A method for grinding and polishing the lip edge of a micro-hemispherical

By adopting integrated grinding and polishing equipment and bonding material filling technology in the microhemisphere lip edge treatment, combined with negative pressure clamping, the edge collapse and thermal stress problems are solved, the Q value and production efficiency of the microhemisphere are improved, and the cost is reduced.

CN118559515BActive Publication Date: 2024-11-05HUNAN 208 ADVANCED TECH CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411035763.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-05
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The prior art has problems of edge collapse, thermal stress residue and high investment costs in the microhemispheric lip edge treatment, which is difficult to meet the requirements of high Q value.

Method used

Point grinding and surface grinding are used to adopt integrated grinding equipment, combining bonded material filling and negative pressure clamping technology to reduce contact compressive stress, avoid collapse and fragmentation, and polish it through diamond resin grinding wheel.

Benefits of technology

Effectively eliminate edge collapse, improve the flatness and Q value of the lip edge, reduce production costs, and ensure the stability and grinding efficiency of the microhemisphere during long-term grinding and polishing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118559515B_ABST
    Figure CN118559515B_ABST
Patent Text Reader

Abstract

The present invention provides a method for grinding and polishing the lip edge of a micro-hemispherical ball, which belongs to the field of preparing a hemispherical resonant gyroscope. The grinding and polishing method comprises the following steps: S1: placing the micro-hemispherical ball upside down on a grinding and polishing integrated device through a clamping mechanism, rotating and / or lifting the clamping mechanism so that the outer circle of the bottom surface of the skirt edge of the micro-hemispherical ball contacts the grinding disk of the grinding and polishing integrated device, and starting the grinding and polishing integrated device to perform point grinding on the skirt edge of the micro-hemispherical ball until the outer diameter of the skirt edge is ground to a set size to form a lip edge; S2: rotating and lifting the clamping mechanism so that the bottom surface of the lip edge of the micro-hemispherical ball contacts the grinding disk of the grinding and polishing integrated device, and starting the grinding and polishing integrated device to perform surface grinding on the lip edge surface of the micro-hemispherical ball. The present invention eliminates the phenomenon of edge collapse during the grinding process of the micro-hemispherical ball, thereby improving the reduction of the Q value of the resonator caused by improper lip grinding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hemispherical resonant gyroscope preparation, and in particular to a micro-hemispherical lip edge grinding and polishing method. Background Art

[0002] Micro-hemisphere is a hemispherical resonant gyroscope. It is a solid wave gyroscope based on the Coriolis effect. It has the advantage of low cost and is an important direction for the development of gyroscopes in the future. Conventional micro-hemispheres are blown into shape using flat quartz sheets. Before becoming finished products for assembly, Figure 1 As shown, it is necessary to remove the excess skirt after molding, and grind and polish the lip edge of the micro-hemispherical with the skirt removed to remove excess mass and form a smooth, non-chipped, uniform lip edge to ensure a high quality factor Q value.

[0003] The commonly used method for processing the lip edge of a micro-hemispherical ball is to first remove the skirt edge by laser cutting or laser ablation, and then use mechanical grinding + polishing to process the lip edge of the micro-hemispherical ball with the skirt removed. However, the laser ablation method is prone to produce a jagged lip edge with a depth of about 2-5um, which cannot meet the requirements of low roughness to maintain a high Q value. The laser cutting edge is prone to microcracks (collapsed edges, etc.), and the residual thermal stress generated by the laser further reduces the Q value of the micro-hemispherical ball. In addition, cutting (or ablation) and polishing are not completed in the same process, repeated replacement of the fixture cannot guarantee the flatness of the product, and it is necessary to invest in two processing equipment, which has a high investment cost. The present invention attempts to design an integrated grinding + polishing device to process the lip edge of the micro-hemispherical ball, that is, mechanically grinding to remove the skirt edge, and then polishing to remove the lip edge of the micro-hemispherical ball with the skirt edge. However, practice shows that the traditional mechanical grinding method mostly uses a diamond grinding wheel for grinding. The diamond grinding wheel is diamond sand electroplated on the metal surface, and the sand grains are unevenly distributed. Long-term grinding makes the grinding wheel pattern of the skirt edge of the micro-hemispherical ball uneven after grinding, and the collapse point is large, which cannot be eliminated by polishing, which will reduce the Q value of the micro-hemispherical ball. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a micro-hemispherical lip edge grinding and polishing method to eliminate the edge collapse phenomenon produced during the micro-hemispherical grinding process, thereby improving the situation in which the resonator Q value is reduced due to improper lip grinding and polishing.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A micro-hemispherical lip edge grinding and polishing method comprises the following steps:

[0007] S1: The micro-hemispherical ball is placed upside down on the grinding and polishing integrated device through a clamping mechanism, and the outer circle of the bottom surface of the skirt of the micro-hemispherical ball is brought into contact with the grinding disk of the grinding and polishing integrated device by rotating and / or lifting the clamping mechanism, and the grinding and polishing integrated device is started to perform point grinding on the skirt of the micro-hemispherical ball until the outer diameter of the skirt is ground to a set size to form a lip edge;

[0008] S2: The bottom surface of the lip edge of the micro-hemispherical ball is made to fit with the grinding disk of the grinding and polishing equipment by rotating and lifting the clamping mechanism, and the grinding and polishing equipment is started to perform surface grinding on the lip edge surface of the micro-hemispherical ball.

[0009] Optionally, the clamping mechanism includes a jig, a mounting hole is formed on the lower end surface of the jig, the upper and middle parts of the inverted micro-hemisphericity extend into the mounting hole, the skirt and lower part of the micro-hemisphericity are exposed outside the mounting hole, a first bonding mixture is filled between the middle part of the outer wall of the micro-hemisphericity and the corresponding inner wall of the mounting hole, other positions of the mounting hole are filled with a second bonding mixture, the micro-hemisphericity is also filled with the first bonding mixture, the adhesion of the second bonding mixture is greater than that of the first bonding mixture, and the micro-hemisphericity is fixedly connected to the jig after the first bonding mixture and the second bonding mixture are cured.

[0010] When mechanical grinding and polishing is used to remove the skirt, an adhesive material is required to bond the micro-hemispherical ball to a jig, and the jig is then fixed to the grinding and polishing equipment through fasteners. Since the skirt grinding process takes a long time, the adhesive material must have good rigidity so that the micro-hemispherical ball does not move relative to the jig during the long grinding and polishing process, and must also have good viscosity so that the micro-hemispherical ball does not crack due to the toughness of the adhesive material during the long grinding and polishing process. In addition, the adhesive material must also have good cleaning properties to ensure that it can be thoroughly cleaned. It is currently difficult to find a suitable adhesive material.

[0011] The present invention fills adhesive material between the micro-hemispherical ball and the jig, and inside the micro-hemispherical ball. Compared with only filling adhesive material between the micro-hemispherical ball and the jig, the present invention can increase the vibration reduction and buffering effects. It can not only ensure that the micro-hemispherical ball does not move relative to the jig during a long period of grinding and polishing, but also prevent the micro-hemispherical ball from cracking due to the toughness of the adhesive material during a long period of grinding and polishing.

[0012] The practice of the present invention further shows that improper selection of bonding materials will also affect the grinding quality. For example, when rosin and asphalt are mixed to fill the space between the micro-hemisphere and the fixture, as well as the interior of the micro-hemisphere, the above substances are easy to adhere to the diamond or resin grinding wheel, making the grinding surface sticky and without cutting force, further damaging the skirt of the micro-hemisphere and reducing the grinding efficiency. In addition, the grinding wheel with bonding materials needs to be further deeply cleaned with alcohol, acetone, gasoline, etc., which affects the electroplating layer and is easy to lose sand.

[0013] The present invention adopts a method of filling a second bonding mixture with greater adhesion between the position of the micro-hemispheric near the shoulder and the jig, and filling a first bonding mixture with less adhesion between the position near the lip edge and the jig, and inside the micro-hemispheric. The second bonding mixture can effectively protect the thinner shoulder from damage and achieve better adhesion performance. The first bonding mixture has three functions: first, it isolates the second bonding mixture from the grinding wheel, second, its filling can protect the micro-hemispheric from breaking during the grinding and polishing process, and third, due to its smaller adhesion, it will not adhere to the grinding wheel and is easy to clean. Therefore, the bonding method of the micro-hemispheric and the jig of the present invention can not only ensure that the micro-hemispheric does not move relative to the jig during long-term grinding and polishing, but also ensure grinding efficiency, avoid micro-hemispheric skirt damage, and facilitate the cleaning of the micro-hemispheric and the grinding tool.

[0014] Optionally, the first bonding mixture includes powder and water, the powder is gypsum powder or dental tray powder, and the mass ratio of the powder to water is 1:1-3:1; the second bonding mixture includes rosin and asphalt, and the mass ratio of the rosin to asphalt is 2:1-4:1.

