Bismuth-containing functional auxiliary agent and antibacterial and healing-promoting bismuth-containing dressing and preparation method thereof

By using zeolite as a carrier and organic ligand for coordination reaction in bismuth tribromophenol dressing, a bismuth-containing functional additive was prepared, which was combined with petroleum jelly, liquid paraffin and glycerin to solve the problems of dispersion and burst release and achieve efficient antibacterial effect. And the effect of promoting healing avoids the risk of secondary wound injury and toxicity.

CN118557773BActive Publication Date: 2024-10-15ROOSIN MEDICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048437.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing bismuth tribromophenate dressings have poor dispersion in water and commonly used organic solvents, and are prone to burst release, leading to the accumulation of bismuth compounds in skin tissues, causing toxicity risks and affecting long-lasting antibacterial effects.

Method used

Using zeolite as a carrier, bismuth-containing functional additives are prepared through ion exchange and organic ligand coordination reactions. Combining petroleum jelly, liquid paraffin and glycerin, an antibacterial and healing bismuth-containing dressing is prepared through a blending coating process, utilizing the porous nature of zeolite The structure and chemical coordination bonds improve the dispersion and antibacterial effect of bismuth agent.

Benefits of technology

It improves the dispersion and antibacterial effect of the bismuth agent, reduces the mobility of bismuth ions, achieves long-lasting antibacterial properties and promotes wound healing, avoids secondary wound injuries, and has the advantages of low toxicity and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118557773B_ABST
    Figure CN118557773B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of biomedical materials. The present invention relates to a bismuth-containing functional auxiliary agent and an antibacterial and healing-promoting bismuth-containing dressing and a preparation method thereof, wherein the dressing comprises gauze and an effective component. The effective component is 75-85 parts of vaseline; 9-19 parts of liquid paraffin; 5-10 parts of glycerol; and 0.5-10 parts of a bismuth-containing functional auxiliary agent as raw materials, and the total mass of the vaseline, liquid paraffin, and glycerol is 100 parts; and a dressing is obtained through a mixing pulping and coating process. The preparation of the novel antibacterial and healing-promoting bismuth-containing dressing not only effectively solves the problems of poor dispersibility or sudden release defects during use of bismuth tribromophenate, and poor long-term antibacterial properties, but also has the effects of absorbing exudate, moisturizing, and avoiding secondary injuries to the wound surface, etc., and the material can be widely used in various medical materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a bismuth-containing functional auxiliary agent and an antibacterial and healing-promoting bismuth-containing dressing and a preparation method thereof. The invention belongs to the field of biomedical materials. Background Art

[0002] In clinical practice, some infectious or chronic wounds will have exudate, and medical staff usually choose vaseline gauze dressings for covering and care, such as burn wounds, anorectal surgery wounds, pressure sores, and donor site wounds. This type of dressing has the ability to prevent gauze from adhering to the wound due to its oily ingredients, avoid secondary damage to the wound during dressing changes, and is conducive to the growth of fresh granulation tissue.

[0003] However, the healing time of such chronic wounds or infected wounds is usually relatively long. The oily coating of traditional vaseline dressings is hydrophobic, which prevents the exudate from the wound from being discharged, affecting the healing efficiency. In addition, the wound is directly exposed to the outside world, and high and long-term antibacterial properties are also basic requirements for dressings.

[0004] With the diversification of demand, antibacterial burn wound dressings have attracted more and more attention. Commonly used antibacterial dressings include silver-based dressings, bismuth-based dressings, etc. Silver-based dressings have many advantages such as excellent antibacterial and reduced inflammation, but they also have high costs, long-term use of drug resistance and the risk of silver poisoning. Although rare, excessive exposure to silver ions does lead to silver poisoning (silver deposition disease) and other defects; relatively speaking, bismuth is considered to be one of the least toxic heavy metals. Compared with silver, bismuth-based low toxicity and avoidance of drug resistance are more suitable for in vivo application (Research Progress of Bismuth-based Nanomaterials in the Field of Antibacterial (DOI: 10.13523 / j.cb.2308011)). As one of the bismuth-based compounds, vaseline dressings with bismuth tribromophenate as an antibacterial agent have been widely proven to have low cost, ease of use and low infection rate, and bismuth can effectively inhibit bacterial proliferation and accelerate wound healing. The existing bismuth tribromophenate vaseline dressing is obtained by coating vaseline containing bismuth tribromophenate on a substrate such as non-woven fabric, and has good antibacterial and therapeutic effects. However, bismuth tribromophenate is difficult to effectively disperse in water and common organic solvents, and bismuth compounds are prone to sudden release during use. A large amount of bismuth falls off and accumulates in the skin tissue, further entering the blood, and accumulating in human tissues or organs, which is prone to risks. In addition, the sharp decrease in the bismuth content in the dressing after the sudden release will affect the long-term antibacterial effect of the dressing. Summary of the invention

[0005] The purpose of the present invention is to provide a novel antibacterial and healing-promoting bismuth-containing dressing and its preparation method in view of the problems of poor dispersibility or burst release defects during use and poor long-term antibacterial properties of bismuth tribromophenate dressings in the prior art. The present invention uses a homemade bismuth-containing functional auxiliary agent and vaseline, liquid paraffin, and glycerin as raw materials, and obtains an antibacterial and healing-promoting bismuth-containing dressing through a blending and coating process. While solving the problems of the prior art, it also has the effects of absorbing exudate, moisturizing and avoiding secondary injury to the wound surface, etc. The material can be widely used in various medical materials. The technical solution adopted by the present invention to solve its technical problems is:

[0006] The present invention provides a method for preparing a bismuth-containing functional additive, comprising the following steps:

[0007] S11, adding zeolite into a salt solution to perform an ion exchange reaction to obtain an intermediate product I;

[0008] S12, performing coordination reaction on the intermediate product I and the organic ligand to obtain an intermediate product II;

[0009] S13, subjecting the intermediate product II and the bismuth agent to a coordination reaction to obtain a bismuth-containing functional auxiliary agent, i.e., the target product.

