A kind of biochar foam concrete with high carbon fixation efficiency and preparation method thereof

By using rice straw to prepare calcium metaaluminate-mixed biochar composite gel and combining it with reinforced aggregate, the problem of insufficient mechanical properties and carbon sequestration and emission reduction performance of biochar foam concrete is solved, and the compressive strength and carbon sequestration efficiency are improved. Achieving green and environmentally friendly production results.

CN118561569BActive Publication Date: 2024-10-11CHINA CONSTR WESTERN CONSTR (GUANGDONG) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040805.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-11
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The mechanical properties and carbon sequestration and emission reduction performance of existing biochar foam concrete need to be further improved. Especially when the biochar content is large, the compactness and strength of the concrete will be reduced, resulting in poor emission reduction effects.

Method used

Rice straw is used as biochar raw material, and a biochar composite gel mixed with calcium metaaluminate is prepared through pretreatment and activation, and combined with reinforced aggregates, using modified silicone polyether emulsion and other composite foaming agents for foaming. Foam treatment to form biochar foam concrete with high carbon sequestration efficiency.

Benefits of technology

It improves the mechanical properties and carbon sequestration performance of foam concrete, enhances its compressive strength and porosity, promotes the fixation and emission reduction of carbon dioxide, and realizes a green and environmentally friendly production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561569B_ABST
    Figure CN118561569B_ABST
Patent Text Reader

Abstract

The invention discloses a biochar foam concrete with high carbon fixation efficiency and a preparation method thereof, belongs to the technical field of foam concrete processing, and is used to solve the technical problem that the mechanical properties and carbon fixation and emission reduction performance of the biochar foam concrete in the prior art need to be further improved; the invention comprises the following components in parts by weight: 30-60 parts of cement, 70-80 parts of reinforcing aggregate, 7-11 parts of biochar composite gel, 50-60 parts of water, 2-3 parts of water reducer and 20-40 parts of composite foaming agent; the invention strengthens the foam concrete by preparing the biochar composite gel mixed with calcium aluminate and the reinforcing aggregate, not only effectively improves the mechanical properties of the foam concrete, but also improves the carbon fixation and emission reduction performance of the foam concrete, reduces the pollution of the foam concrete to the environment during the preparation process, realizes low-carbon and environmentally friendly production, and conforms to the current concepts of environmental protection and sustainable development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam concrete processing, and in particular to biochar foam concrete with high-efficiency carbon fixation and a preparation method thereof. Background Art

[0002] Biochar is a porous carbonaceous material made from agricultural waste and other biomass raw materials through high-temperature pyrolysis under anoxic or low-oxygen conditions. Due to its high porosity and large specific surface area, biochar has good adsorption properties and stability, and can effectively adsorb and fix greenhouse gases such as carbon dioxide. With the increasing severity of global climate change and environmental problems, reducing greenhouse gas emissions and achieving carbon reduction have become important issues of common concern to the international community. Applying biochar to building materials is of great significance for reducing carbon emissions and achieving green and sustainable development in the construction industry.

[0003] In the prior art, a Chinese patent with publication number CN116969723A discloses a biochar foam concrete with high-efficiency carbon fixation performance, which belongs to the technical field of carbon sequestration materials. The biochar is loaded with a foam concrete material to obtain a biochar foam concrete material. The biochar foam concrete material of the present invention has a uniform pore structure and good stability. It can show excellent carbon fixation effect by virtue of the synergistic carbon fixation effect of the characteristics of biochar itself, the adsorption characteristics of carbon dioxide and the carbonization reaction characteristics of cement-based materials, and has a good demonstration effect of low-carbon cement-based materials. According to actual experimental results, when the biochar replacement rate is 6% and 7.5%, the carbon dioxide emission reduction rate of the material over its entire life cycle can exceed 50% and 60% respectively; according to theoretical calculations, when the biochar replacement rate reaches 12%, the carbon dioxide emission reduction rate can reach 100%.

[0004] When existing biochar is used to enhance foam concrete materials, it is usually added directly to the foam concrete material. In order to achieve the expected emission reduction effect, a large amount of biochar material is often required. However, the addition of biochar will increase the porosity of concrete, especially when the biochar content is large, it will reduce the density and strength of the concrete. The mechanical properties and carbon fixation and emission reduction performance of biochar foam concrete need to be further improved.

[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a biochar foam concrete with high carbon fixation efficiency and a preparation method thereof, so as to solve the technical problem in the prior art that the mechanical properties and carbon fixation and emission reduction performance of biochar foam concrete need to be further improved.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A biochar foam concrete with high carbon fixation efficiency, comprising the following components in parts by weight: 30-60 parts of cement, 70-80 parts of reinforcing aggregate, 7-11 parts of biochar composite gel, 50-60 parts of water, 2-3 parts of water reducing agent and 20-40 parts of composite foaming agent;

[0009] The preparation method of the biochar composite gel is as follows: activated straw carbon powder, octamethyl silicone oil, tetraethyl silicate and tetrahydrofuran are added into a nitrogen-protected reactor and stirred for 20-30 minutes at room temperature, an alkali catalytic solution is added into the reactor, the temperature of the reactor is increased to reflux the system, the reaction is carried out for 6-8 hours, and the biochar composite gel is obtained by post-processing.