[0015] The present invention adopts a method of filling a mixture of rosin and asphalt between the position of the micro-hemispherical near the shoulder and the jig, and filling gypsum powder or tooth tray powder between the position near the lip edge and the jig, and inside the micro-hemispherical. The mixture of rosin and asphalt is a relatively soft medium material, which can effectively protect the thinner shoulder from damage and achieve better adhesion performance. Gypsum powder and tooth tray powder are powdery substances, which can protect the micro-hemispherical from breaking during the grinding and polishing process, and will not adhere to the grinding wheel, and have appropriate hardness and are easy to clean. Therefore, the bonding method of the micro-hemispherical and the jig of the present invention can not only ensure that the micro-hemispherical does not move relative to the jig during the long-term grinding and polishing process, but also ensure grinding efficiency, avoid micro-hemispherical skirt damage, and facilitate the cleaning of the micro-hemispherical and the abrasive tool.

[0016] Optionally, assuming that the overall height of the micro-hemisphere is h, and the bottom surface of the skirt of the micro-hemisphere is taken as a reference plane, the filling boundary line between the first bonding mixture and the second bonding mixture is located 1 / 2h-3 / 5h above the reference plane.

[0017] Optionally, the clamping mechanism also includes a clamping assembly, which can be rotatably mounted on a three-axis moving mechanism of the grinding and polishing equipment. The jig is fixed to the bottom of the clamping assembly, and there is an air duct connected to a negative pressure device between the clamping assembly and the jig. The negative pressure device is used to evacuate the air duct to form negative pressure so that the jig is adsorbed on the clamping assembly.

[0018] The present invention connects an external air nozzle to the clamping mechanism so that the tension of the fixture with the micro-hemispherical ball can be strengthened under the negative pressure of the clamping mechanism, thereby preventing the fixture from being skewed during the grinding and polishing process, thereby ensuring the symmetry of the lip edge of the micro-hemispherical ball after grinding and polishing.

[0019] Optionally, after step S2, step S3 is further included: by moving the clamping mechanism, the bottom surface of the lip edge of the micro-hemispherical sphere is made to fit with the polishing disk of the grinding and polishing device, and the grinding and polishing device is started to perform surface polishing on the lip edge surface of the micro-hemispherical sphere.

[0020] Further end face polishing of the lip edge after the skirt is removed and ground can reduce the surface roughness of the lip edge, improve the flatness, and eliminate small chipping points.

[0021] Optionally, the grinding disc is a diamond grinding wheel disc, and the polishing disc is a diamond resin grinding wheel or a cubic boron nitride resin grinding wheel.

[0022] The practice of the present invention shows that polishing with a diamond resin grinding wheel or a cubic boron nitride resin grinding wheel can effectively eliminate the small chipping points generated by grinding the micro-hemispherical lip edge and reduce the surface roughness of the lip edge. In practice, after the skirt edge is generally removed and the surface is ground with a diamond grinding wheel, the micro-hemispherical lip edge is polished with a resin grinding wheel after the height gauge is measured and a processing allowance of 0.2-0.8 mm is reserved.

[0023] Optionally, after step S3, step S4 is further included: softening the first bonding mixture and the second bonding mixture by heating to separate the micro-hemispherical ball from the jig, and cleaning the micro-hemispherical ball to remove the first bonding mixture and the second bonding mixture on the surface of the micro-hemispherical ball.

[0024] After the micro-hemispherical grinding and polishing, it is necessary to clean and remove dirt. Since the shoulder wall thickness of the micro-hemispherical is very thin, the conventional ultrasonic cleaning machine is easy to cause the micro-hemispherical to break during the cleaning process due to the frequency and power. The present invention preferably uses a bubble cleaning machine, and each tank can be filled with different cleaning liquids. During cleaning, the gas is first connected through the air pipe to generate bubbles in the cleaning liquid, resulting in a liquid tumbling effect. The turbulent kinetic energy generated can accelerate the removal of dirt adhered to the micro-hemispherical. The bubble cleaning machine is preferably made of PVC material, and cleaning liquids such as hydrochloric acid, hydrogen peroxide, pure water, and sulfuric acid can be placed in each tank in turn. When cleaning, the micro-hemispherical is transferred to the next cleaning tank for the next step of cleaning. After completing all cleaning steps, it is observed under a microscope. If there is any residue, it is further cleaned.

[0025] Optionally, after step S4, the method further includes step S5: chemically polishing the lip edge surface of the micro-hemispherical ball to remove micro-cracks on the lip edge surface of the micro-hemispherical ball.

[0026] Practice shows that microcracks will appear on the lip edge of the micro-hemispherical ball after grinding. These microcracks are filled with a large number of impurities produced during the mechanical grinding process, which will aggravate the loss of Q value. It is difficult to remove them by mechanical polishing alone. Therefore, chemical treatment is required to remove the damaged layer and impurities on the surface.