[0010] Furthermore, the usage ratio of the zeolite and the salt solution is 10 g: 100-200 mL; and

[0011] The salt solution is calcium salt or iron salt and has a concentration of 1.0-3.0 mol / L.

[0012] Furthermore, the mesh size of the zeolite is 200-400 meshes.

[0013] Furthermore, the usage ratio of the intermediate product I and the organic ligand solution is 10 g: 100-500 mL; and

[0014] The organic ligand is a multidentate ligand and has a concentration of 1.0-3.0 mol / L.

[0015] Furthermore, the multidentate ligand is a polycarboxyl structure, a polyamino structure or an aminocarboxyl structure.

[0016] Furthermore, the usage ratio of the intermediate product II and the bismuth agent is 10g:0.5-8.0g.

[0017] Furthermore, the bismuth agent is bismuth tribromophenate.

[0018] Another object of the present invention is to provide a bismuth-containing functional auxiliary agent prepared by the above-mentioned method for preparing a bismuth-containing functional auxiliary agent.

[0019] Another object of the present invention is to provide an antibacterial and healing-promoting bismuth-containing dressing, comprising gauze and an effective ingredient, wherein the effective ingredient is as follows in parts by weight:

[0020] 75-85 parts of Vaseline;

[0021] 9-19 parts of liquid paraffin;

[0022] Glycerin 5-10 parts;

[0023] 0.5-10 parts of the above-mentioned bismuth-containing functional additive;

[0024] The total mass of the vaseline, the liquid paraffin and the glycerin is 100 parts.

[0025] Another object of the present invention is to provide a method for preparing the antibacterial and healing-promoting bismuth-containing dressing as described above, comprising the following steps:

[0026] S21, mixing vaseline, liquid paraffin, glycerin and bismuth-containing functional additive uniformly to obtain a mixed slurry for standby use;

[0027] S22, applying the mixed slurry obtained in step S21 on gauze, with the coating amount being 150-300 g per square meter of gauze;

[0028] S23, after coating is completed, the gauze is folded to obtain an antibacterial and healing-promoting bismuth-containing dressing.

[0029] Beneficial effects of the present invention:

[0030] (1) The present invention provides an antibacterial and healing-promoting bismuth-containing dressing, which uses a homemade bismuth-containing functional auxiliary agent as a raw material. The zeolite is used as a carrier and contains metal ions, organic ligand structures, and tribromophenate bismuth. First, tribromophenate bismuth has excellent antibacterial and anti-inflammatory properties; second, the bismuth agent uses zeolite as a carrier, and the porous structure of zeolite forms a large specific surface area, which can greatly improve the antibacterial effect of the bismuth agent; third, the bismuth agent and zeolite are connected by a chemical coordination bond, which can effectively improve the dispersibility of the bismuth agent and improve the performance of the bismuth agent; on the other hand, the zeolite anchors the bismuth agent, and the bismuth ions are not easy to fall off, which has long-lasting antibacterial properties. Fourth, the porous structure of zeolite can effectively absorb wound exudate and accelerate wound healing; fifth, the metal ions (mainly calcium ions or iron ions) enriched on the surface of zeolite have a rapid response coagulation effect after contact with blood, further accelerating wound healing.

[0031] (2) The present invention provides an antibacterial and healing-promoting bismuth-containing dressing, which uses homemade bismuth-containing functional additives, vaseline, liquid paraffin, and glycerol as raw materials. First, the oily coating with vaseline and liquid paraffin as the main body can soften the skin and wound surface, avoiding secondary damage when the dressing is removed after the wound surface heals; second, glycerol has excellent water solubility and excellent compatibility among the main components. It can be used as a transmission channel for exudate, and the exudate from the wound surface is introduced into the zeolite structure of the bismuth-containing functional additive, accelerating the scab of the wound surface and promoting healing; third, the bismuth-containing functional additive uses zeolite as a carrier, and the porous structure of zeolite and after being modified with organic ligands, it has excellent dispersibility in the matrix, and at the same time has good compatibility with each component, no migration and precipitation, and has long-lasting antibacterial and anti-inflammatory and healing-promoting functions; at the same time, bismuth tribromophenate has a unique smell, which can cover the stench of the wound and has a wider range of applications.

