Anti-skid and wear-resistant rubber composition for shoes and preparation method thereof
By using a combination of hydrogenated nitrile rubber, chlorinated polyethylene rubber and other materials in rubber soles, combined with specific processes, the problem of poor wear resistance and anti-slip properties of natural rubber soles is solved, achieving better wear resistance and Anti-slip and toughness properties reduce production costs.
Patent Information
- Application Number
- CN202411008463.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing natural rubber soles have poor wear resistance and anti-slip properties during use, and there is an urgent need for a rubber composition with good wear resistance and anti-slip properties for shoes.
Made of hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, ethylene-vinyl acetate copolymer, coumaron resin, reinforcing agent, paraffin wax, vulcanizing agent, antioxidant, zinc stearate, stearin Calcium acid, accelerator and polyethylene An anti-slip and wear-resistant rubber composition for shoes composed of olefin wax, etc., and is prepared through a specific mixing and internal mixing process. The preferred reinforcing agent is composed of four needle-like zinc oxide whiskers and a titanate coupling agent, and is prepared through sodium rosinate. Dilution treatment to improve interface status.
The wear resistance, anti-skid property and toughness of the rubber composition are improved, the mechanical properties are enhanced, the production cost is reduced, and the wearing comfort is improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of shoe rubber preparation, and in particular relates to a non-slip and wear-resistant rubber composition for shoes and a preparation method thereof. Background Art
[0002] Rubber soles refer to soles made of rubber. The materials of rubber soles can be roughly divided into natural rubber or synthetic rubber. The advantage of natural rubber is that it is very soft and elastic, and it can be suitable for various sports to play a shock-absorbing role, but the disadvantage is also obvious, that is, it is not wear-resistant, and sports shoes mostly use natural rubber. Due to the natural shortcomings of natural rubber, the wear resistance and anti-skid performance of natural rubber soles are extremely poor when they are used; therefore, a rubber composition with good wear resistance and anti-skid performance for shoes is urgently needed. Summary of the invention
[0003] The purpose of the present invention is to overcome the disadvantages of the prior art and provide an anti-skid and wear-resistant rubber composition for shoes and a preparation method thereof.
[0004] The present invention adopts the following technical solution:
[0005] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0006] 50 parts of hydrogenated nitrile rubber
[0007] Chlorinated polyethylene rubber 20-30 parts
[0008] Polyamide thermoplastic elastomer 10-15 parts
[0009] 8-12 parts of ethylene-vinyl acetate copolymer
[0010] 6-10 parts of Coumarone resin
[0011] Reinforcing agent 18-22 parts
[0012] 2-3 parts paraffin
[0013] Vulcanizing agent 1.2-1.3 parts
[0014] Anti-aging agent 0.8-1 part
[0015] Zinc stearate 1.2-1.5 parts
[0016] Calcium stearate 0.3-0.5 parts
[0017] Accelerator 0.8-1 part
[0018] 1-2 parts of polyethylene wax.
[0019] Preferably, the reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosinate.
[0020] Preferably, the reinforcing agent is prepared as follows: first, tetrapod-shaped zinc oxide whiskers and sodium rosin acid are fed into a high-speed mixer and stirred for 8 minutes, then the diluted titanate coupling agent is sprayed in a mist form, and stirring is continued for 15 minutes; then the temperature is raised to 90° C. and stirred for 5 minutes to obtain the reinforcing agent.
[0021] Preferably, the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0022] Preferably, the vulcanizing agent is insoluble sulfur.
[0023] Preferably, the accelerator is one or more of vulcanization accelerator M, vulcanization accelerator D, and vulcanization accelerator TMTD.
[0024] Preferably, the antioxidant is antioxidant MB.
[0025] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0026] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 15-20 minutes to obtain a premix;
[0027] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, discharging at 116-118° C., and leaving at room temperature for more than 24 hours;
[0028] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
[0029] Preferably, in step 2, the banburying process specifically includes: putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into a banbury mixer, mixing and banburying for 5-10 minutes; then adjusting the banburying temperature to 90°C, keeping it for 3 minutes and then turning the material once; when the banburying temperature rises to 95°C, turning the material twice; when the banburying temperature rises to 104°C, turning the material three times; when the banburying temperature rises to 110°C, turning the material four times; when the banburying temperature rises to 116-118°C, turning the material five times, and then banburying for 1 minute, debonding, and leaving it at room temperature for more than 24 hours.