[0010] Further, the cement is silicate cement;

[0011] The reinforcing aggregate is composed of expanded perlite and river sand in a weight ratio of 3:2, and the particle sizes of the expanded perlite and river sand are both 0.1-2 mm;

[0012] The composite foaming agent is composed of modified silicone resin polyether emulsion, sodium lauryl sulfate, calcium stearate and purified water in a weight ratio of 20:2-4:3-5:6-8, wherein the solid content of the modified silicone resin polyether emulsion is 45-55%.

[0013] The synthesis reaction principle of biochar composite gel is:

[0014] Under alkaline conditions, the siloxane bonds on the activated straw charcoal powder, octamethyl silicone oil, and tetraethyl silicate are hydrolyzed to form silanols, and then self-assembly polycondensation reactions occur to form polysiloxanes with a three-dimensional network structure. Under high temperature conditions, the growth of the siloxane network can be promoted. When the siloxane network grows to a certain extent, the system begins to gel, thereby preparing a biochar composite gel mixed with calcium aluminate.

[0015] Furthermore, the amount ratio of the activated straw charcoal powder, octamethyl silicone oil, tetraethyl silicate, tetrahydrofuran and alkaline catalytic solution is 5g:10g:2g:100mL:30g, the alkaline catalytic solution is composed of potassium hydroxide, calcium aluminate and purified water in a weight ratio of 1:3:10, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is reduced to 40-48°C, and the tetrahydrofuran is evaporated under reduced pressure to obtain a biochar composite gel.

[0016] Furthermore, the activated straw charcoal powder is obtained by processing the following steps:

[0017] A1. Using rice straw as raw material, pretreating it to prepare pretreated straw;

[0018] A2, placing the pretreated straw in a nitrogen-protected tubular furnace and performing programmed temperature calcination to obtain cracked straw charcoal powder;

[0019] A3, adding cracked straw charcoal powder, KH-550 and anhydrous ethanol into a reactor and stirring, raising the temperature of the reactor to 45-55°C, adding sodium hydroxide solution into the reactor, and heat-treating for 4-6 hours, and post-treating to obtain an activated straw charcoal powder precursor;

[0020] A4. Add activated straw charcoal powder precursor and tetrahydrofuran into a nitrogen-protected reactor and stir. Add isocyanatepropyltriethoxysilane into the reactor at room temperature. Raise the temperature of the reactor to 45-55°C. Keep the reaction warm for 60-80 minutes. Post-treat to obtain activated straw charcoal powder.

[0021] The preparation principle of activated straw charcoal powder is:

[0022] Calcination under nitrogen protection is to prevent the straw from being oxidized by oxygen in the air at high temperature. Through programmed temperature increase calcination, it can be ensured that the straw is gradually cracked at a controlled temperature and time to form carbon powder, thereby removing most of the non-carbon elements in the straw, increasing the carbon content, and forming cracked straw carbon powder; after the cracked straw carbon powder is modified with KH-550, the amino group on it undergoes a condensation reaction with the isocyanate group on isocyanatepropyltriethoxysilane, forming triethoxysilane modification on the outside of the carbon powder, and preparing activated straw carbon powder.

[0023] Further, in step A2, the programmed temperature step includes: the tubular furnace is first heated to 280-320°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, then the temperature is increased to 460-500°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 680-720°C at a heating rate of 3°C / min, and the temperature is kept for 3 hours, and the temperature is naturally cooled to room temperature, and the material is discharged; in step A3, the amount ratio of the pyrolysis straw charcoal powder, KH-550, anhydrous ethanol and sodium hydroxide solution is 5g:2g:40mL:10mL, the concentration of the sodium hydroxide solution is 2-3mol / L, and the latter The treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed twice with purified water and then dried, the filter cake is transferred to a drying oven at a temperature of 70-80°C, and dried to constant weight to obtain an activated straw carbon powder precursor; in step A4, the amount ratio of the activated straw carbon powder precursor, tetrahydrofuran and isocyanatepropyltriethoxysilane is 5g:40mL:4g, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed twice with tetrahydrofuran and then dried, the filter cake is transferred to a drying oven at a temperature of 50-60°C, and vacuum dried to constant weight to obtain activated straw carbon powder.

[0024] Furthermore, the preprocessing in step A1 includes the following steps:

[0025] B1. Use a guillotine to cut the rice straw into pieces with a length of 2-3 cm;

[0026] B2. Add the straw segments and the pretreatment solution into a reactor and stir. The temperature of the reactor is raised to 60-70° C. and the reactor is kept warm for 2-3 hours. The pretreated straw is obtained by post-processing.

[0027] The preparation principle of pretreated straw is:

[0028] By chopping rice straw into shorter straw segments of relatively uniform size, the shorter straw segments can be heated faster and cracked evenly, thereby improving the cracking efficiency; sodium dodecyl sulfate in the pretreatment solution acts as a surfactant and can form a thin film on the surface of the straw, which helps to improve the wettability and dispersibility of the straw, making it easier to mix and react with the pretreatment solution during the pretreatment process; potassium hydroxide is a strong base that can react with cellulose, hemicellulose and other components in the straw, promote its structural opening, increase the porosity and specific surface area of ​​the straw, and thus facilitate the subsequent cracking process, making the straw easier to crack into fine charcoal powder and increasing the specific surface area and porosity of the cracked straw charcoal powder.