[0032] (3) The present invention provides a method for preparing an antibacterial and healing-promoting bismuth-containing dressing. On the one hand, the folding process is adopted, which can be used in large wound scenarios to improve production efficiency and dressing quality; on the other hand, the production process is simple, low-cost, and reduces environmental pollution. It is an economical, environmentally friendly and practical medical dressing. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0034] Figure 1 is the infrared spectrum of the intermediate product I in Example 1 of the present invention;

[0035] Figure 2 is the infrared spectrum of the intermediate product II in Example 1 of the present invention;

[0036] Figure 3 It is the infrared spectrum of the bismuth-containing functional additive in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0038] The purpose of the present invention is to develop a novel vaseline gauze dressing with excellent dispersibility of bismuth tribromophenate, no burst release, long-lasting antibacterial property and healing promotion in view of the shortcomings of existing bismuth-containing vaseline gauze dressings. The idea of ​​realization is: combining the characteristics of the coordination of bismuth tribromophenate, coordinating it with an organic ligand to improve its solubility; at the same time, using the porous structure of zeolite, anchoring bismuth tribromophenate to reduce its release mobility in the dressing. The theoretical basis of realization is: first, ion exchange is carried out through zeolite, a large amount of metal ions are enriched on the surface of zeolite, and a hanging structure is formed after coordination by multi-dentate organic ligands, and coordinated with bismuth tribromophenate. A self-made bismuth-containing functional auxiliary agent is added to the raw material mainly composed of vaseline, and a bismuth-containing dressing for antibacterial and healing promotion is obtained after blending and slurrying. On the one hand, the dispersibility problem of bismuth tribromophenate is solved, and on the other hand, bismuth tribromophenate is anchored on the surface of zeolite for enhanced sustained release; at the same time, the antibacterial function of bismuth tribromophenate and the hemostatic function of zeolite for absorbing exudate are combined, and the exudate is absorbed into the zeolite, and the exudate is sterilized and disinfected by using bismuth tribromophenate as the main component; bismuth tribromophenate, zeolite and organic ligand work synergistically, and have excellent long-term antibacterial and healing-promoting effects. The embodiments of the present invention are as follows:

[0039] The embodiment of the present invention provides a method for preparing a bismuth-containing functional additive, comprising the following steps:

[0040] S11, adding zeolite to a salt solution, reacting at 70-90°C for 3-5h, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out insoluble matter, washing with deionized water A for 3 times, and drying at 90-100°C for 2-4h to obtain an intermediate product I;

[0041] The dosage ratio of zeolite, salt solution and deionized water A is 10g:100-200mL:500mL;

[0042] The concentration of the salt solution is 1.0-3.0 mol / L.

[0043] The mesh number of zeolite is 200-400 mesh, which can be 200 mesh, 325 mesh, 400 mesh, or a range value composed of any two values; it is a micron-sized zeolite structure, and the specification of zeolite is greater than 400 mesh, and the adsorption effect on tribromophenate bismuth is poor; the specification of zeolite is less than 200 mesh, and its specific surface area is relatively low, and the adsorption and synergistic effect on tribromophenate bismuth is reduced, and a "foreign body sensation" may appear in the dressing.

[0044] In addition, a more important point is that nano-scale medical devices are easily engulfed by human cells during use in the body, aggregated in tissues or organs, and cause toxic reactions; and the particle size of the zeolite carrier used in the present invention is micron-level, which can effectively avoid the problems existing in nano-scale materials while ensuring that the loaded tribromophenate bismuth improves the antibacterial property.

[0045] The zeolite in the following embodiments of the present invention is zeolite powder purchased from Hebei Runhuabang New Material Technology Co., Ltd.

[0046] The salt solution is a calcium salt or an iron salt;

[0047] The calcium salt is calcium chloride, calcium nitrate, etc.; and, unless otherwise specified, the calcium salt in the following embodiments and comparative examples of the present invention is calcium chloride;

[0048] The iron salt is ferric chloride, ferric sulfate, ferric nitrate, etc.; and, unless otherwise specified, the iron salt in the following embodiments and comparative examples of the present invention is ferric chloride.

[0049] S12, adding the intermediate product I to the organic ligand solution, stirring and shaking at 20-30° C. for 4-6 hours, filtering and taking out the insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 hours to obtain the intermediate product II;

[0050] The usage ratio of intermediate product I, organic ligand solution and deionized water B is 10 g: 100-500 mL: 500 mL;

[0051] The concentration of the organic ligand solution is 1.0-3.0 mol / L.

[0052] The organic ligand is a multidentate ligand;

[0053] The multidentate ligand is a multi-carboxyl structure, a multi-amino structure or an aminocarboxyl structure; and the number of C atoms in the main chain is preferably 4-10. It acts as a reaction "bridge". If the number of C atoms is greater than 10, it will form a coordination with the same metal ion, forming a closed structure and cannot participate in the next reaction; if the number of C atoms is less than 4, it will affect its coordination efficiency with tribromophenate bismuth in the next step.

[0054] The polycarboxyl structure may be an aliphatic polycarboxyl structure, an alicyclic polycarboxyl structure or an aromatic polycarboxyl structure;

[0055] The aliphatic polycarboxyl structure may be glutaric acid, adipic acid, suberic acid, sebacic acid, malic acid, tartaric acid, citric acid or butanetetracarboxylic acid, etc.;

[0056] The alicyclic polycarboxyl structure may be 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid or cyclohexane-1,2,4,5-tetracarboxylic acid, etc.;

[0057] The aromatic polycarboxyl structure may be phthalic acid, isophthalic acid, terephthalic acid, 1,2,4-benzenetricarboxylic acid, 1,2,3-benzenetricarboxylic acid or pyromellitic acid, etc.;

[0058] The polyamino structure may be a polyamide structure, a polyguanidine structure, an amino-amide structure or an amino-guanidine structure;

[0059] The polyamide structure can be succinamide, adipamide, etc.;

[0060] The polyguanidine structure may be biguanide octylamine triacetate, polyhexamethylene biguanide hydrochloride, etc.;

[0061] The amino-amide structure can be aminobutanamide, etc.;

[0062] The amino-guanidine structure may be agmatine, etc.;

[0063] The aminocarboxyl structure is a commonly used amino acid structure, which may be arginine, lysine, serine, glutamic acid, isoleucine, phenylalanine, and the like.

