phosphate material with a lithium source and a carbon source.

[0128] The lithium source may exemplarily but not limitatively include lithium carbonate and the like, and the carbon source may exemplarily but not limitatively include glucose and the like.

[0129] In some of the enumerated embodiments, the positive electrode material can be prepared according to the following method: the iron phosphate material is mixed with lithium carbonate and glucose in a molar ratio of n (iron element in the iron phosphate material): n (Li): n (glucose) = 1: 1.04: 0.05 to obtain a mixed raw material; the mixed raw material is mixed with ethanol and ground in a grinder for 6 hours to obtain a slurry; the slurry is dried in a vacuum oven at 80°C for 4 hours to obtain a dry material; the dry material is calcined at 750°C under a nitrogen atmosphere for 9 hours, and after screening, a lithium iron phosphate positive electrode material can be obtained.

[0130] In some embodiments, the D of the positive electrode material 50 It is 0.87μm~1.17μm, such as 0.87μm, 0.95μm, 1.05μm, 1.11μm, 1.12μm, 1.14μm or 1.17μm, etc., and can also be other values ​​within the range of 0.87μm~1.17μm.

[0131] In some embodiments, the specific surface area of ​​the positive electrode material is 12.13 cm 2 / g~12.85cm 2 / g, such as 12.13cm 2 / g, 12.21cm 2 / g, 12.28cm 2 / g, 12.47cm 2 / g, 12.67cm 2 / g, 12.85cm 2 / g or 13.24cm 2 / g, etc., can also be 12.13cm 2 / g~12.85cm 2 / Other values ​​within the range of g.

[0132] In some embodiments, the 0.1C charging specific capacity of the positive electrode material is not less than 161.5 mAh / g, for example, it can be 161.7 mAh / g to 163.5 mAh / g, such as 161.7 mAh / g, 162.2 mAh / g, 162.7 mAh / g, 162.8 mAh / g, 163.2 mAh / g or 163.5 mAh / g, etc., or it can be other values ​​within the range of 161.7 mAh / g to 163.5 mAh / g.

[0133] In some embodiments, the 0.1C discharge specific capacity of the positive electrode material is not less than 158.5 mAh / g, for example, it can be 158.8 mAh / g to 161.6 mAh / g, such as 158.8 mAh / g, 159.0 mAh / g, 159.4 mAh / g, 161.3 mAh / g, 161.5 mAh / g or 161.6 mAh / g, etc., or it can be other values ​​within the range of 158.8 mAh / g to 161.6 mAh / g.

[0134] In some embodiments, the 1C discharge specific capacity of the positive electrode material is not less than 143.0 mAh / g, for example, it can be 143.3 mAh / g to 149.0 mAh / g, such as 143.3 mAh / g, 144.1 mAh / g, 144.8 mAh / g, 147.3 mAh / g, 148.1 mAh / g, 148.8 mAh / g or 149.0 mAh / g, etc., or it can be other values ​​within the range of 143.3 mAh / g to 149.0 mAh / g.

[0135] In addition, the present invention also provides a positive electrode plate, in which the active material includes the above-mentioned positive electrode material.

[0136] The present invention also provides a battery cell, which includes the above-mentioned positive electrode plate.

[0137] For example, the battery cells may be used in, but are not limited to, electrical devices such as vehicles, ships or aircraft.

[0138] The present invention also provides a battery comprising the battery monomer.

[0139] The present invention also provides an electric device, which includes the above-mentioned battery cell and / or battery. As an example, the electric device can be, but not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy can include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft can include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0140] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0141] Example 1

[0142] This embodiment provides an anhydrous ferric phosphate, the preparation method of which includes:

[0143] Step (1): preparing a mixed solution according to the feed ratio of iron source to phosphorus source of n(P):n(Fe) of 1.3:1, wherein the iron source is an aqueous solution of ferrous sulfate heptahydrate with a ferrous ion concentration of 1.5 mol / L, and the phosphorus source is a phosphoric acid solution with a phosphate ion concentration of 1.92 mol / L.