[0027] Furthermore, since the shoulder of the micro-hemispherical ball is very thin, the corrosion caused by the acidic substances in the chemical treatment process can easily cause the shoulder and the skirt to fall off from the supporting column as a whole. The present invention raises the micro-hemispherical ball to a suitable height by adding a chemical polishing jig, so that only the lip edge of the micro-hemispherical ball contacts the chemical polishing solution. After the micro-hemispherical ball is left to stand in the chemical polishing solution for 10-30 minutes, the micro-hemispherical ball is taken out for further cleaning to complete the micro-hemispherical ball grinding and polishing treatment.

[0028] Optionally, before step S1, the method further includes: coating the micro-hemispherical body as a whole to form a film layer on the inner and outer walls of the micro-hemispherical body, wherein the film layer includes one of an aluminum film, a copper film or a silver film, and the thickness of the film layer is 20-400 nm;

[0029] The method further includes polishing the micro-hemispherical body to remove the film layer on the surface of the micro-hemispherical body between step S4 and step S5.

[0030] In order to avoid the filling material from leaving residues on the surface of the micro-hemispherical surface after cleaning, the micro-hemispherical surface is first subjected to overall magnetron sputtering coating after the micro-hemispherical surface is hot-formed and before the lip edge is ground and polished. The film layer selected is aluminum film, copper film or silver film, and the film layer is removed after cleaning.

[0031] Compared with the prior art, the advantages of the present invention are:

[0032] The present invention adopts a method of clamping and grinding the skirt edge at a rotating angle to perform point grinding on the skirt edge of the micro-hemispherical ball until the outer diameter of the skirt edge is ground to the size of the lip edge, that is, the skirt edge is removed; then the surface of the lip edge of the micro-hemispherical ball is plane ground, thereby completing the grinding process of the lip edge of the micro-hemispherical ball. Since the grinding process time of the skirt edge accounts for more than 80% of the grinding time of the lip edge of the micro-hemispherical ball, the present invention changes the overall grinding of the skirt edge plane to single-point grinding, thereby reducing the contact pressure stress, avoiding the phenomenon of the micro-hemispherical ball generating a collapse point or even breaking during the polishing process, and improving the situation where the resonator Q value is reduced due to improper grinding of the lip edge. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the blow-molded micro-hemispherical structure, where a) is a longitudinal section diagram and b) is a three-dimensional diagram.

[0034] Figure 2 It is a schematic diagram of the three-dimensional structure of the integrated grinding and polishing equipment used in this embodiment.

[0035] Figure 3 This is a schematic diagram of the main structure of the grinding and polishing equipment used in this embodiment.

[0036] Figure 4 for Figure 3 A local enlarged schematic diagram of point A in the middle.

[0037] Figure 5 It is a schematic diagram of the cross-sectional structure of the clamping mechanism.

[0038] Figure 6 This is a specific implementation flow chart of the micro-hemispherical lip edge grinding and polishing method of this embodiment.

[0039] Figure 7 Schematic diagram of the cross-sectional structure of the micro-hemisphere solidified in the fixture.

[0040] Figure 8 This is a schematic diagram of the state of a micro-hemispherical ball being polished in a polishing fixture.

[0041] Fig. 9 This is a schematic diagram of the explosion state of the micro-hemispherical being chemically polished in a chemical polishing fixture.

[0042] Legend:

[0043] 100. Clamping mechanism; 1. Motor; 2. Rotating shaft; 21. Center axis hole; 3. Hexagon socket screw; 4. Fixture; 41. Mounting hole; 42. Through hole; 5. Plug; 6. Micro hemisphere; 7. First bonding mixture; 8. Second bonding mixture; 9. Vertical plate; 10. Horizontal plate; 11. Auxiliary fixture; 12. Chemical polishing fixture; 200. Three-axis sliding mechanism; 300. Grinding and polishing disc. DETAILED DESCRIPTION

[0044] The present invention is further described below in conjunction with specific preferred embodiments, but the protection scope of the present invention is not limited thereby.

[0045] The micro-hemispherical lip edge grinding and polishing method of this embodiment comprises the following steps:

[0046] 1) The micro-hemispherical body is coated as a whole to form a film layer on the inner and outer walls of the micro-hemispherical body.

[0047] 2) Place the micro-hemispherical ball upside down on the grinding and polishing device through the clamping mechanism, and make the outer circle of the bottom surface of the skirt of the micro-hemispherical ball contact the grinding disk of the grinding and polishing device by rotating and / or lifting the clamping mechanism. Start the grinding and polishing device to perform point grinding on the skirt of the micro-hemispherical ball until the outer diameter of the skirt is ground to the set size to form a lip edge.