[0064] S13, grind the bismuth agent and add it to tetrahydrofuran, perform ultrasonic oscillation, add the intermediate product II, heat to 25-60°C and stir for 4-6 hours, filter, take out the insoluble matter, wash it with eluent 3 times, wash it with deionized water C 3 times, and dry it at 60°C for 8 hours to obtain a bismuth-containing functional auxiliary agent, i.e., the target product.

[0065] The dosage ratio of the intermediate product II, the bismuth agent, tetrahydrofuran, the eluent, and the deionized water C is 10 g: 0.5-8.0 g: 500 mL: 600 mL: 600 mL.

[0066] The bismuth agent is bismuth tribromophenate; the particle size is 2-4 μm.

[0067] Bismuth tribromophenate is blended with vaseline at a mass ratio of 1:10 and then ground, and the desired particle size is obtained by testing with a laser particle size analyzer.

[0068] The eluent in the following examples of the present invention is a tetrahydrofuran solution of stearic acid with a concentration of 1.0 mol / L.

[0069] Unless otherwise specified in the following embodiments of the present invention, the solvent of the organic ligand solution is water or a co-solvent of water and N,N-dimethylformamide, for the purpose of dissolving the solute; and water is preferably used as the solvent.

[0070] In the bismuth-containing functional auxiliary agent and the preparation method thereof of the present invention: in step S11, zeolite and salt solution (calcium salt or iron salt) are used as starting materials; the salt ions in the salt solution are used as the connection site for the next reaction on the one hand, and also as a wound hemostatic agent on the other hand to accelerate the wound scab healing. In step S12, an organic ligand is used as a reaction "bridge" to connect the tribromophenol bismuth structure. In addition, the organic ligand can be selected for antibacterial properties, such as amino acid structure and guanidine structure, which have good antibacterial properties, and guanidine has better coordination with bismuth. In step S13, the organic ligand is coordinated with tribromophenol bismuth to solve the problem that tribromophenol bismuth is difficult to dissolve and disperse in conventional solvents, and is dispersed on the surface of zeolite to form a large specific surface area and improve the antibacterial performance; in addition, according to the theory of hard and soft acid-base, bismuth ions belong to soft acids, phenols belong to soft bases, and amino ions and carboxylic acid ions belong to hard bases. According to the rule of hard-hard and soft-soft, the coordination of the organic ligand will not displace phenol, which can ensure the integrity of tribromophenol bismuth.

[0071] The embodiment of the present invention provides an antibacterial and healing-promoting bismuth-containing dressing, comprising gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0072] 75-85 parts of Vaseline;

[0073] 9-19 parts of liquid paraffin;

[0074] Glycerin 5-10 parts;

[0075] 0.5-10 parts of the above-mentioned bismuth-containing functional additive;

[0076] The total mass of vaseline, liquid paraffin and glycerin is 100 parts.

[0077] The gauze can be non-woven fabric, warp knitted fabric, Nile gauze or webbing; and the gauze in the following embodiments is non-woven fabric.

[0078] The vaseline in the following embodiments of the present invention is commercially available pharmaceutical grade white vaseline, and the present invention does not make any special requirements.

[0079] The liquid paraffin in the following embodiments of the present invention can be selected from pharmaceutical grade liquid paraffin available on the market, and the present invention does not make any special requirements.

[0080] The glycerol in the following embodiments of the present invention may be of conventional pharmaceutical grade, and the present invention does not make any special requirements.

[0081] The present invention provides a method for preparing an antibacterial and healing-promoting bismuth-containing dressing, comprising the following steps:

[0082] S21, mixing vaseline, liquid paraffin, glycerin and bismuth-containing functional additives in proportion, degassing and setting aside;

[0083] S22, adding the mixed slurry obtained in S21 into a coating machine, and impregnating the gauze with the coating slurry, with a coating amount of 150-300 g per square meter of gauze;

[0084] S23, after coating is completed, the gauze is folded into an "accordion" shape to obtain an antibacterial and healing-promoting bismuth-containing dressing.

[0085] In order to further understand the present invention, an antibacterial and healing-promoting bismuth-containing dressing provided by the present invention is described in detail below in conjunction with specific embodiments, and the protection scope of the present invention is not limited by the following embodiments. Example 1

[0086] A method for preparing a bismuth-containing functional additive comprises the following steps:

[0087] S11, adding zeolite to the calcium salt solution, reacting at 80°C for 4 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out the insoluble matter, washing it with deionized water A for 3 times, and drying it at 95°C for 3.5 hours to obtain an intermediate product I;

[0088] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0089] The concentration of the calcium salt solution is 2.0 mol / L.

[0090] The mesh number of zeolite is 325 mesh.