[0144] Step (2): The mixed solution, 0.6 mol / L hydrogen peroxide and 2 mol / L ammonia water are added to the reactor in parallel by a constant flow pump. The flow rates of the mixed solution and hydrogen peroxide are both 120 mL / h. The flow rate of ammonia water is controlled to maintain the pH of the reaction solution at 1.2±0.1. The temperature is controlled to maintain at 60°C during the reaction. The reaction time is 2 hours and the stirring speed is 600 rpm. After the reaction is completed, the mixture is filtered and washed with deionized water to obtain an amorphous iron phosphate precipitate (wet material, solid content of 87.6 wt%).

[0145] The mixed solution is reacted with air by a micro-bubble generator and then enters the reactor. The bubble particle size generated by the micro-nano bubble generator is 200nm-4.0μm, and the bubble content is 20vt%.

[0146] Step (3): uniformly dispersing the amorphous iron phosphate precipitate in the aging solution to carry out an aging and crystallization reaction. After the reaction is completed, filtering and washing with deionized water are performed. The filter residue is spray-dried to obtain dihydrate iron phosphate crystals.

[0147] The aging solution is a phosphoric acid solution containing ammonium lignin sulfonate, the pH value of the aging solution is 2, and the concentration of ammonium lignin sulfonate in the aging solution is 2.5wt%. The feeding ratio of amorphous iron phosphate precipitate to aging solution is 1g:200mL. The aging crystallization reaction temperature is 90°C, the time is 2h, and the stirring rate is 200rpm.

[0148] Step (4): calcining the dihydrate ferric phosphate crystals to obtain anhydrous ferric phosphate.

[0149] The calcination temperature was 700°C, the heating rate was 4°C / min, and the calcination time was 2h.

[0150] Example 2

[0151] The difference between this embodiment and embodiment 1 is that the concentration of ammonium lignin sulfonate in the aging solution is 1 wt %.

[0152] Example 3

[0153] The difference between this embodiment and embodiment 1 is that the concentration of ammonium lignin sulfonate in the aging solution is 5 wt %.

[0154] Example 4

[0155] The difference between this embodiment and embodiment 1 is that the bubble particle size generated by the micro-nano bubble generator is 200nm-4.0μm, and the bubble content is 10vt%.

[0156] Example 5

[0157] The difference between this embodiment and embodiment 1 is that the bubble particle size generated by the micro-nano bubble generator is 200nm-4.0μm, and the bubble content is 30vt%.

[0158] Example 6

[0159] This embodiment provides an anhydrous ferric phosphate, the preparation method of which includes:

[0160] Step (1): preparing a mixed solution according to the feed ratio of iron source to phosphorus source of n(P):n(Fe)=1.05:1, wherein the iron source is an aqueous solution of ferrous chloride with a ferrous ion concentration of 0.8 mol / L, and the phosphorus source is a sodium dihydrogen phosphate solution with a phosphate ion concentration of 0.85 mol / L.

[0161] Step (2): The mixed solution, sodium hypochlorite with a concentration of 1 mol / L, and sodium hydroxide solution with a concentration of 1 mol / L are added to the reactor in parallel by a constant flow pump, the flow rate of the mixed solution and sodium hypochlorite is 200 mL / h, the flow rate of the sodium hydroxide solution is controlled to maintain the pH of the reaction solution at 1.1±0.1, and the temperature is controlled to maintain at 70°C during the reaction, the reaction time is 1 hour, and the stirring speed is 400 rpm. After the reaction is completed, the mixture is filtered and washed with deionized water to obtain an amorphous iron phosphate precipitate (wet material, solid content of 88.1 wt%).

[0162] The mixed solution is reacted with air by a micro-bubble generator and then enters the reactor. The bubble particle size generated by the micro-nano bubble generator is 200nm-4.0μm, and the bubble content is 30vt%.