[0030] From the above description of the present invention, it can be seen that compared with the prior art, the present invention has the following beneficial effects: the present invention limits the use of hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer to be mixed with each other, which can complement each other in performance and increase the tolerance to fillers, so that the prepared rubber composition has good wear resistance and good anti-skid properties; wherein, the introduction of coumarone resin and polyethylene wax to make the compatibility and dispersibility of the components between the molecules are good, and the wear resistance of the prepared composition is improved while the compatibility of the system is improved, and the loss of mechanical properties of the composition is reduced; paraffin wax and ethylene-vinyl acetate copolymer are introduced to match the polyamide thermoplastic elastomer to compensate for the problem of poor toughness caused by the increase in the amount of reinforcing agent with rubber as the main body, so as to ensure that the composition has excellent wear resistance and anti-skid properties, and can also improve the toughness of the composition to improve the comfort of wearing;
[0031] The reinforcing agent takes four-needle zinc oxide whisker as a matrix, and sodium rosin acid salt and titanate coupling agent are introduced to process the added four-needle zinc oxide whisker. The titanate coupling agent is evenly distributed on the surface of the four-needle zinc oxide whisker through the added sodium rosin acid salt, thereby improving the interface state of the reinforcing agent, forming a strong interface adhesion between the reinforcing agent and other components, thereby effectively improving the mechanical properties of the prepared rubber composition, reducing the amount of rubber without significantly increasing the amount of the reinforcing agent, and reducing the production cost while ensuring the performance of the rubber composition. DETAILED DESCRIPTION
[0032] The present invention is further described below through specific implementation modes.
[0033] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0034] 50 parts of hydrogenated nitrile rubber
[0035] Chlorinated polyethylene rubber 20-30 parts
[0036] Polyamide thermoplastic elastomer 10-15 parts
[0037] 8-12 parts of ethylene-vinyl acetate copolymer
[0038] 6-10 parts of Coumarone resin
[0039] Reinforcing agent 18-22 parts
[0040] 2-3 parts paraffin
[0041] Insoluble sulfur 1.2-1.3 parts
[0042] Anti-aging agent MB 0.8-1 part
[0043] Zinc stearate 1.2-1.5 parts
[0044] Calcium stearate 0.3-0.5 parts
[0045] Accelerator 0.8-1 part
[0046] 1-2 parts of polyethylene wax.
[0047] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosin acid. The preparation method is as follows: first, the tetrapod-shaped zinc oxide whiskers and sodium rosin acid are fed into a high-speed mixer and stirred for 8 minutes, and then the diluted titanate coupling agent is sprayed in a mist form and stirred for 15 minutes; then the temperature is raised to 90°C and stirred for 5 minutes to obtain the reinforcing agent; and the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0048] The accelerator is one or more of the vulcanization accelerator M, the vulcanization accelerator D, and the vulcanization accelerator TMTD.
[0049] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0050] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 15-20 minutes to obtain a premix;
[0051] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, and mixing and internal mixing for 5-10 minutes; then adjusting the internal mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the internal mixing temperature rises to 95°C, turning the material twice; when the internal mixing temperature rises to 104°C, turning the material three times; when the internal mixing temperature rises to 110°C, turning the material four times; when the internal mixing temperature rises to 116-118°C, turning the material five times, and then internal mixing for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0052] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes. Example 1
[0053] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0054] 50 parts of hydrogenated nitrile rubber
[0055] Chlorinated polyethylene rubber 20 parts
[0056] Polyamide thermoplastic elastomer 15 parts
[0057] 8 parts of ethylene-vinyl acetate copolymer
[0058] 6 parts of Coumarone resin
[0059] 18 parts of reinforcing agent
[0060] 2 parts paraffin
[0061] 1.2 parts insoluble sulfur
[0062] Anti-aging agent MB 1 part
[0063] 1.5 parts of zinc stearate
[0064] 0.3 parts of calcium stearate
[0065] Vulcanization accelerator M 1 part
[0066] 1 part of polyethylene wax.