[0091] See also Figure 1 As shown, its infrared data are as follows: 3441 cm-1: the presence of -OH broad peak; 1048 cm-1: the presence of -Si-O-Si-; 794 cm-1, 724 cm-1: silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-; 899 cm-1: the presence of Ca-O.

[0092] S12, adding the intermediate product I to the arginine solution, stirring and shaking at 30°C for 5 hours, filtering and taking the insoluble matter; washing with deionized water B for 3 times, and drying at 60°C for 8 hours to obtain the intermediate product II;

[0093] The usage ratio of intermediate product I, arginine solution, and deionized water B is 10 g: 300 mL: 500 mL;

[0094] The concentration of the arginine solution was 2.0 mol / L.

[0095] See also Figure 2As shown, its infrared data are as follows: 3441 cm-1: the presence of -OH broad peak; 1048 cm-1: the presence of -Si-O-Si-; 794 cm-1, 724 cm-1: silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-; 899 cm-1: the presence of Ca-O; 3281 cm-1: the presence of -NH (coordinated with calcium ions); 1674 cm-1: the presence of -C=O (coordinated with calcium ions); 3312 cm-1: the presence of -NH; 1620 cm-1: the presence of -C=N-.

[0096] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 25°C and stir for 4 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0097] The usage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 4.0 g: 500 mL: 600 mL: 600 mL.

[0098] See also Figure 3 As shown, its infrared data are as follows: 3441cm-1: -OH broad peak exists; 1048cm-1: -Si-O-Si- exists; 794cm-1, 724cm-1: silicon oxygen tetrahedron -Si-O-Si-, aluminum oxygen octahedron -Al-O-Si-; 899 cm-1: Ca-O exists; 3280-3290 cm-1: -NH (coordinated with calcium ions) exists; 1674 cm-1: -C=O (coordinated with calcium ions) exists; 3312cm-1: -NH exists; 1603 cm-1: -C=N- (coordinated with bismuth ions) exists; 3011 cm-1: benzene ring -CH exists; 1495cm-1, 1591cm-1: benzene ring exists.

[0099] This embodiment provides an antibacterial and healing-promoting bismuth-containing dressing, comprising gauze and effective ingredients, which are as follows in parts by weight:

[0100] Vaseline 80 parts;

[0101] 14 parts of liquid paraffin;

[0102] 6 parts of glycerol;

[0103] Contains 3 parts of bismuth functional additive.

[0104] The preparation method of the antibacterial and healing-promoting bismuth-containing dressing comprises the following steps:

[0105] S21, mixing vaseline, liquid paraffin, glycerin and bismuth-containing functional additives in proportion, degassing and setting aside;

[0106] S22, adding the mixed slurry obtained in S21 into a coating machine, and impregnating the gauze with the coating slurry, with a coating amount of 200 g per square meter of gauze;

[0107] S23, after coating is completed, the gauze is folded into an "accordion" shape to obtain an antibacterial and healing-promoting bismuth-containing dressing. Example 2

[0108] The rest is the same as in Example 1, except that:

[0109] A method for preparing a bismuth-containing functional additive comprises the following steps:

[0110] S11, adding zeolite to a calcium salt solution, reacting at 70°C for 5 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out insoluble matter, washing with deionized water A for 3 times, and drying at 90°C for 4 hours to obtain an intermediate product I;

[0111] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:100mL:500mL;

[0112] The concentration of the calcium salt solution is 3.0 mol / L.

[0113] The mesh number of zeolite is 200 mesh.

[0114] S12, adding the intermediate product I to the arginine solution, stirring and shaking at 20° C. for 6 h, filtering and taking the insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 h to obtain the intermediate product II;

[0115] The usage ratio of intermediate product I, arginine solution, and deionized water B is 10 g: 200 mL: 500 mL;

[0116] The concentration of the arginine solution was 3.0 mol / L.

[0117] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 25°C and stir for 4 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0118] The usage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 4.0 g: 500 mL: 600 mL: 600 mL. Example 3

[0119] The rest is the same as in Example 1, except that:

[0120] A method for preparing a bismuth-containing functional additive comprises the following steps:

[0121] S11, adding zeolite to a calcium salt solution, reacting at 90°C for 3 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking insoluble matter, washing with deionized water A for 3 times, and drying at 100°C for 2 hours to obtain an intermediate product I;

[0122] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g: 200mL: 500mL;

[0123] The concentration of the calcium salt solution is 1.5 mol / L.

[0124] The mesh number of zeolite is 400 mesh.

[0125] S12, adding the intermediate product I to the arginine solution, stirring and shaking at 30°C for 4 hours, filtering and taking out the insoluble matter; washing with deionized water B for 3 times, and drying at 60°C for 8 hours to obtain the intermediate product II;

[0126] The usage ratio of intermediate product I, arginine solution, and deionized water B is 10 g: 400 mL: 500 mL;

[0127] The concentration of the arginine solution is 1.5 mol / L.

[0128] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 25°C and stir for 4 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0129] The usage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 4.0 g: 500 mL: 600 mL: 600 mL. Example 4

[0130] The rest is the same as in Example 1, except that:

[0131] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0132] The concentration of the calcium salt solution is 1.0 mol / L. Example 5

[0133] The rest is the same as in Example 1, except that:

[0134] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0135] The concentration of the calcium salt solution is 3.0 mol / L. Example 6

[0136] The rest is the same as in Example 1, except that:

[0137] Replace calcium salts with iron salts. Example 7

[0138] The rest is the same as in Example 1, except that:

[0139] S11, adding zeolite to the calcium salt solution, reacting at 80°C for 4 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out the insoluble matter, washing it with deionized water A for 3 times, and drying it at 95°C for 3.5 hours to obtain an intermediate product I;

[0140] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0141] The concentration of the calcium salt solution is 2.0 mol / L.