[0029] Furthermore, in step B2, the pretreatment solution is composed of potassium hydroxide, sodium dodecyl sulfate and drinking water in a weight ratio of 2:0.5:10, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with drinking water 2-3 times and then dried, and the filter cake is transferred to a drying oven at a temperature of 70-80°C and dried to constant weight to obtain pretreated straw.

[0030] A method for preparing biochar foam concrete with high carbon fixation efficiency comprises the following steps:

[0031] S1. Add cement, reinforced aggregate, biochar composite gel, water reducer and water into a mixer, mix at high speed for 20-30 minutes, reduce the stirring speed of the mixer, maintain low speed stirring, and obtain a premix;

[0032] S2, adding the composite foaming agent into the foaming machine, using carbon dioxide as the gas source for foaming, and adding the prepared foam into the premix, and after the addition is completed, stirring is maintained for 1-3 minutes to obtain a ready-mixed concrete;

[0033] S3. Add the premixed concrete into the forming mold, cure it at room temperature for 6-8 hours, solidify the sample, remove the mold, and transfer the sample to a curing box for curing to obtain foamed concrete.

[0034] Furthermore, in step S1, the speed of the high-speed stirring of the mixer is 60-70 r / min, and the speed of the low-speed stirring is 20-30 r / min; in step S2, the purity of the carbon dioxide is higher than 99.9%, the delivery pressure of the carbon dioxide in the foaming machine is 0.35-0.45 MPa, and the density of the foamed foam is 60±2 kg / m 3 ; In step S3, the temperature of the curing box is 18-22°C, the humidity is 85-95%, and the curing time is 28 days.

[0035] The present invention has the following beneficial effects:

[0036] 1. The highly efficient carbon-fixing biochar foam concrete of the present application is prepared by selecting rice straw as the biochar raw material, pre-treating it and then cracking and carbonizing it to prepare biochar, and then activating the biochar to prepare a biochar composite gel mixed with calcium aluminate, which is then combined with reinforcing aggregate to reinforce the foam concrete, which not only effectively improves the mechanical properties of the foam concrete, but also improves the carbon fixation performance of the foam concrete.

[0037] 2. The highly efficient carbon-fixing biochar foam concrete of the present application is prepared by pre-treating rice straw to obtain cracked straw carbon powder with a porous structure, activating it to improve its activity, and reacting it with octamethyl silicone oil and tetraethyl silicate in an alkaline environment to form a three-dimensional network structure of biochar and polysiloxane cross-linking. Calcium aluminate is used as a component of the catalytic solution. On the one hand, it can cooperate with potassium hydroxide to catalyze the reaction during the reaction, and on the other hand, it can be used as an inorganic substance to enhance the doping of biochar composite gel. The high specific surface area, weather resistance and chemical stability of the straw carbon powder in the biochar composite gel can increase its contact area with the cement matrix, and it cooperates with the polysiloxane gel to improve the water resistance of the foamed concrete while promoting the formation of a firm bond between the straw carbon powder and the cement material. The combination of straw charcoal powder and biochar composite gel can improve the strength of foam concrete; as a biomass material, straw charcoal powder itself has a certain carbon fixation ability. During the production process of foam concrete, the carbon element in the straw charcoal powder can be fixed in the concrete to reduce carbon emissions. At the same time, the high specific surface area and pore structure of the straw charcoal powder may also increase its contact area with carbon dioxide and improve carbon fixation efficiency; calcium aluminate introduced into the biochar composite gel as an early strength activator can promote the cement hydration reaction, increase the early strength and final strength of cement, thereby improving the compressive strength of foam concrete. In addition, calcium aluminate can also absorb and fix carbon dioxide in the foam during the production and use of foam concrete, and generate aluminum hydroxide, calcium carbonate, etc., produce a slight volume expansion, increase the porosity of foam concrete, and promote carbon fixation and emission reduction.

[0038] 3. The biochar foam concrete with high carbon fixation in the present application is prepared by using a composite foaming agent composed of modified silicone resin polyether emulsion, sodium dodecyl sulfate, calcium stearate and purified material, and foaming the composite foam with carbon dioxide as carrier gas, adjusting the foaming process, and preparing high-density foamed foam. The foaming process with carbon dioxide as carrier gas can also fix the carbon dioxide in the foam concrete through chemical reaction, thereby improving the emission reduction and reuse of carbon dioxide. In addition, since the foam concrete has a high porosity and specific surface area, more carbon dioxide can be fixed in the foam concrete through carbon dioxide foaming treatment, further improving its carbon fixation performance, reducing environmental pollution, and realizing the green production and use of foam concrete. Expanded perlite and river sand are used as reinforcing agents to strengthen foam concrete. Expanded perlite has a porous structure. These pores can effectively absorb and store moisture, reduce the free movement of moisture in concrete, and thus reduce the risk of moisture penetration. By adjusting the particle size of the reinforcing aggregate, the voids in the concrete can be filled to make the concrete more compact, reducing the penetration channels for moisture and other harmful substances. By optimizing the particle size of the reinforcing aggregate, it also helps to enhance the uniform dispersion of the aggregate in the foam concrete, further improve the anti-penetration performance of the foam concrete, and form a uniformly distributed skeleton support in the foam concrete, thereby improving the stability and strength of the overall structure of the foam concrete, making the foam concrete stronger when subjected to external forces, and improving the mechanical properties of the foam concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 is a SEM image of the biochar composite gel in the present invention;