[0067] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosin acid. The preparation method is as follows: first, the tetrapod-shaped zinc oxide whiskers and sodium rosin acid are fed into a high-speed mixer and stirred for 8 minutes, and then the diluted titanate coupling agent is sprayed in a mist form and stirred for 15 minutes; then the temperature is raised to 90°C and stirred for 5 minutes to obtain the reinforcing agent; and the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0068] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0069] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 15 minutes to obtain a premix;
[0070] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, and mixing and internal mixing for 10 minutes; then adjusting the internal mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the internal mixing temperature rises to 95°C, turning the material twice; when the internal mixing temperature rises to 104°C, turning the material three times; when the internal mixing temperature rises to 110°C, turning the material four times; when the internal mixing temperature rises to 116°C, turning the material five times, and then internal mixing for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0071] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes. Example 2
[0072] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0073] 50 parts of hydrogenated nitrile rubber
[0074] Chlorinated polyethylene rubber 30 parts
[0075] Polyamide thermoplastic elastomer 10 parts
[0076] 12 parts of ethylene-vinyl acetate copolymer
[0077] 10 parts of Coumarone resin
[0078] 22 parts of reinforcing agent
[0079] 3 parts paraffin
[0080] 1.3 parts insoluble sulfur
[0081] Anti-aging agent MB 0.8 parts
[0082] 1.2 parts of zinc stearate
[0083] 0.5 parts of calcium stearate
[0084] Vulcanization accelerator M 0.8 parts
[0085] 2 parts of polyethylene wax.
[0086] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosin acid. The preparation method is as follows: first, the tetrapod-shaped zinc oxide whiskers and sodium rosin acid are fed into a high-speed mixer and stirred for 8 minutes, and then the diluted titanate coupling agent is sprayed in a mist form and stirred for 15 minutes; then the temperature is raised to 90°C and stirred for 5 minutes to obtain the reinforcing agent; and the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0087] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0088] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 20 minutes to obtain a premix;
[0089] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, and mixing and internal mixing for 5 minutes; then adjusting the internal mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the internal mixing temperature rises to 95°C, turning the material twice; when the internal mixing temperature rises to 104°C, turning the material three times; when the internal mixing temperature rises to 110°C, turning the material four times; when the internal mixing temperature rises to 118°C, turning the material five times, and then internal mixing for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0090] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes. Example 3
[0091] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0092] 50 parts of hydrogenated nitrile rubber
[0093] Chlorinated polyethylene rubber 25 parts
[0094] Polyamide thermoplastic elastomer 12 parts
[0095] 10 parts of ethylene-vinyl acetate copolymer
[0096] 8 parts of Coumarone resin
[0097] 20 parts of reinforcing agent
[0098] 2.5 parts paraffin
[0099] 1.26 parts insoluble sulfur
[0100] Anti-aging agent MB 0.9 parts
[0101] 1.3 parts of zinc stearate
[0102] 0.4 parts of calcium stearate
[0103] Vulcanization accelerator M 0.6 parts
[0104] Vulcanization accelerator TMTD 0.3 parts
[0105] 1.5 parts of polyethylene wax.
[0106] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosin acid. The preparation method is as follows: first, the tetrapod-shaped zinc oxide whiskers and sodium rosin acid are fed into a high-speed mixer and stirred for 8 minutes, and then the diluted titanate coupling agent is sprayed in a mist form and stirred for 15 minutes; then the temperature is raised to 90°C and stirred for 5 minutes to obtain the reinforcing agent; and the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0107] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0108] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 18 minutes to obtain a premix;
[0109] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, and mixing and internal mixing for 8 minutes; then adjusting the internal mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the internal mixing temperature rises to 95°C, turning the material twice; when the internal mixing temperature rises to 104°C, turning the material three times; when the internal mixing temperature rises to 110°C, turning the material four times; when the internal mixing temperature rises to 118°C, turning the material five times, and then internal mixing for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0110] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
[0111] Comparative Example 1
[0112] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0113] 50 parts of hydrogenated nitrile rubber
[0114] Chlorinated polyethylene rubber 25 parts
[0115] 10 parts of ethylene-vinyl acetate copolymer
[0116] 8 parts of Coumarone resin
[0117] 20 parts of reinforcing agent
[0118] 2.5 parts paraffin
[0119] 1.26 parts insoluble sulfur
[0120] Anti-aging agent MB 0.9 parts
[0121] 1.3 parts of zinc stearate
[0122] 0.4 parts of calcium stearate
[0123] Vulcanization accelerator M 0.6 parts
[0124] Vulcanization accelerator TMTD 0.3 parts
[0125] 1.5 parts of polyethylene wax.