[0142] The mesh number of zeolite is 325 mesh.

[0143] S12, adding the intermediate product I to the adipic acid solution, stirring and shaking at 30° C. for 5 h, filtering and taking out the insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 h to obtain the intermediate product II;

[0144] The usage ratio of intermediate product I, adipic acid solution, and deionized water B is 10 g: 400 mL: 500 mL;

[0145] The concentration of the adipic acid solution was 2.0 mol / L.

[0146] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 60°C and stir for 5 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0147] The usage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 8.0 g: 500 mL: 600 mL: 600 mL. Example 8

[0148] The rest is the same as in Example 1, except that:

[0149] S11, adding zeolite to the calcium salt solution, reacting at 80°C for 4 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out the insoluble matter, washing it with deionized water A for 3 times, and drying it at 95°C for 3.5 hours to obtain an intermediate product I;

[0150] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0151] The concentration of the calcium salt solution is 2.0 mol / L.

[0152] The mesh number of zeolite is 325 mesh.

[0153] S12, adding the intermediate product I to the biguanide octylamine triacetate solution, stirring and shaking at 30° C. for 5 h, filtering and taking the insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 h to obtain the intermediate product II;

[0154] The usage ratio of the intermediate product I, the biguanide octylamine triacetate solution, and the deionized water B is 10 g: 100 mL: 500 mL;

[0155] The concentration of the octylamine triacetate solution is 3.0 mol / L.

[0156] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 25°C and stir for 4 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0157] The dosage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 0.5 g: 500 mL: 600 mL: 600 mL. Example 9

[0158] The rest is the same as in Example 1, except that:

[0159] S11, adding zeolite to the calcium salt solution, reacting at 80°C for 4 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out the insoluble matter, washing it with deionized water A for 3 times, and drying it at 95°C for 3.5 hours to obtain an intermediate product I;

[0160] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0161] The concentration of the calcium salt solution is 2.0 mol / L.

[0162] The mesh number of zeolite is 325 mesh.

[0163] S12, adding the intermediate product I to the aminobutanamide solution, stirring and shaking at 30° C. for 4 h, filtering and taking out the insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 h to obtain the intermediate product II;

[0164] The usage ratio of intermediate product I, aminobutanamide solution, and deionized water B is 10 g: 500 mL: 500 mL;

[0165] The concentration of the aminobutanamide solution is 1.0 mol / L.

[0166] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 60°C and stir for 6 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0167] The dosage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 3.0 g: 500 mL: 600 mL: 600 mL. Example 10

[0168] The rest is the same as in Example 1, except that:

[0169] S11, adding zeolite to the calcium salt solution, reacting at 80°C for 4 hours, cooling to room temperature, centrifuging in a centrifuge, filtering, taking out the insoluble matter, washing it with deionized water A for 3 times, and drying it at 95°C for 3.5 hours to obtain an intermediate product I;

[0170] The dosage ratio of zeolite, calcium salt solution: deionized water A is 10g:150mL:500mL;

[0171] The concentration of the calcium salt solution is 2.0 mol / L.

[0172] The mesh number of zeolite is 325 mesh.

[0173] S12, adding the intermediate product I to the agmatine solution, stirring and shaking at 30° C. for 5 h, filtering and taking the insoluble matter; washing with deionized water B for 3 times, and drying at 60° C. for 8 h to obtain the intermediate product II;

[0174] The usage ratio of intermediate product I, agmatine solution, and deionized water B is 10 g: 300 mL: 500 mL;

[0175] The concentration of the agmatine solution is 2.0 mol / L.

[0176] S13, grind bismuth tribromophenate and add it to tetrahydrofuran, perform ultrasonic oscillation, add intermediate product II, heat to 25°C and stir for 5 hours, filter, take insoluble matter, wash with eluent 3 times, wash with deionized water C 3 times, dry at 60°C for 8 hours, and obtain bismuth-containing functional auxiliary agent, i.e., target product.

[0177] The dosage ratio of the intermediate product II, bismuth tribromophenate, tetrahydrofuran, eluent, and deionized water C is 10 g: 6.0 g: 500 mL: 600 mL: 600 mL. Embodiment 11

[0178] The rest is the same as in Example 1, except that:

[0179] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0180] Vaseline 85 parts;

[0181] 9 parts of liquid paraffin;

[0182] 6 parts of glycerol;

[0183] Contains 5 parts of bismuth functional additive. Example 12

[0184] The rest is the same as in Example 1, except that:

[0185] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0186] Vaseline 75 parts;

[0187] 19 parts of liquid paraffin;

[0188] 6 parts of glycerol;

[0189] Contains 1 part of bismuth functional additive. Embodiment 13

[0190] The rest is the same as in Example 1, except that:

[0191] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0192] Vaseline 80 parts;

[0193] 15 parts of liquid paraffin;

[0194] Glycerin 5 parts;

[0195] Contains 0.5 parts of bismuth functional additive. Embodiment 14

[0196] The rest is the same as in Example 1, except that:

[0197] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0198] Vaseline 80 parts;

[0199] 10 parts of liquid paraffin;

[0200] Glycerin 10 parts;

[0201] Contains 10 parts of bismuth functional additive. Embodiment 15

[0202] The rest is the same as in Example 1, except that:

[0203] The coating amount of gauze per square meter in S22 is 150g. Example 16

[0204] The rest is the same as in Example 1, except that:

[0205] The coating amount of gauze per square meter in S22 is 300g.