[0163] Step (3): the amorphous iron phosphate precipitate is uniformly dispersed in the aging solution for aging and crystallization reaction. After the reaction is completed, the amorphous iron phosphate precipitate is filtered and washed with deionized water. The filter residue is vacuum dried at 100° C. for 12 h to obtain iron phosphate dihydrate crystals.

[0164] The aging solution is a phosphoric acid solution containing sodium β-naphthalenesulfonate formaldehyde condensate, the pH value of the aging solution is 1, and the concentration of sodium β-naphthalenesulfonate formaldehyde condensate in the aging solution is 2.5wt%. The feeding ratio of amorphous iron phosphate precipitate to aging solution is 1g:300mL. The temperature of aging crystallization reaction is 80°C, the time is 1h, and the stirring rate is 100rpm.

[0165] Step (4): calcining the dihydrate ferric phosphate crystals to obtain anhydrous ferric phosphate.

[0166] The calcination temperature was 700°C, the heating rate was 4°C / min, and the calcination time was 2h.

[0167] Example 7

[0168] Step (1): preparing a mixed solution according to the feed ratio of iron source to phosphorus source of n(P):n(Fe) of 1.5:1, wherein the iron source is an aqueous solution of ferrous nitrate with a ferrous ion concentration of 2 mol / L, and the phosphorus source is an ammonium dihydrogen phosphate solution with a phosphate ion concentration of 3 mol / L.

[0169] Step (2): The mixed solution, ammonium persulfate with a concentration of 0.8 mol / L, and ammonia water with a concentration of 4 mol / L are added to the reactor in parallel by a constant flow pump. The flow rates of the mixed solution and ammonium persulfate are both 150 mL / h. The flow rate of ammonia water is controlled to maintain the pH of the reaction solution at 1.5±0.1, and the temperature is controlled to maintain at 50°C during the reaction. The reaction time is 4 hours and the stirring speed is 800 rpm. After the reaction is completed, the mixture is filtered and washed with deionized water to obtain an amorphous iron phosphate precipitate (wet material, solid content of 85.9 wt%).

[0170] The mixed solution is reacted with air by a micro-bubble generator and then enters the reactor. The bubble particle size generated by the micro-nano bubble generator is 200nm-4.0μm, and the bubble content is 20vt%.

[0171] Step (3): the amorphous iron phosphate precipitate is uniformly dispersed in the aging solution for aging and crystallization reaction. After the reaction is completed, the amorphous iron phosphate precipitate is filtered and washed with deionized water. The filter residue is vacuum dried at 100° C. for 12 h to obtain iron phosphate dihydrate crystals.

[0172] The aging solution is a phosphoric acid solution containing sodium α-methylnaphthalene sulfonate formaldehyde condensate, the pH value of the aging solution is 1, and the concentration of sodium α-methylnaphthalene sulfonate formaldehyde condensate in the aging solution is 1wt%. The feeding ratio of amorphous iron phosphate precipitate to aging solution is 1g:100mL. The temperature of aging crystallization reaction is 80℃, the time is 3h, and the stirring rate is 300rpm.

[0173] Step (4): calcining the dihydrate ferric phosphate crystals to obtain anhydrous ferric phosphate.

[0174] The calcination temperature was 700°C, the heating rate was 4°C / min, and the calcination time was 2h.

[0175] Comparative Example 1

[0176] The difference between this comparative example and Example 1 is that air is introduced into the liquid phase of the reactor in the form of ordinary air intake, with a flow rate of 1 mL / min.

[0177] Comparative Example 2

[0178] The difference between this comparative example and Example 1 is that sodium hexadecylbenzenesulfonate is used instead of ammonium ligninsulfonate.

[0179] Comparative Example 3

[0180] The difference between this comparative example and Example 1 is that hydroxymethyl cellulose is used instead of ammonium lignin sulfonate.

[0181] Comparative Example 4

[0182] The difference between this comparative example and Example 1 is that the aging solution does not contain a surfactant.

[0183] Comparative Example 5

[0184] The difference between this comparative example and Example 1 is that the oxidant is only hydrogen peroxide and does not contain air.