[0126] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosin acid. The preparation method is as follows: first, the tetrapod-shaped zinc oxide whiskers and sodium rosin acid are fed into a high-speed mixer and stirred for 8 minutes, and then the diluted titanate coupling agent is sprayed in a mist form and stirred for 15 minutes; then the temperature is raised to 90°C and stirred for 5 minutes to obtain the reinforcing agent; and the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0127] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0128] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 18 minutes to obtain a premix;
[0129] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, and mixing and internal mixing for 8 minutes; then adjusting the internal mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the internal mixing temperature rises to 95°C, turning the material twice; when the internal mixing temperature rises to 104°C, turning the material three times; when the internal mixing temperature rises to 110°C, turning the material four times; when the internal mixing temperature rises to 118°C, turning the material five times, and then internal mixing for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0130] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
[0131] Comparative Example 2
[0132] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0133] 50 parts of hydrogenated nitrile rubber
[0134] Chlorinated polyethylene rubber 25 parts
[0135] Polyamide thermoplastic elastomer 12 parts
[0136] 10 parts of ethylene-vinyl acetate copolymer
[0137] 8 parts of Coumarone resin
[0138] 20 parts of talcum powder
[0139] 2.5 parts paraffin
[0140] 1.26 parts insoluble sulfur
[0141] Anti-aging agent MB 0.9 parts
[0142] 1.3 parts of zinc stearate
[0143] 0.4 parts of calcium stearate
[0144] Vulcanization accelerator M 0.6 parts
[0145] Vulcanization accelerator TMTD 0.3 parts
[0146] 1.5 parts of polyethylene wax.
[0147] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0148] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 18 minutes to obtain a premix;
[0149] Step 2, putting the premix prepared in step 1, talcum powder, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into a mixer, mixing and mixing for 8 minutes; then adjusting the mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the mixing temperature rises to 95°C, turning the material twice; when the mixing temperature rises to 104°C, turning the material three times; when the mixing temperature rises to 110°C, turning the material four times; when the mixing temperature rises to 118°C, turning the material five times, mixing for 1 minute, draining the glue, and leaving it at room temperature for more than 24 hours;
[0150] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
[0151] Comparative Example 3
[0152] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0153] 50 parts of hydrogenated nitrile rubber
[0154] Chlorinated polyethylene rubber 25 parts
[0155] Polyamide thermoplastic elastomer 12 parts
[0156] 10 parts of ethylene-vinyl acetate copolymer
[0157] 8 parts of Coumarone resin
[0158] 20 parts of reinforcing agent
[0159] 2.5 parts paraffin
[0160] 1.26 parts insoluble sulfur
[0161] Anti-aging agent MB 0.9 parts
[0162] 1.3 parts of zinc stearate
[0163] 0.4 parts of calcium stearate
[0164] Vulcanization accelerator M 0.6 parts
[0165] Vulcanization accelerator TMTD 0.3 parts
[0166] 1.5 parts of polyethylene wax.
[0167] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers and 0.18 parts of titanate coupling agent, and its preparation method is as follows: after the tetrapod-shaped zinc oxide whiskers are fed into a high-speed mixer, the diluted titanate coupling agent is sprayed in a mist form and stirred for 15 minutes; then the temperature is raised to 90° C. and stirred for 5 minutes to obtain the reinforcing agent; and the titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:12.