[0048] 3) By rotating and lifting the clamping mechanism, the bottom surface of the lip edge of the micro-hemispherical ball is made to fit with the grinding disk of the grinding and polishing equipment, and the grinding and polishing equipment is started to perform surface grinding on the lip edge surface of the micro-hemispherical ball.

[0049] 5) By moving the clamping mechanism, the bottom surface of the lip edge of the micro-hemispherical ball is made to fit with the polishing disk of the grinding and polishing device, and the grinding and polishing device is started to perform surface polishing on the lip edge surface of the micro-hemispherical ball.

[0050] 6) Softening the first bonding mixture and the second bonding mixture by heating to separate the micro-hemispherical ball from the jig, and cleaning the micro-hemispherical ball to remove the first bonding mixture and the second bonding mixture on the surface of the micro-hemispherical ball.

[0051] 7) Polishing the micro-hemisphere to remove the film layer on the surface of the micro-hemisphere.

[0052] 8) Chemically polish the lip surface of the micro-hemispherical ball to remove micro-cracks on the lip surface of the micro-hemispherical ball.

[0053] In this embodiment, the clamping mechanism includes a jig, the lower end surface of the jig is provided with a mounting hole, the upper and middle parts of the inverted micro-hemispheric ball extend into the mounting hole, the skirt and lower part of the micro-hemispheric ball are exposed outside the mounting hole, the middle part of the outer wall of the micro-hemispheric ball and the corresponding inner wall of the mounting hole are filled with a first bonding mixture, the other positions of the mounting hole are filled with a second bonding mixture, the micro-hemispheric ball is also filled with the first bonding mixture, the adhesion of the second bonding mixture is greater than that of the first bonding mixture, and the first bonding mixture and the second bonding mixture are cured to fix the micro-hemispheric ball to the jig.

[0054] In this embodiment, the first bonding mixture includes powder and water, the powder is gypsum powder or dental tray powder, and the mass ratio of the powder to water is 1:1-3:1; the second bonding mixture includes rosin and asphalt, and the mass ratio of the rosin to asphalt is 2:1-4:1.

[0055] In this embodiment, the overall height of the micro-hemisphere is denoted as h, and the bottom surface of the skirt of the micro-hemisphere is taken as a reference plane. The filling boundary line between the first bonding mixture and the second bonding mixture is located 1 / 2h-3 / 5h above the reference plane.

[0056] In this embodiment, the grinding disc is a diamond grinding wheel disc, and the polishing disc is a diamond resin grinding wheel or a cubic boron nitride resin grinding wheel.

[0057] In this embodiment, in step 1), the film layer includes one of an aluminum film, a copper film or a silver film, and the thickness of the film layer is 20-400 nm.

[0058] In this embodiment, the clamping mechanism also includes a clamping assembly, which can be rotatably mounted on the three-axis moving mechanism of the grinding and polishing equipment. The fixture is fixed to the bottom of the clamping assembly, and there is an air duct connected to the negative pressure device between the clamping assembly and the fixture. The negative pressure device is used to evacuate the air duct to form negative pressure so that the fixture is adsorbed on the clamping assembly.

[0059] like Figure 2As shown, the integrated grinding and polishing equipment of this embodiment generally includes a three-axis sliding mechanism 200 and a grinding and polishing disc 300. The grinding and polishing disc 300 includes a coaxially arranged grinding disc and a polishing disc. The workpiece to be ground and polished is mounted on the clamping mechanism 100. The clamping mechanism 100 is mounted on the three-axis sliding mechanism 200. The three-axis sliding mechanism 200 drives the clamping mechanism 100 to move up and down, left and right, and forward and backward so that the workpiece on the clamping mechanism 100 contacts the grinding disc / polishing disc.

[0060] In this embodiment, Figure 2-4 As shown, the clamping mechanism 100 can be rotatably mounted on the three-axis sliding mechanism 200, and the clamping mechanism 100 can rotate in a vertical plane relative to the three-axis sliding mechanism 200. The clamping mechanism 100 rotates and cooperates with the movement of the three-axis sliding mechanism 200 to make the outer circle of the skirt bottom surface of the micro-hemispherical ball contact with the grinding disk of the grinding and polishing equipment, so that the grinding and polishing equipment can perform point grinding on the skirt of the micro-hemispherical ball; or make the bottom surface of the lip edge of the micro-hemispherical ball fit with the grinding disk / polishing disk of the grinding and polishing equipment, so that the grinding and polishing equipment can perform surface grinding / polishing on the lip edge of the micro-hemispherical ball.