[0041] Figure 2 is a SEM image of the biochar composite gel in the present invention;

[0042] Figure 3 This is a physical picture of the biochar composite gel in the present invention. DETAILED DESCRIPTION

[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] The modified silicone resin polyether emulsion used in the present invention is a commercially available material selected from Green Union (Jining) Chemical Technology Co., Ltd.

[0045] Example 1

[0046] This embodiment provides a method for preparing a biochar composite gel for biochar foam concrete with high carbon fixation efficiency, comprising the following steps:

[0047] S1. Preparation of pretreated straw

[0048] The rice straw is cut into pieces with a guillotine to prepare straw segments with a length of 2-3 cm;

[0049] Potassium hydroxide, sodium lauryl sulfate and drinking water are mixed in a weight ratio of 2:0.5:10 to obtain a pretreatment solution for later use;

[0050] Add the straw segments and pretreatment solution into the reactor so that the straw segments can be completely immersed and stirred. The temperature of the reactor is raised to 60°C and kept warm for 2 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature and filtered. The filter cake is washed twice with drinking water and then dried. The filter cake is transferred to a drying oven at 70°C and dried to constant weight to obtain pretreated straw.

[0051] S2. Preparation of pyrolysis straw charcoal powder

[0052] The pretreated straw was placed in a nitrogen-protected tubular furnace. The temperature was first increased to 280°C at a heating rate of 5°C / min, and kept warm for 1 hour. The temperature was then increased to 460°C at a heating rate of 5°C / min, and kept warm for 1 hour. The temperature was then increased to 680°C at a heating rate of 3°C / min, and kept warm for 3 hours. The temperature was naturally lowered to room temperature, and the material was discharged to obtain pyrolysis straw charcoal powder.

[0053] S3. Preparation of activated straw charcoal powder

[0054] Weigh: 50g of cracked straw charcoal powder, 20g of KH-550, and 400mL of anhydrous ethanol, add them into a reactor and stir, raise the temperature of the reactor to 45°C, add 100mL of 2mol / L sodium hydroxide solution into the reactor, and keep it warm for 4h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water twice and then drain, transfer the filter cake to a drying oven at 70°C, and dry it to constant weight to obtain an activated straw charcoal powder precursor;

[0055] Weigh: 50 g of activated straw charcoal powder precursor and 400 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. At room temperature, 40 g of isocyanatepropyltriethoxysilane is first added to the reactor, the reactor temperature is raised to 45°C, and the reaction is kept warm for 60 minutes. After the reaction is completed, the reactor temperature is lowered to room temperature, filtered, the filter cake is washed twice with tetrahydrofuran and then dried, and the filter cake is transferred to a drying oven at a temperature of 50°C and vacuum dried to constant weight to obtain activated straw charcoal powder.

[0056] S4. Preparation of biochar composite gel

[0057] Mix potassium hydroxide, calcium aluminate and purified water in a weight ratio of 1:3:10 to obtain an alkaline catalytic solution;

[0058] Weigh: 50 g of activated straw charcoal powder, 100 g of octamethyl silicone oil, 20 g of tetraethyl silicate, and 1000 mL of tetrahydrofuran, add them into a nitrogen-protected reactor and stir, stir at room temperature for 20 min, add 300 g of base catalytic solution into the reactor, increase the temperature of the reactor to reflux the system, and react for 6 h. After the reaction is completed, the temperature of the reactor is reduced to 40 ° C, and tetrahydrofuran is evaporated under reduced pressure to obtain a biochar composite gel.

[0059] Example 2

[0060] This embodiment provides a method for preparing a biochar composite gel for biochar foam concrete with high carbon fixation efficiency, comprising the following steps:

[0061] S1. Preparation of pretreated straw

[0062] The rice straw is cut into pieces with a guillotine to prepare straw segments with a length of 2-3 cm;

[0063] Potassium hydroxide, sodium lauryl sulfate and drinking water are mixed in a weight ratio of 2:0.5:10 to obtain a pretreatment solution for later use;

[0064] Add the straw segments and pretreatment solution into the reactor so that the straw segments can be completely immersed and stirred. The temperature of the reactor is raised to 65°C and kept warm for 2.5 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature and filtered. The filter cake is washed three times with drinking water and then dried. The filter cake is transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain pretreated straw.

[0065] S2. Preparation of pyrolysis straw charcoal powder

[0066] The pretreated straw was placed in a nitrogen-protected tubular furnace. The temperature of the tubular furnace was first increased to 300°C at a heating rate of 5°C / min, and kept warm for 1 hour. The temperature was then increased to 480°C at a heating rate of 5°C / min, and kept warm for 1 hour. The temperature was then increased to 700°C at a heating rate of 3°C / min, and kept warm for 3 hours. The temperature was naturally lowered to room temperature, and the material was discharged to obtain pyrolysis straw charcoal powder.