[0206] The antibacterial and healing-promoting bismuth-containing dressings of comparative examples 1-11 were compared with example 1: Comparative Example 1

[0207] The rest is the same as in Example 1, except that:

[0208] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0209] Vaseline 80 parts;

[0210] 14 parts of liquid paraffin;

[0211] 6 parts of glycerol. Comparative Example 2

[0212] The rest is the same as in Example 1, except that:

[0213] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0214] Vaseline 80 parts;

[0215] 14 parts of liquid paraffin;

[0216] 6 parts of glycerol;

[0217] 3 parts of bismuth tribromophenate. Comparative Example 3

[0218] The rest is the same as in Example 1, except that:

[0219] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0220] Vaseline 80 parts;

[0221] 14 parts of liquid paraffin;

[0222] 6 parts of glycerol;

[0223] 3 parts of zeolite. Comparative Example 4

[0224] The rest is the same as in Example 1, except that:

[0225] A method for preparing a bismuth-containing functional additive is as follows

[0226] After grinding bismuth tribromophenate, add it to tetrahydrofuran, perform ultrasonic oscillation, add zeolite, heat to 25°C and stir for 4 hours, filter, take insoluble matter, wash it with eluent 3 times, wash it with deionized water 3 times, and dry it at 60°C for 8 hours to obtain a bismuth-containing functional auxiliary agent, i.e., the target product.

[0227] The dosage ratio of zeolite, bismuth tribromophenate, tetrahydrofuran, eluent and deionized water is 10g:4.0g:500mL:600mL:600mL. Comparative Example 5

[0228] The rest is the same as in Example 1, except that:

[0229] The arginine solution was replaced with oxalic acid solution. Comparative Example 6

[0230] The rest is the same as in Example 1, except that:

[0231] The arginine solution was replaced with dodecanedioic acid solution. Comparative Example 7

[0232] The rest is the same as in Example 1, except that:

[0233] The arginine solution was replaced with lysine solution. Comparative Example 8

[0234] The rest is the same as in Example 1, except that:

[0235] The bismuth tribromophenate was replaced with bismuth nitrate. Comparative Example 9

[0236] The rest is the same as in Example 1, except that:

[0237] The bismuth tribromophenate was replaced with bismuth citrate. Comparative Example 10

[0238] The rest is the same as in Example 1, except that:

[0239] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0240] Vaseline 80 parts;

[0241] 14 parts of liquid paraffin;

[0242] Contains 3 parts of bismuth functional additive. Comparative Example 11

[0243] The rest is the same as in Example 1, except that:

[0244] An antibacterial and healing-promoting bismuth-containing dressing comprises gauze and effective ingredients, wherein the effective ingredients are as follows in parts by weight:

[0245] Vaseline 80 parts;

[0246] 14 parts of liquid paraffin.

[0247] The physical properties of the antibacterial and healing-promoting bismuth-containing dressings prepared in Examples 1-16 of the present invention and Comparative Examples 1-11 were measured respectively, and the results are shown in Table 1.

[0248] .

[0249] First, it can be seen from Examples 1-16 in Table 1 that the antibacterial and healing-promoting bismuth-containing dressing of the present invention has low bismuth ion mobility, rapid hemostasis, high efficiency (long-lasting) antibacterial properties and the effect of promoting wound healing.

[0250] Second, it can be observed from Example 1 and Comparative Examples 1-4 that the zeolite and bismuth tribromophenate in the bismuth-containing functional auxiliary agent in the antibacterial and healing-promoting bismuth-containing dressing of the present invention have a synergistic effect on low bismuth ion mobility, rapid hemostasis, high-efficiency (long-acting) antibacterial property and the effect of promoting wound healing; in addition, relative to physical blending, chemical modification has better performance; it can be observed from Example 1 and Comparative Examples 5-6 that the appropriate carbon chain length of the organic ligand in the bismuth-containing functional auxiliary agent has a positive effect on the coordination effect, which can reduce the mobility of bismuth tribromophenate; it can be observed from Example 1 and Comparative Examples 7-9 that the bismuth-containing functional auxiliary agent There is a compatibility relationship between the bismuth agent and the organic ligand. The guanidine group in arginine is a soft base structure, lysine is a hard base structure, and the bismuth ion is a soft acid structure, so the coordination effect of arginine and tribromophenate bismuth is better; bismuth nitrate and bismuth citrate will have the problem of guanidine group replacing nitrate and citric acid structure; at the same time, the phenol group in tribromophenate bismuth can destroy the cell wall and cell membrane of bacteria and has certain antibacterial properties, so arginine and tribromophenate bismuth coordination have better antibacterial properties; from Example 1 and Comparative Examples 1 and 10-11, it can be observed that the bismuth-containing functional auxiliary agent has excellent antibacterial and healing-promoting effects and glycerol has a positive effect on absorption, penetration and healing.