[0185] Comparative Example 6

[0186] The difference between this comparative example and Example 1 is that the stirring rate of the crystallization reaction in step (3) is 400 rpm.

[0187] Test Example 1

[0188] The iron phosphate materials prepared in Examples 1 to 7 and Comparative Examples 1 to 6 were subjected to the following performance tests.

[0189] (1) The microstructure of the material was observed using a JEOL JSM-6490LV scanning electron microscope, and ImageJ was used to analyze the particle size and average aspect ratio of the primary particles in the scanning electron microscope image. The average diameter of the primary particles is the number average of the equivalent particle size of the primary particles, and the equivalent particle size refers to the diameter of a sphere with the same volume as the primary particle. The average aspect ratio of the primary particles refers to the ratio of the average length of the longest axis to the average length of the shortest axis of the primary particles. The average length of the longest axis refers to the sum of the lengths of the longest axes of the primary particles divided by the number of primary particles, and the longest axis refers to the length of the longest diagonal line in the image. The average length of the shortest axis refers to the sum of the lengths of the shortest axes of the primary particles divided by the number of primary particles, and the longest axis refers to the length of the shortest diagonal line in the image. The number of primary particles measured for each sample was 50, which were randomly selected.

[0190] (2) Particle size D 50 : The test was carried out using MS3000 laser particle size analyzer.

[0191] (3) Determination of specific surface area and specific pore volume: According to GB / T 21650.2-2008 "Determination of pore size distribution and porosity of solid materials by mercury intrusion and gas adsorption method Part 2: Analysis of mesopores and macropores by gas adsorption method". The Autosorb IQ2 fully automatic specific surface area pore size analyzer was used to test the powdered sample to obtain the nitrogen adsorption and desorption curve, the temperature condition was a constant temperature of -196°C, and the pressure condition was 0.005MPa~0.100MPa; the data in the medium and low pressure stages were processed and calculated using the BET formula to obtain the specific surface area, and the specific pore volume was calculated using the BJH model.

[0192] (4) Determination of grinding efficiency: Weigh the same mass of anhydrous iron phosphate for dry ball milling, take samples at certain times to measure the particle size and calculate the particle size distribution width span = (D 90 -D 10 ) / D 50 Ball milling conditions: frequency of 30 Hz, 1 mm zirconia beads, volume ratio of zirconia beads to anhydrous ferric phosphate of 1:1, and rotation speed of 600 rpm.

[0193] (5) XRD: X-ray powder diffractometer (XRD, Rigaku D / max-2600PC, Japan) was used to study the crystal phase and crystal structure of the material. The K α XRD, wavelength λ is 0.154056nm, voltage is 40kV, current is 40mA, scanning range 2θ is 10° to 80°. XRD test results are analyzed using Jade 6 software.

[0194] (6) The Fe and P contents in FePO3·2H2O were tested by titration analysis as follows: Weigh the sample and dissolve it completely in hydrochloric acid. 3+ Reduction to Fe 2+ , then add saturated solution of mercuric chloride, use sodium diphenylamine sulfonate as indicator, and titrate with K2Cr2O7 standard solution to calculate the iron content of the sample. Dissolve the sample with hydrochloric acid, then add quinomolybdenum reagent and nitric acid, the reaction will produce a yellow precipitate, filter it, add NaOH to dissolve the precipitate, then titrate the excess NaOH with HCl to calculate the phosphorus content of the sample.

[0195] The test results are as follows Figures 1 to 6 , as shown in Table 1 and Table 2.