[0067] S3. Preparation of activated straw charcoal powder

[0068] Weigh: 50g of cracked straw charcoal powder, 20g of KH-550, and 400mL of anhydrous ethanol, add them into a reactor and stir, raise the temperature of the reactor to 50°C, add 100mL of 2.5mol / L sodium hydroxide solution into the reactor, and keep it warm for 5h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water twice and then drain, transfer the filter cake to a drying oven at 75°C, and dry it to constant weight to obtain an activated straw charcoal powder precursor;

[0069] Weigh: 50 g of activated straw charcoal powder precursor and 400 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. At room temperature, 40 g of isocyanatepropyltriethoxysilane is first added to the reactor, the reactor temperature is raised to 50°C, and the reaction is kept warm for 70 minutes. After the reaction is completed, the reactor temperature is lowered to room temperature, filtered, the filter cake is washed twice with tetrahydrofuran and then dried, the filter cake is transferred to a drying oven at a temperature of 55°C, and vacuum dried to constant weight to obtain activated straw charcoal powder.

[0070] S4. Preparation of biochar composite gel

[0071] Mix potassium hydroxide, calcium aluminate and purified water in a weight ratio of 1:3:10 to obtain an alkaline catalytic solution;

[0072] Weigh: 50 g of activated straw charcoal powder, 100 g of octamethyl silicone oil, 20 g of tetraethyl silicate, and 1000 mL of tetrahydrofuran, add them into a nitrogen-protected reactor and stir, stir at room temperature for 25 min, add 300 g of base catalytic solution into the reactor, increase the temperature of the reactor to reflux the system, and react for 7 h. After the reaction is completed, the temperature of the reactor is reduced to 44 ° C, and tetrahydrofuran is evaporated under reduced pressure to obtain a biochar composite gel.

[0073] Example 3

[0074] This embodiment provides a method for preparing a biochar composite gel for biochar foam concrete with high carbon fixation efficiency, comprising the following steps:

[0075] S1. Preparation of pretreated straw

[0076] The rice straw is cut into pieces with a guillotine to prepare straw segments with a length of 2-3 cm;

[0077] Potassium hydroxide, sodium lauryl sulfate and drinking water are mixed in a weight ratio of 2:0.5:10 to obtain a pretreatment solution for later use;

[0078] Add the straw segments and pretreatment solution into the reactor so that the straw segments can be completely immersed and stirred. The temperature of the reactor is raised to 70°C and kept warm for 3 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature and filtered. The filter cake is washed twice with drinking water and then dried. The filter cake is transferred to a drying oven at 80°C and dried to constant weight to obtain pretreated straw.

[0079] S2. Preparation of pyrolysis straw charcoal powder

[0080] The pretreated straw was placed in a nitrogen-protected tubular furnace, and the temperature was first increased to 320°C at a heating rate of 5°C / min, and kept warm for 1 hour, then increased to 500°C at a heating rate of 5°C / min, and kept warm for 1 hour, and then increased to 720°C at a heating rate of 3°C / min, and kept warm for 3 hours. The temperature was naturally cooled to room temperature, and the material was discharged to obtain pyrolysis straw charcoal powder.

[0081] S3. Preparation of activated straw charcoal powder

[0082] Weigh: 50g of cracked straw charcoal powder, 20g of KH-550, and 400mL of anhydrous ethanol, add them into a reactor and stir, raise the temperature of the reactor to 55°C, add 100mL of 3mol / L sodium hydroxide solution into the reactor, and keep it warm for 6h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water twice and then drain, transfer the filter cake to a drying oven at 80°C, and dry it to constant weight to obtain an activated straw charcoal powder precursor;

[0083] Weigh: 50 g of activated straw charcoal powder precursor and 400 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. At room temperature, 40 g of isocyanatepropyltriethoxysilane is first added to the reactor, the reactor temperature is raised to 55°C, and the reaction is kept warm for 80 minutes. After the reaction is completed, the reactor temperature is lowered to room temperature, filtered, the filter cake is washed twice with tetrahydrofuran and then dried, the filter cake is transferred to a drying oven at a temperature of 60°C, and vacuum dried to constant weight to obtain activated straw charcoal powder.

[0084] S4. Preparation of biochar composite gel

[0085] Mix potassium hydroxide, calcium aluminate and purified water in a weight ratio of 1:3:10 to obtain an alkaline catalytic solution;

[0086] Weigh: 50 g of activated straw charcoal powder, 100 g of octamethyl silicone oil, 20 g of tetraethyl silicate, and 1000 mL of tetrahydrofuran, add them into a nitrogen-protected reactor and stir, stir at room temperature for 30 min, add 300 g of base catalytic solution into the reactor, increase the temperature of the reactor to reflux the system, and react for 8 h. After the reaction is completed, the temperature of the reactor is reduced to 48 ° C, and tetrahydrofuran is evaporated under reduced pressure to obtain a biochar composite gel.