[0251] In summary, the antibacterial and healing-promoting bismuth-containing dressing of the present invention has low bismuth ion mobility, rapid hemostasis, high efficiency (long-lasting) antibacterial properties and the effect of promoting wound healing; in addition, its oily surface can effectively avoid secondary trauma to the wound during replacement, which has great practical significance.

[0252] The test method is as follows:

[0253] (1) Liquid absorption test: Prepare liquid A according to the steps in Part 1 Liquid Absorption of YY / T 0471.1-2004 Test Methods for Contact Wound Dressings for liquid absorption test. The test sample is 5 cm × 5 cm.

[0254] (2) Bismuth ion release test: Liquid A was prepared as the dissolution medium in accordance with the steps in Part 1 of YY / T 0471.1-2004 Test Method for Contact Wound Dressings, Liquid Absorption. 500 ml of Liquid A was injected into a beaker, and then the sample was cut into 50 cm × 50 cm dressings. After removing the release layer, the dressing was placed at the bottom of the beaker with the absorbent layer facing upwards for dissolution test. Since the dressing is generally used for no more than 7 days per piece, the sampling points were set at 1 day, 3 days, 5 days, and 7 days. The bismuth ion dissolution was determined by ICP-MS.

[0255] (3) Antibacterial rate: Tested in accordance with AATCC TM100-2019, test microorganism: Aspergillus brasiliensis (ATCC16404).

[0256] (4) Hemostasis time: 100 rabbits (in good health, weighing 2-3 kg) were divided into 10 groups, with 10 rabbits in each group. A 5 cm × 5 cm area was reserved on the back of the rabbits to remove the dorsal hair. After disinfection, a 1 cm × 1 cm wound was made on the back with a scalpel. The dressings prepared in the examples of the present invention and the comparative examples were cut into a size of 5 cm × 5 cm and applied to the wound surface. The hemostasis of the wound was observed and the hemostasis time was recorded.

[0257] (5) Male Wister rats were used for modeling, with 10 rats in each group. The wound healing status on the 20th day was recorded during the experiment. The specific experimental conditions are as follows:

[0258] a. Depilate the abdomen of male Wister rats 3×3 cm 2 After successful anesthesia, a 3 mm thick, 2 × 3 cm 2 The gauze was immersed in 100°C water, and after the temperature was constant, it was spread on the abdomen of the rat for 10s to form a deep II degree burn wound. After the model was prepared, the dressings of the embodiment group and the comparative example group were respectively used to cover the wound, and then bandaged with a bandage; the wound healing rate was calculated at each sampling point, and a pathological examination was performed to understand the wound healing quality, and the healing time was determined according to the wound healing situation. The test results are shown in the table above;

[0259] b. The wound healing rate is calculated as follows:

[0260] Wound healing rate (%) = (original wound area - unhealed wound area) / original wound area × 100%.

[0261] With the above-mentioned ideal embodiments of the present invention as inspiration, through the above-mentioned description content, relevant personnel can make various changes and modifications without departing from the scope of the technical idea of ​​the present invention.

Claims

1. A method for preparing a bismuth-containing functional additive, characterized in that: The following steps are involved: S11, adding zeolite into a salt solution to perform an ion exchange reaction to obtain an intermediate product I; S12, subjecting the intermediate product I and the organic ligand solution to a coordination reaction to obtain an intermediate product II; S13, subjecting the intermediate product II and the bismuth agent to a coordination reaction to obtain a bismuth-containing functional auxiliary agent, i.e., a target product; The organic ligand solution is a solution of a multidentate ligand and has a concentration of 1.0-3.0 mol / L; The multidentate ligand is a polycarboxyl structure, a polyamino structure or an aminocarboxyl structure; The usage ratio of the zeolite and the salt solution is 10 g: 100-200 mL; and The salt solution is a calcium salt or an iron salt and has a concentration of 1.0-3.0 mol / L; The dosage ratio of the intermediate product I to the organic ligand solution is 10 g: 100-500 mL; The usage ratio of the intermediate product II and the bismuth agent is 10g:0.5-8.0g; The bismuth agent is bismuth tribromophenate.

2. The method for preparing the bismuth-containing functional additive according to claim 1, characterized in that: The mesh number of the zeolite is 200-400 meshes.

3. A bismuth-containing functional additive, characterized in that: The bismuth-containing functional auxiliary agent is prepared by the preparation method of claim 1 or 2.

4. An antibacterial and healing-promoting bismuth-containing dressing, characterized in that: Comprising gauze and effective ingredients, in parts by weight, the effective ingredients are as follows: 75-85 parts of Vaseline; 9-19 parts of liquid paraffin; Glycerin 5-10 parts; 0.5-10 parts of the bismuth-containing functional additive as claimed in claim 3; The total mass of the vaseline, the liquid paraffin and the glycerin is 100 parts.

5. A method for preparing the antibacterial and healing-promoting bismuth-containing dressing as claimed in claim 4, characterized in that: The steps include: S21, mixing vaseline, liquid paraffin, glycerin and bismuth-containing functional additive uniformly to obtain a mixed slurry for standby use; S22, coating the mixed slurry obtained in step S21 on gauze, with the coating amount being 150-300 g per square meter of gauze; S23, after coating, folding the gauze to obtain an antibacterial and healing-promoting bismuth-containing dressing.