[0196] Depend on Figures 1 to 5It can be seen that the primary particles of anhydrous iron phosphate prepared in Example 1 are spherical, uniform in particle size, with an average particle size of about 400nm, and the agglomeration of primary particles is relatively loose. Comparative Example 1 uses ordinary air intake to introduce air, and the uniformity of the obtained particles is poor, so the agglomeration is tighter than that of Example 1; Comparative Example 2 uses sodium hexadecylbenzene sulfonate as a surfactant, and the particle size of the obtained crystals is large, with an average particle size of about 800nm. The electrochemical performance is poor due to the excessive particle size. The reason is that although sodium hexadecylbenzene sulfonate can be electrostatically adsorbed on the surface of the crystals to regulate the crystal morphology, it cannot inhibit the growth and agglomeration of the particles due to the low steric hindrance effect provided; Comparative Example 3 uses sodium hydroxymethyl cellulose as a surfactant, and the primary particles obtained are spherical, but the size uniformity is poor, and there are more large particles, and the agglomeration is serious. The reason is that the overall polarity of sodium hydroxymethyl cellulose is relatively uniform, so the dispersibility of the crystals is weak; Comparative Example 4 does not add a surfactant, and the primary particles obtained are disc-shaped, and the agglomeration is serious.

[0197] Depend on Figure 6 It can be seen that: each sample is consistent with the standard spectrum of monoclinic FePO4·2H2O (PDF#33-0666), indicating that the addition of surfactant has no effect on the structure of ferric phosphate dihydrate; however, the peak value of the main peak of the diffraction peak of Example 1, Comparative Examples 2 and 3 is higher, the half-peak width is reduced, and the crystallinity of the product is improved, indicating that the addition of surfactant improves the crystallinity of the material; the crystallinity of Comparative Example 1 is relatively low, which is because the gaseous oxidant is introduced in an ordinary manner, which cannot play a role in loosening the amorphous agglomerates, and the obtained amorphous agglomerates have a larger particle size. In the subsequent crystallization stage, part of the amorphous remains inside the crystal, resulting in a decrease in crystallinity.

[0198] Table 1 Test results

[0199]

[0200] Table 2 Test results

[0201]

[0202] It can be seen from Table 1 and Table 2 that:

[0203] The surfactant provided in the embodiment of the present invention has a similar effect on the morphology regulation of ferric phosphate dihydrate, and can obtain nearly spherical primary particles, exert steric hindrance, and inhibit the agglomeration of primary particles. Examples 1 to 3 use different surfactant addition amounts. When the addition amount is small, the average major-minor axis ratio of the primary particles is larger; when the addition amount is large, the average major-minor axis ratio of the primary particles decreases, but the particle size of the primary particles becomes smaller, resulting in a larger specific surface area, which is conducive to agglomeration, thereby resulting in a decrease in specific pore volume. Although the hardness index of Example 3 is smaller than that of Examples 1 to 2, due to its smallest particle size, the grinding effect (the smaller the Span, the worse the grinding effect) is not as good as that of Examples 1 and 2.

[0204] The difference between Examples 1, 4 and 5 is that the bubble content of the mixed solution after passing through the micro-nano bubble generator is controlled, and the comparative example 1 adopts the ordinary ventilation method to add air. When the bubble content is low or the air is introduced in the ordinary way, the loosening effect of the bubbles on the agglomerates is worse, the agglomerates obtained are larger in volume, and the crystallization efficiency in the crystallization stage is lower. On the one hand, part of the amorphous remains in the crystal, resulting in a lower crystallinity (poor electrochemical performance); on the other hand, it leads to fewer crystal nuclei formed initially, larger grain size, and tight combination, which is not conducive to grinding, so the span is low; and too much bubble content will make the primary particles smaller, which is also not conducive to grinding, so the span of Example 1 is the highest.

[0205] Example 1 and Comparative Examples 2, 3, and 4 are single-factor tests of surfactants. Comparative Example 2 uses a small molecule surfactant, which provides a poor steric hindrance effect, so the primary particle size obtained is larger, thereby reducing the specific surface area. However, due to the large primary particle size and relatively uniform distribution, its specific pore volume is smaller than that of Example 1; in addition, due to the excessive size of its primary particles, the lithium iron phosphate particles obtained under the same grinding conditions are also larger, and the electrochemical performance is reduced. Although Comparative Example 3 is a polymer surfactant, the polarity within its molecular chain is low, the dispersibility of the particles is poor, and the steric hindrance effect provided is not as good as that of Example 1. Therefore, the obtained dihydrate iron phosphate has a wide particle size distribution, a large bulk density, a low specific pore volume, a reduced grinding efficiency, and a low span; and the secondary particles formed are larger, so the particles obtained after grinding are still larger, resulting in the D of the iron phosphate. 50 The chemical properties are low. In Comparative Example 4, no surfactant was added, and the primary particles obtained were disc-shaped, so the BET was large. Due to the large diameter ratio, the hardness index was high, the grinding efficiency was low, and the D of the iron phosphate obtained by sintering was 50 Large, so the chemical performance is low.