[0061] like Figure 5 As shown, the clamping mechanism 100 includes a horizontal plate 10, a vertical plate 9 and a clamping assembly. The vertical plate 9 is rotatably connected to the three-axis sliding mechanism 200. The horizontal plate 10 is horizontally connected to the lower end of the vertical plate 9. The clamping assembly is installed on the horizontal plate 10. The clamping assembly includes a motor 1 and a rotating shaft 2 connected to the motor 1. The fixture 4 is detachably connected to the lower end of the rotating shaft 2. The motor 1 drives the rotating shaft 2 to rotate, thereby driving the micro-hemispherical in the fixture 4 to rotate circumferentially. In addition, the rotating shaft 2 is provided with a central shaft hole 21. The upper end of the central shaft hole 21 is connected to the negative pressure device, and the lower end passes through the bottom surface of the rotating shaft 2 to expose the fixture part, so that the negative pressure device evacuates the central shaft hole 21 to form a negative pressure, so as to firmly adsorb the fixture 4 on the clamping mechanism 100, avoid the fixture 4 from being skewed during the grinding and polishing process, and thus ensure the symmetry of the lip edge of the micro-hemispherical after grinding and polishing.

[0062] Alternatively, a through hole 42 penetrating the fixture 4 is provided on the bottom surface of the mounting hole 41 provided on the lower end surface of the fixture 4, and a central axis hole 21 connecting the through hole 42 and the negative pressure device is provided on the rotating shaft 2, so that the negative pressure device evacuates the channel formed by the through hole 42 and the central axis hole 21 to form a negative pressure to fix the fixture 4 on the clamping mechanism 100. A sealing plug 5 is provided between the channel and the second bonding mixture to prevent the second bonding mixture 8 from being sucked into the negative pressure device. The through hole 42 is provided on the fixture 4, so that the fixture is suitable for the grinding and polishing installation of flat sheets in addition to being used for the grinding and polishing installation of micro-hemispherical sheets.

[0063] refer to Figure 6 The implementation process of this embodiment is described in detail as follows:

[0064] Step 1: Micro-hemispherical thermoforming: A fused quartz sheet is used to thermoform the micro-hemispherical 6 on a micro-hemispherical molding device. The micro-hemispherical 6 has a skirt after molding, and the skirt needs to be removed;

[0065] Step 2: coating the entire micro-hemisphere: placing the micro-hemisphere in a magnetron sputtering coating machine, coating the entire micro-hemisphere 6, and one of aluminum film, copper film or silver film can be selected, and the thickness can be selected from 20-400nm;

[0066] Step 3: Install the plug 5 on the fixture 4, and then bond the micro-hemispherical ball to the set position in the fixture 4 with a mixture of rosin and asphalt (i.e., the second bonding mixture 8), wherein the rosin and asphalt mixture ratio is between 2:1 and 4:1. The plug 5 is used for sealing, helping the fixture 4 to form a negative pressure with the grinding and polishing equipment, preventing the fixture 4 from tilting during the grinding and polishing process, and improving the symmetry of the micro-hemispherical ball after grinding and polishing; wherein the fixture 4 is initially fastened to the rotating shaft 2 of the clamping mechanism by the hexagon socket screw 3, and then connected to the grinding and polishing equipment;

[0067] Step 4: Fill the first bonding mixture 7 (a mixture of gypsum powder or tooth tray powder and water) in the remaining tiny gap area between the outer wall of the micro-hemispherical 6 and the fixture 4 to isolate the mixture of rosin and asphalt from the outside world to prevent the above mixture from adhering to the grinding wheel and causing a decrease in the grinding efficiency of the grinding wheel; at the same time, fill the entire inner spherical surface of the micro-hemispherical 6 with gypsum powder or tooth tray powder to protect the micro-hemispherical 6 from breaking during the grinding and polishing process; in this process, the gypsum powder or tooth tray powder needs to be mixed and diluted with water before filling, and the dilution ratio can be selected between 1:1 and 3:1. During the filling process of the outer spherical surface, the filler in step 3 needs to be filled to a height of 1 / 2 to 3 / 5 of the micro-hemispherical from the skirt (that is, with the bottom surface of the micro-hemispherical skirt as the reference plane, the boundary line of the two fillers is located 1 / 2h-3 / 5h above the reference plane, and h is the overall height of the micro-hemispherical), and the remaining area is filled with gypsum powder or tooth tray powder. For details, see Figure 7 ; In this embodiment, gypsum powder is selected to be mixed with water to form a first bonding mixture 7, wherein the mass ratio of gypsum powder to water is 2:1; rosin and asphalt are mixed to obtain a second bonding mixture 8, wherein the mass ratio of rosin to asphalt is 3:1; the filling boundary line between the first bonding mixture 7 and the second bonding mixture 8 is located 3 / 5h above the reference plane.