[0087] Example 4

[0088] This embodiment provides a method for preparing biochar foam concrete with high carbon fixation efficiency, comprising the following steps:

[0089] Step 1: Prepare the ingredients

[0090] Portland cement is selected as cement;

[0091] Select polycarboxylate water reducer as water reducer;

[0092] The expanded perlite with a particle size of 0.1-2 mm and the river sand with a particle size of 0.1-2 mm are mixed evenly in a weight ratio of 3:2 to obtain a reinforcing aggregate;

[0093] The modified silicone resin polyether emulsion, sodium lauryl sulfate, calcium stearate and purified water are uniformly mixed in a weight ratio of 20:2:3:6 to obtain a composite foaming agent, wherein the solid content of the modified silicone resin polyether emulsion is 45%;

[0094] Weigh by weight: 30 parts of cement, 70 parts of reinforcing aggregate, 7 parts of the biochar composite gel prepared in Example 1, 50 parts of water, 2 parts of water reducing agent, and 20 parts of composite foaming agent, and store them separately for later use.

[0095] Step 2: Premix

[0096] The cement, reinforced aggregate, biochar composite gel, water and water reducing agent prepared in step 1 are added to the mixer, the stirring speed of the mixer is increased to 60r / min, and high-speed stirring is performed for 20min. The stirring speed of the mixer is reduced to 20r / min, and low-speed stirring is maintained to obtain a premix.

[0097] Step 3: Foaming

[0098] Add the composite foaming agent prepared in step 1 into the foaming machine, use carbon dioxide with a purity higher than 99.9% as the gas source, set the delivery pressure of carbon dioxide to 0.35MPa, and foam to obtain a foam with a density of 60±2kg / m 3 of bubbles.

[0099] Step 4: Prepare ready-mixed concrete

[0100] The prepared foam is added to the premix in step 1. After the addition is completed, stirring is continued for 1 minute to obtain ready-mixed concrete.

[0101] Step 5: Prepare foam concrete

[0102] Add the premixed concrete into the forming mold and cure it for 6 hours at room temperature. After the sample is solidified, remove the mold and transfer the sample to a curing box. Set the temperature of the curing box to 18°C ​​and the humidity to 85%. Curing time is 28 days to obtain foamed concrete.

[0103] Example 5

[0104] This embodiment provides a method for preparing biochar foam concrete with high carbon fixation efficiency, comprising the following steps:

[0105] Step 1: Prepare the ingredients

[0106] Portland cement is selected as cement;

[0107] Select polycarboxylate water reducer as water reducer;

[0108] The expanded perlite with a particle size of 0.1-2 mm and the river sand with a particle size of 0.1-2 mm are mixed evenly in a weight ratio of 3:2 to obtain a reinforcing aggregate;

[0109] The modified silicone resin polyether emulsion, sodium lauryl sulfate, calcium stearate and purified water are uniformly mixed in a weight ratio of 20:3:4:7 to obtain a composite foaming agent, wherein the solid content of the modified silicone resin polyether emulsion is 50%;

[0110] Weigh by weight: 45 parts of cement, 75 parts of reinforcing aggregate, 9 parts of the biochar composite gel prepared in Example 2, 55 parts of water, 2.5 parts of water reducing agent, and 30 parts of composite foaming agent, and store them separately for later use.

[0111] Step 2: Premix

[0112] The cement, reinforced aggregate, biochar composite gel, water and water reducing agent prepared in step 1 are added to the mixer, the stirring speed of the mixer is increased to 65r / min, and high-speed stirring is performed for 25min. The stirring speed of the mixer is reduced to 25r / min, and low-speed stirring is maintained to obtain a premix.

[0113] Step 3: Foaming

[0114] Add the composite foaming agent prepared in step 1 into the foaming machine, use carbon dioxide with a purity higher than 99.9% as the gas source, set the delivery pressure of carbon dioxide to 0.40 MPa, and foam to obtain a foam with a density of 60±2 kg / m 3 of bubbles.

[0115] Step 4: Prepare ready-mixed concrete

[0116] The prepared foam is added to the premix in step 1. After the addition is completed, stirring is continued for 2 minutes to obtain ready-mixed concrete.

[0117] Step 5: Prepare foam concrete

[0118] Add the premixed concrete into the forming mold and cure it for 7 hours at room temperature. After the sample is solidified, remove the mold and transfer the sample to a curing box. Set the temperature of the curing box to 20°C and the humidity to 90%. Curing time is 28 days to obtain foamed concrete.

[0119] Example 6

[0120] This embodiment provides a method for preparing biochar foam concrete with high carbon fixation efficiency, comprising the following steps:

[0121] Step 1: Prepare the ingredients

[0122] Portland cement is selected as cement;

[0123] Select polycarboxylate water reducer as water reducer;

[0124] The expanded perlite with a particle size of 0.1-2 mm and the river sand with a particle size of 0.1-2 mm are mixed evenly in a weight ratio of 3:2 to obtain a reinforcing aggregate;

[0125] The modified silicone resin polyether emulsion, sodium lauryl sulfate, calcium stearate and purified water are uniformly mixed in a weight ratio of 20:4:5:8 to obtain a composite foaming agent, wherein the solid content of the modified silicone resin polyether emulsion is 55%;

[0126] Weigh out by weight: 60 parts of cement, 80 parts of reinforcing aggregate, 11 parts of the biochar composite gel prepared in Example 3, 60 parts of water, 3 parts of water reducing agent, and 40 parts of composite foaming agent, and store them separately for later use.