[0206] Test Example 2

[0207] The iron phosphate material prepared in Examples 1 to 7 and Comparative Examples 1 to 6 was mixed with lithium carbonate and glucose in a molar ratio of n (iron element in the iron phosphate material): n (Li): n (glucose) = 1: 1.04: 0.05 to obtain a mixed raw material; the mixed raw material was mixed with ethanol and ground in a grinder for 6 hours to obtain a slurry; the slurry was dried in a vacuum oven at 80° C. for 4 hours to obtain a dry material; the dry material was calcined at 750° C. for 9 hours under a nitrogen atmosphere, and after screening, a lithium iron phosphate positive electrode material was obtained.

[0208] The above positive electrode materials were mixed into a uniform slurry according to the mass ratio of positive electrode material: acetylene black: PVDF = 75:15:10, and evenly coated on an aluminum foil substrate as the positive electrode of the simulated battery. The negative electrode of the simulated battery used a lithium sheet, a polypropylene porous membrane as a diaphragm, and an electrolyte of 1 mol LiPF6 dissolved in a mixed solvent of 1L EC and DMC (volume ratio 1:1). The positive electrode, negative electrode, electrolyte, and diaphragm were assembled into a battery in an argon-protected glove box.

[0209] The battery constant current charge and discharge and cycle performance tests were performed using the LAND battery test system. At 25°C, the charge and discharge voltage range was 2.5V to 4.2V.

[0210] The electrochemical performance test results of each positive electrode material are shown in Table 3.

[0211] Table 3 Test results

[0212]

[0213] It can be seen from Table 3 that the positive electrode materials prepared from the iron phosphate materials provided in the embodiments of the present invention can have a higher charge-discharge specific capacity.

[0214] In summary, the present invention reduces the primary particle equivalent particle size of the iron phosphate material and the secondary particle D 50 And the hardness index of the iron phosphate material is limited to a specific range, so that the iron phosphate material meeting the above characteristics has a loose structure and a lower overall hardness. When used to prepare positive electrode materials, it can improve the efficiency of grinding with the lithium source and cause less wear on the machine. The prepared positive electrode material has good electrochemical properties, which is conducive to the further preparation of batteries and electrical devices with excellent electrochemical properties.

[0215] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An iron phosphate material, characterized in that: The iron phosphate material is a secondary particle formed by agglomeration of primary particles, the equivalent particle size of the primary particles is 20nm~600nm, and the equivalent particle size is the diameter of a standard sphere with the same volume as the primary particles; the D 50 5μm~20μm; The hardness index of the iron phosphate material has a value of ≤5; The hardness index = ,in, is the average major-minor axis ratio of the primary particles, which refers to the ratio of the average length of the longest axis to the average length of the shortest axis of the primary particles; is the specific pore volume of the iron phosphate material, in cm 3 / g.

2. The iron phosphate material according to claim 1, characterized in that: The iron phosphate material also has at least one of the following characteristics: Feature 1: The iron phosphate material is anhydrous iron phosphate material; Feature 2: The iron phosphate material 0.3cm 3 / g~1.3cm 3 / g; Feature 3: The average aspect ratio of the primary particles is no more than 3.5; Feature 4: The hardness index of the iron phosphate material is 0.98-3.57; Feature 5: The equivalent particle size of the primary particles is 254nm~411nm; Feature 6: D of the secondary particles 50 It is 8.74μm~10.28μm.