[0068] Step 5: The fixture 4 with the micro-hemisphere 6 bonded thereto is clamped on the grinding and polishing equipment through the clamping mechanism 100, and an external air nozzle is used to evacuate air to form a negative pressure between the fixture 4 and the rotating shaft 2, thereby increasing the clamping force of the fixture 4;

[0069] Step 6: Install the diamond grinding wheel on the grinding and polishing equipment, rotate the clamping mechanism 100 to a suitable angle, form the point grinding of the micro-hemispherical 6 skirt and the diamond grinding wheel, start grinding, and grind the outer diameter of the skirt to the specified outer diameter size; the diamond grinding wheel can be selected between 800 mesh and 2000 mesh;

[0070] Step 7: Adjust the clamping mechanism 100 to be parallel to the Z-axis direction of the grinding and polishing equipment, and further grind the lip edge to a specified height value;

[0071] Step 8: Replace the diamond grinding wheel with a resin grinding wheel, and further polish the lip edge to a specified height value; the mesh size of the resin grinding wheel is between 2000 and 4000 mesh; the resin grinding wheel used is a diamond resin grinding wheel or a cubic boron nitride resin grinding wheel, which has high toughness and elasticity; this embodiment uses a diamond resin grinding wheel produced by Tengda Abrasives Co., Ltd. as a polishing disc.

[0072] Step 9: Remove the jig 4 with the micro-hemispheres from the grinding and polishing equipment, and observe whether there is edge collapse under a microscope. If there is edge collapse, proceed to step 8. If there is no edge collapse, proceed to the cleaning step;

[0073] Step 10: Separation and cleaning of the micro-hemisphere and the jig. First, heat the jig 4 to separate the micro-hemisphere 6 from the jig 4, and then put the micro-hemisphere 6 into the bubble cleaning machine. Each tank can hold different cleaning solutions, including hydrochloric acid, hydrogen peroxide, pure water, sulfuric acid, etc. When cleaning, first introduce gas into the tank to generate bubbles in the cleaning solution to produce a liquid tumbling effect. The turbulent kinetic energy generated can accelerate the removal of dirt adhered to the micro-hemisphere. The bubble cleaning machine is made of PVC material. After cleaning at a rate of about 3-8 minutes per tank, the micro-hemisphere is transferred to the next cleaning tank for the next cleaning step. After all cleaning steps are completed, observe under a microscope. If there is any residue, further clean it.

[0074] Step 11: Removal of metal film layer and polishing with chemical solution. Place the cleaned micro-hemispherical ball into a solution suitable for film removal to remove the metal film layer (such as using a strong acid solution). This can be done in a tank in a bubble cleaning machine by bubble cleaning. The micro-hemispherical ball is then polished with a chemical solution (a mixed solution of 49% hydrofluoric acid solution + ammonium fluoride + disodium ethylenediaminetetraacetic acid + sodium tetraborate + deionized water is used in this embodiment, and the mass ratio of the above compounds is 3.5:6.9:0.3:0.3:89). In order to avoid corrosion caused by the chemical solution in the thinnest area of ​​the shoulder of the micro-hemispherical ball, causing irreversible loss or breakage of the micro-hemispherical ball, as follows: Figure 8 and 9As shown, an auxiliary jig 11 is added to raise the micro-hemisphere 6 to a suitable height of the chemical polishing jig 12, so that only the lip of the micro-hemisphere contacts the chemical polishing solution in the chemical polishing jig. After the micro-hemisphere is left in the chemical polishing solution for 10-30 minutes, the micro-hemisphere is taken out for further cleaning to complete the micro-hemisphere grinding and polishing process.

[0075] It should be noted that, the “front” and “rear” in the front and rear surfaces and the “upper” and “lower” in the upper and lower end surfaces involved in the textual description of this embodiment are used to express the relative relationship of the above-mentioned surfaces or end surfaces, and should not be understood as a description of the absolute position relationship of the above-mentioned surfaces or end surfaces, which may be expressed differently under different azimuth viewing angles.