[0168] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0169] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 18 minutes to obtain a premix;
[0170] Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, and mixing and internal mixing for 8 minutes; then adjusting the internal mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the internal mixing temperature rises to 95°C, turning the material twice; when the internal mixing temperature rises to 104°C, turning the material three times; when the internal mixing temperature rises to 110°C, turning the material four times; when the internal mixing temperature rises to 118°C, turning the material five times, and then internal mixing for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0171] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
[0172] Comparative Example 4
[0173] The anti-skid and wear-resistant rubber composition for shoes is composed of the following raw materials in parts by weight:
[0174] 50 parts of hydrogenated nitrile rubber
[0175] Chlorinated polyethylene rubber 25 parts
[0176] Polyamide thermoplastic elastomer 12 parts
[0177] 10 parts of ethylene-vinyl acetate copolymer
[0178] 8 parts of Coumarone resin
[0179] 20 parts of reinforcing agent
[0180] 2.5 parts paraffin
[0181] 1.26 parts insoluble sulfur
[0182] Anti-aging agent MB 0.9 parts
[0183] 1.3 parts of zinc stearate
[0184] 0.4 parts of calcium stearate
[0185] Vulcanization accelerator M 0.6 parts
[0186] Vulcanization accelerator TMTD 0.3 parts
[0187] 1.5 parts of polyethylene wax.
[0188] The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosinate.
[0189] The method for preparing an anti-skid and wear-resistant rubber composition for shoes comprises the following steps:
[0190] Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 18 minutes to obtain a premix;
[0191] Step 2, putting the premix prepared in step 1, tetrapod-shaped zinc oxide whiskers, titanate coupling agent, sodium rosin acid, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into a banbury mixer, mixing and banburying for 8 minutes; then adjusting the banburying temperature to 90° C., keeping for 3 minutes and then turning the material once; when the banburying temperature rises to 95° C., turning the material twice; when the banburying temperature rises to 104° C., turning the material three times; when the banburying temperature rises to 110° C., turning the material four times; when the banburying temperature rises to 118° C., turning the material five times, and then banburying for 1 minute, debonding, and leaving at room temperature for more than 24 hours;
[0192] Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
[0193] The rubber compositions prepared in Examples 1-3 and Comparative Examples 1-4 were cut into sole shapes and put into rubber shoe molds for vulcanization to obtain rubber soles, and then the prepared rubber soles were subjected to corresponding performance tests to obtain the following results; wherein, DIN abrasion was tested in accordance with GB / T9867:2001; dry anti-skid and wet anti-skid were tested in accordance with TM144:2011; and the rebound value was tested using a GT-7042-RE impact elasticity testing machine.
[0194] Table 1 Performance test table of rubber soles prepared in various embodiments
[0195]
[0196] It can be seen from the above table that the rubber composition prepared in the present application has good wear resistance and good anti-slip properties; among them, by comparing Example 3 with Comparative Example 1, it can be seen that paraffin wax and ethylene-vinyl acetate copolymer are introduced to cooperate with polyamide thermoplastic elastomer to make up for the problem of poor toughness caused by the increase in the amount of reinforcing agent with rubber as the main body, so as to ensure that the composition has excellent wear resistance and anti-slip properties, and at the same time, the toughness of the composition can be improved to improve the wearing comfort;
[0197] By comparing Example 3 with Comparative Example 2, it can be seen that the present application specifically defines the composition of the reinforcing agent, and the reinforcing agent can be combined with other components to form a strong interface bond between the reinforcing agent and other components, thereby effectively improving the mechanical properties of the prepared rubber composition;
[0198] By comparing Example 3 with Comparative Examples 3 and 4, it can be seen that the introduction of sodium rosin acid and titanate coupling agent to pretreat the tetrapod-shaped zinc oxide whiskers allows the titanate coupling agent to be evenly distributed on the surface of the tetrapod-shaped zinc oxide whiskers under the action of sodium rosin acid, thereby improving the interface state of the reinforcing agent and effectively improving the mechanical properties of the prepared rubber composition.
[0199] In summary, the present invention limits the mixing of hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer, which can complement each other in performance and increase the tolerance to fillers, so that the prepared rubber composition has good wear resistance, good anti-slip property, and good toughness; wherein, the introduction of coumarone resin and polyethylene wax to make the compatibility and dispersibility between the molecules of each component good, improves the wear resistance of the prepared composition, improves the compatibility of the system, and reduces the loss of mechanical properties of the composition; paraffin wax and ethylene-vinyl acetate copolymer are introduced to cooperate with polyamide thermoplastic elastomer to make up for the problem of poor toughness caused by the increase in the amount of reinforcing agent with rubber as the main body, so as to ensure that the composition has excellent wear resistance and anti-slip property, and can also improve the toughness of the composition to improve the wearing comfort.