3. A method for preparing the iron phosphate material according to claim 1 or 2, characterized in that: The following steps are involved: The mixed solution consisting of the iron source solution and the phosphorus source solution is reacted with air through a microbubble generator and then mixed with an oxidant and a pH regulator to undergo a synthesis reaction, and the amorphous iron phosphate precipitate obtained by the reaction is collected; the amorphous iron phosphate precipitate is aged and crystallized to obtain dihydrate iron phosphate crystals; the dihydrate iron phosphate crystals are calcined to obtain anhydrous iron phosphate material; The oxidant comprises at least one of hydrogen peroxide, ozone, sodium persulfate, ammonium persulfate, sodium hypochlorite, sodium ferrate and oxygen; The aging and crystallization process comprises: dispersing the amorphous iron phosphate precipitate in an aging solution to perform a crystallization reaction; Wherein, the aging solution is a phosphoric acid solution containing a surfactant; The surfactant comprises at least one of lignin sulfonate and naphthalene sulfonate formaldehyde condensate; wherein the lignin sulfonate comprises at least one of sodium lignin sulfonate and ammonium lignin sulfonate; the naphthalene sulfonate formaldehyde condensate comprises at least one of β-naphthalene sulfonate sodium formaldehyde condensate, benzyl naphthalene sulfonate sodium formaldehyde condensate, α-methyl naphthalene sulfonate sodium formaldehyde condensate and alkyl benzene sulfonate sodium formaldehyde condensate; The stirring rate of the crystallization reaction is 100rpm~300rpm.

4. The preparation method according to claim 3, characterized in that: The synthesis reaction includes at least one of the following characteristics: Feature 7: The iron source solution is a soluble ferrous salt solution; Feature 8: The phosphorus source includes at least one of phosphoric acid, sodium dihydrogen phosphate, sodium monohydrogen phosphate, ammonium dihydrogen phosphate and ammonium monohydrogen phosphate; Feature 9: The pH adjuster includes at least one of ammonia water, sodium hydroxide, sulfuric acid, hydrochloric acid and nitric acid; Feature 10: The concentration of the iron source solution is 0.8 mol / L to 1.5 mol / L; Feature 11: The concentration of the phosphorus source solution is 0.85 mol / L~3 mol / L; Feature 12: The iron source and the phosphorus source are added in a ratio of the amount of P to the amount of Fe of 1.05:1 to 1.5:1; Feature 13: The total amount of the air and the oxidant is not less than the theoretical amount of Fe in the iron source. 2+ All oxidized to Fe 3+ The amount of feature 14: The pH value of the synthesis reaction is 1~2.5; Feature 15: The temperature of the synthesis reaction is 50°C~70°C; Feature 16: The synthesis reaction time is 1h~4h; Feature 17: The stirring speed of the synthesis reaction is 400 rpm to 800 rpm.

5. The preparation method according to claim 3, characterized in that: The crystal transformation reaction includes at least one of the following characteristics: Feature 18: The pH value of the aging solution is 1 to 2.5; Feature 19: The concentration of the surfactant contained in the aging solution is 1wt%~5wt%; Feature 20: The feed ratio of the amorphous iron phosphate precipitate to the aged solution is 1 g: 100 mL to 1 g: 300 mL; Feature 21: The temperature of the crystallization reaction is 80℃~90℃; Feature 22: The crystallization reaction time is 1h~3h.

6. The preparation method according to claim 3, characterized in that: Calcination includes at least one of the following characteristics: Feature 23: The calcination temperature is 600°C~750°C; Feature 24: Calcination time is 2h~3h; Feature 25: The heating rate during the calcination process is 3℃ / min~5℃ / min.

7. A positive electrode material, characterized in that: The positive electrode material is prepared by mixing and sintering the iron phosphate material according to claim 1 or 2 with a lithium source and a carbon source.

8. A positive electrode sheet, characterized in that: The active material in the positive electrode sheet includes the positive electrode material according to claim 7.

9. A battery, characterized in that: The battery comprises the positive electrode sheet according to claim 8.