[0076] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for grinding and polishing the micro-hemispherical lip edge. It is characterized in that The following steps are involved: S1: The micro-hemispherical ball is placed upside down on the grinding and polishing integrated device through a clamping mechanism, and the outer circle of the bottom surface of the skirt of the micro-hemispherical ball is brought into contact with the grinding disk of the grinding and polishing integrated device by rotating and / or lifting the clamping mechanism, and the grinding and polishing integrated device is started to perform point grinding on the skirt of the micro-hemispherical ball until the outer diameter of the skirt is ground to a set size to form a lip edge; S2: The bottom surface of the lip edge of the micro-hemispherical ball is made to fit with the grinding disk of the grinding and polishing equipment by rotating and lifting the clamping mechanism, and the grinding and polishing equipment is started to perform surface grinding on the lip edge surface of the micro-hemispherical ball.

2. The micro-hemispherical lip edge grinding and polishing method according to claim 1, It is characterized in that The clamping mechanism includes a jig, a mounting hole is formed on the lower end surface of the jig, the upper and middle parts of the inverted micro-hemisphericity extend into the mounting hole, the skirt and lower part of the micro-hemisphericity are exposed outside the mounting hole, a first bonding mixture is filled between the middle part of the outer wall of the micro-hemisphericity and the corresponding inner wall of the mounting hole, a second bonding mixture is filled at other positions of the mounting hole, the micro-hemisphericity is also filled with the first bonding mixture, the adhesion of the second bonding mixture is greater than that of the first bonding mixture, and the micro-hemisphericity is fixedly connected to the jig after the first bonding mixture and the second bonding mixture are cured.

3. The micro-hemispherical lip edge grinding and polishing method according to claim 2, It is characterized in that The first bonding mixture includes powder and water, the powder is gypsum powder or dental tray powder, and the mass ratio of the powder to water is 1:1-3:1; the second bonding mixture includes rosin and asphalt, and the mass ratio of the rosin to asphalt is 2:1-4:

1.

4. The micro-hemispherical lip edge grinding and polishing method according to claim 2, It is characterized in that Assuming that the overall height of the micro-hemisphere is h, and the bottom surface of the skirt of the micro-hemisphere is taken as the reference plane, the filling boundary line between the first bonding mixture and the second bonding mixture is located 1 / 2h-3 / 5h above the reference plane.

5. The micro-hemispherical lip edge grinding and polishing method according to claim 2, It is characterized in that The clamping mechanism also includes a clamping assembly, which can be rotatably mounted on the three-axis moving mechanism of the grinding and polishing equipment. The fixture is fixed to the bottom of the clamping assembly, and there is an air passage connected to the negative pressure device between the clamping assembly and the fixture. The negative pressure device is used to evacuate the air passage to form negative pressure so that the fixture is adsorbed on the clamping assembly.

6. The micro-hemispherical lip edge grinding and polishing method according to any one of claims 1 to 5, It is characterized in that After step S2, step S3 is also included: by moving the clamping mechanism, the bottom surface of the lip edge of the micro-hemispherical ball is made to fit with the polishing disk of the grinding and polishing device, and the grinding and polishing device is started to perform surface polishing on the lip edge surface of the micro-hemispherical ball.

7. The micro-hemispherical lip edge grinding and polishing method according to claim 6, It is characterized in that The grinding disc is a diamond grinding wheel disc; the polishing disc is a diamond resin grinding wheel or a cubic boron nitride resin grinding wheel.

8. The micro-hemispherical lip edge grinding and polishing method according to claim 6, It is characterized in that After step S3, step S4 is also included: softening the first bonding mixture and the second bonding mixture by heating to separate the micro-hemispherical ball from the jig, and cleaning the micro-hemispherical ball to remove the first bonding mixture and the second bonding mixture on the surface of the micro-hemispherical ball.

9. The micro-hemispherical lip edge grinding and polishing method according to claim 8, It is characterized in that After step S4, the method further includes step S5: chemically polishing the lip edge surface of the micro-hemispherical ball to remove micro-cracks on the lip edge surface of the micro-hemispherical ball.

10. The micro-hemispherical lip edge grinding and polishing method according to claim 9, It is characterized in that Before step S1, the method further includes: coating the micro-hemispherical body as a whole to form a film layer on the inner and outer walls of the micro-hemispherical body; the film layer includes one of an aluminum film, a copper film or a silver film, and the thickness of the film layer is 20-400 nm; The method further includes polishing the micro-hemispherical body to remove the film layer on the surface of the micro-hemispherical body between step S4 and step S5.

Citation Information

Cited By

  • Micro-hemisphere batch polishing device and method

    CN120055945A

  • Micro-hemisphere grinding and polishing equipment

    CN120095668A

  • Micro-hemispherical harmonic oscillator lip edge batch polishing device and method

    CN122606450A

  • Batch polishing device for micro hemispheres

    CN223889647U

  • Micro-hemisphere grinding and polishing equipment

    CN223981605U