[0200] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the scope of the patent application of the present invention and the contents of the specification should still fall within the scope covered by the patent of the present invention.
Claims
1. Anti-skid and wear-resistant rubber composition for shoes, Features: It is composed of the following raw materials in parts by weight: 50 parts of hydrogenated nitrile rubber Chlorinated polyethylene rubber 20-30 parts Polyamide thermoplastic elastomer 10-15 parts 8-12 parts of ethylene-vinyl acetate copolymer 6-10 parts of Coumarone resin Reinforcing agent 18-22 parts 2-3 parts paraffin Vulcanizing agent 1.2-1.3 parts Anti-aging agent 0.8-1 part Zinc stearate 1.2-1.5 parts Calcium stearate 0.3-0.5 parts Accelerator 0.8-1 part 1-2 parts of polyethylene wax; The reinforcing agent is composed of the following raw materials in parts by weight: 10 parts of tetrapod-shaped zinc oxide whiskers, 0.18 parts of titanate coupling agent, and 0.18 parts of sodium rosinate; The preparation method of the reinforcing agent is as follows: first, four-needle zinc oxide whiskers and sodium rosin acid are put into a high-speed mixer and stirred for 8 minutes, then the diluted titanate coupling agent is sprayed into it in a mist form, and the stirring is continued for 15 minutes; then the temperature is raised to 90° C. and stirred for 5 minutes to obtain the reinforcing agent; The titanate coupling agent is diluted with isopropyl alcohol, and the titanate coupling agent and isopropyl alcohol are mixed and diluted in a volume ratio of 1:
12.
2. The anti-skid and wear-resistant rubber composition for shoes according to claim 1, Features: The vulcanizing agent is insoluble sulfur.
3. The anti-skid and wear-resistant rubber composition for shoes according to claim 1, Features: The accelerator is one or more of vulcanization accelerator M, vulcanization accelerator D, and vulcanization accelerator TMTD.
4. The anti-skid and wear-resistant rubber composition for shoes according to claim 1, Features: The antioxidant is antioxidant MB.
5. A method for preparing the anti-skid and wear-resistant rubber composition for shoes as claimed in claim 1, Features: The following steps are involved: Step 1, feeding hydrogenated nitrile rubber, chlorinated polyethylene rubber, polyamide thermoplastic elastomer, and ethylene-vinyl acetate copolymer into a high-speed mixer according to the raw material ratio, and stirring for 15-20 minutes to obtain a premix; Step 2, putting the premix prepared in step 1, reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into an internal mixer, discharging at 116-118° C., and leaving at room temperature for more than 24 hours; Step 3, kneading the mixture obtained in step 2 on a double-roll mill, adding the required amount of vulcanizing agent and accelerator, mixing evenly, and sheeting to obtain the anti-skid and wear-resistant rubber composition for shoes.
6. The method for preparing the anti-skid and wear-resistant rubber composition for shoes according to claim 5, Features: In step 2, the mixing process specifically includes: putting the premix prepared in step 1 and the reinforcing agent, paraffin, antioxidant, zinc stearate, calcium stearate, and polyethylene wax into a mixer, mixing and mixing for 5-10 minutes; then adjusting the mixing temperature to 90°C, keeping for 3 minutes and then turning the material once; when the mixing temperature rises to 95°C, turning the material twice; when the mixing temperature rises to 104°C, turning the material three times; when the mixing temperature rises to 110°C, turning the material four times; when the mixing temperature rises to 116-118°C, turning the material five times, mixing for 1 minute, draining the glue, and leaving it at room temperature for more than 24 hours.
Citation Information
Patent Citations
Roller resistant to high-temperature hydrogen peroxide and sodium hydroxide mediums and manufacture method thereof
CN110003546A
Antiskid wear-resistant foaming rain shoe sole and production process thereof
CN112980089A