[0127] Step 2: Premix

[0128] The cement, reinforced aggregate, biochar composite gel, water and water reducing agent prepared in step 1 are added to the mixer, the stirring speed of the mixer is increased to 70 r / min, and high-speed stirring is performed for 30 minutes. The stirring speed of the mixer is reduced to 30 r / min, and low-speed stirring is maintained to obtain a premix.

[0129] Step 3: Foaming

[0130] Add the composite foaming agent prepared in step 1 into the foaming machine, use carbon dioxide with a purity higher than 99.9% as the gas source, set the delivery pressure of carbon dioxide to 0.45MPa, and foam to obtain a foam with a density of 60±2kg / m 3of bubbles.

[0131] Step 4: Prepare ready-mixed concrete

[0132] The prepared foam is added to the premix in step 1. After the addition is completed, stirring is continued for 3 minutes to obtain ready-mixed concrete.

[0133] Step 5: Prepare foam concrete

[0134] Add the premixed concrete into the forming mold and cure it for 8 hours at room temperature. After the sample is solidified, remove the mold and transfer the sample to a curing box. Set the temperature of the curing box to 22°C and the humidity to 95%. Curing time is 28 days to obtain foamed concrete.

[0135] Comparative Example 1

[0136] The difference between this comparative example and Example 6 is that in step 2, when preparing the premix, no biochar composite gel is added.

[0137] Comparative Example 2

[0138] The difference between this comparative example and Example 6 is that in step 1, during the preparation process of the biochar composite gel prepared in Example 3, the pretreated straw in step S2 is replaced by the straw segment in step S1.

[0139] Comparative Example 3

[0140] The difference between this comparative example and Example 6 is that in step 1, during the preparation process of the biochar composite gel prepared in Example 3, steps S3-S4 are omitted, and the pyrolysis straw charcoal powder obtained in step S2 replaces the biochar composite gel in step 1.

[0141] Comparative Example 4

[0142] The difference between this comparative example and Example 6 is that in step 1, the biochar composite gel prepared in Example 3, in step S4 of the preparation process, the alkaline catalytic solution consists of potassium hydroxide and purified water in a weight ratio of 1:10.

[0143] Comparative Example 5

[0144] The difference between this comparative example and Example 6 is that in step 3, air is used instead of carbon dioxide.

[0145] Performance Test:

[0146] The mechanical properties and carbon fixation and emission reduction performance of the foamed concrete prepared in Examples 4-6 and Comparative Examples 1-5 were tested, wherein the mechanical properties were tested for the thermal conductivity, softening coefficient, water absorption and compressive strength of the samples with reference to the standard JC / T 2357-2016 "Test Method for Performance of Foamed Concrete Products"; the carbon fixation and emission reduction performance was based on Comparative Example 1, with reference to the carbon dioxide emissions over the entire life cycle of biochar foamed concrete disclosed in the invention patent with publication number CN116969723A, and the emission reduction rates of the foamed concrete samples prepared in each embodiment and Comparative Examples 2-4 were determined. The specific test results are shown in Table 1:

[0147] Table 1. Performance test data of samples

[0148]

[0149] Data Analysis:

[0150] A comparative analysis of the data in Table 1 shows that the thermal conductivity of the foamed concrete material prepared by the present invention reaches 0.11 W / m·k, the softening coefficient reaches 0.92, the water absorption rate is reduced to 12.01%, the compressive strength reaches 6.8 MPa, and the emission reduction rate reaches 76.83%. The test results of various performances are better than those of the comparative example, indicating that the present invention uses rice straw as a biochar raw material, pre-treats it, cracks it, carbonizes it, and activates it to prepare a biochar composite gel mixed with calcium aluminate, and then uses it with a reinforcing aggregate to reinforce the foamed concrete, which not only effectively improves the mechanical properties of the foamed concrete, but also improves the carbon fixation and emission reduction performance of the foamed concrete, effectively reduces the pollution of the foamed concrete to the environment during the preparation process, realizes low-carbon and environmentally friendly production, and conforms to the current concept of environmental protection and sustainable development.

[0151] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0152] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0153] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A biochar foam concrete with high carbon fixation efficiency, characterized in that: The invention comprises the following components in parts by weight: 30-60 parts of cement, 70-80 parts of reinforcing aggregate, 7-11 parts of biochar composite gel, 50-60 parts of water, 2-3 parts of water reducing agent and 20-40 parts of composite foaming agent, wherein the foaming gas source is carbon dioxide; The preparation method of the biochar composite gel is as follows: activated straw carbon powder, octamethyl silicone oil, tetraethyl silicate and tetrahydrofuran are added into a nitrogen-protected reactor and stirred for 20-30 minutes at room temperature, a base catalytic solution is added into the reactor, the temperature of the reactor is increased to reflux, the reaction is carried out for 6-8 hours, and the biochar composite gel is obtained by post-processing; The activated straw charcoal powder, octamethyl silicone oil, tetraethyl silicate, tetrahydrofuran and alkaline catalytic solution are used in a ratio of 5g:10g:2g:100mL:30g, and the alkaline catalytic solution is composed of potassium hydroxide, calcium aluminate and purified water in a weight ratio of 1:3:

10. The post-treatment includes: after the reaction is completed, the temperature of the reactor is reduced to 40-48°C, and tetrahydrofuran is evaporated under reduced pressure to obtain a biochar composite gel; The activated straw charcoal powder is obtained by processing the following steps: A1. Using rice straw as raw material, pretreating it to prepare pretreated straw; A2, placing the pretreated straw in a nitrogen-protected tubular furnace and performing programmed temperature calcination to obtain cracked straw charcoal powder; A3, adding cracked straw charcoal powder, KH-550 and anhydrous ethanol into a reactor and stirring, raising the temperature of the reactor to 45-55°C, adding sodium hydroxide solution into the reactor, and heat-treating for 4-6 hours, and post-treating to obtain an activated straw charcoal powder precursor; A4, adding activated straw carbon powder precursor and tetrahydrofuran into a nitrogen-protected reactor and stirring, adding isocyanate propyl triethoxysilane into the reactor at room temperature, raising the temperature of the reactor to 45-55°C, keeping the temperature for reaction for 60-80 minutes, and post-treating to obtain activated straw carbon powder; The preprocessing in step A1 includes the following steps: B1. Use a guillotine to cut rice straw into pieces with a length of 2-3 cm; B2. Add the straw segments and the pretreatment solution into a reactor and stir. The temperature of the reactor is raised to 60-70° C. and the reactor is kept warm for 2-3 hours. The pretreated straw is obtained by post-treatment, wherein the pretreatment solution is composed of potassium hydroxide, sodium dodecyl sulfate and drinking water in a weight ratio of 2:0.5:

10.

2. The biochar foam concrete with high carbon fixation efficiency according to claim 1, characterized in that: The cement is silicate cement; The reinforcing aggregate is composed of expanded perlite and river sand in a weight ratio of 3:2, and the particle sizes of the expanded perlite and river sand are both 0.1-2 mm; The composite foaming agent is composed of modified silicone resin polyether emulsion, sodium lauryl sulfate, calcium stearate and purified water in a weight ratio of 20:2-4:3-5:6-8, wherein the solid content of the modified silicone resin polyether emulsion is 45-55%.

3. The biochar foam concrete with high carbon fixation efficiency according to claim 1, characterized in that: In step A2, the programmed temperature calcination step includes: the tubular furnace is first heated to 280-320°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, then the temperature is increased to 460-500°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 680-720°C at a heating rate of 3°C / min, and the temperature is kept for 3 hours, and the temperature is naturally cooled to room temperature, and the material is discharged; in step A3, the amount ratio of the pyrolysis straw charcoal powder, KH-550, anhydrous ethanol and sodium hydroxide solution is 5g:2g:40mL:10mL, the concentration of the sodium hydroxide solution is 2-3mol / L, and the post-treatment The post-treatment comprises: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the filter cake is filtered, the filter cake is washed twice with purified water and then dried, the filter cake is transferred to a drying oven at a temperature of 70-80°C, and dried to constant weight to obtain an activated straw carbon powder precursor; in step A4, the amount ratio of the activated straw carbon powder precursor, tetrahydrofuran and isocyanatepropyltriethoxysilane is 5g:40mL:4g, and the post-treatment comprises: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the filter cake is filtered, the filter cake is washed twice with tetrahydrofuran and then dried, the filter cake is transferred to a drying oven at a temperature of 50-60°C, and vacuum dried to constant weight to obtain activated straw carbon powder.

4. The biochar foam concrete with high carbon fixation efficiency according to claim 1, characterized in that: In step B2, the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the filter cake is filtered, the filter cake is washed with drinking water 2-3 times and then dried, the filter cake is transferred to a drying oven at a temperature of 70-80° C., and dried to constant weight to obtain pretreated straw.

5. The method for preparing a biochar foam concrete with high carbon fixation efficiency according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Add cement, reinforced aggregate, biochar composite gel, water reducer and water into a mixer, mix at high speed for 20-30 minutes, reduce the stirring speed of the mixer, maintain low speed stirring, and obtain a premix; S2, adding the composite foaming agent into the foaming machine, using carbon dioxide as the gas source for foaming, and adding the prepared foam into the premix, and after the addition is completed, stirring is maintained for 1-3 minutes to obtain a ready-mixed concrete; S3. Add the premixed concrete into the forming mold, cure it at room temperature for 6-8 hours, solidify the sample, remove the mold, and transfer the sample to a curing box for curing to obtain foamed concrete.

6. The method for preparing a biochar foam concrete with high carbon fixation efficiency according to claim 5, characterized in that: In step S1, the speed of the high-speed stirring of the mixer is 60-70r / min, and the speed of the low-speed stirring is 20-30r / min; in step S2, the purity of carbon dioxide is higher than 99.9%, the delivery pressure of carbon dioxide in the foaming machine is 0.35-0.45MPa, and the density of the foamed foam is 60±2kg / m 3 ; In step S3, the temperature of the curing box is 18-22°C, the humidity is 85-95%, and the curing time is 28 days.