Preparation process of hyperbranched polyetheramide modified glass fiber reinforced nylon composite material
Through the combination of hyperbranched polyetheramide modified glass fiber and nylon 6, the problem of insufficient strength and hydrophilicity of nylon 6 material is solved, significantly improving its mechanical properties and water absorption, and expanding its application range.
Patent Information
- Application Number
- CN202410802065.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Nylon 6 material has low strength and poor hydrophilicity, which affects its application in high-performance composite materials.
Hyperbranched polyetheramide is used to graft and modify glass fibers, and combine them with nylon 6 material. Hyperbranched polyetheramide modified glass fiber reinforced nylon composite material is prepared through blending and extrusion process to improve the mechanical properties of the material. and hydrophilic.
It significantly improves the elongation, impact strength, tensile strength and bending properties of nylon 6 materials, and significantly improves its water absorption and hydrophilicity, expanding its application potential in fibers and textiles.
Smart Images

Figure CN118562162B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nylon, in particular to a preparation process of a hyperbranched polyetheramide modified glass fiber reinforced nylon composite material. Background Art
[0002] Nylon materials mainly include nylon 6, nylon 66, etc., among which nylon 6 has excellent heat resistance, impact resistance, solubility resistance and other properties. In order to meet the practical application of nylon 6 in high-performance composite materials, its mechanical properties need to be improved. In addition, fabric textiles made of nylon 6 fiber have problems such as poor hydrophilicity and poor moisture permeability. Therefore, it is necessary to improve the hydrophilicity of nylon 6 and its fiber products.
[0003] It is widely used in plastics, alloys, fiber fabrics, etc. Modifiers such as glass fiber, rubber, nanoparticles, etc. are usually added to nylon 6 to improve the mechanical properties of nylon 6. Glass fiber is an inorganic non-metallic material with excellent performance. It is widely used in polymer materials due to its excellent insulation, corrosion resistance, mechanical strength and other properties. Improving the compatibility between glass fiber and polymer material matrices such as nylon can make the glass fiber have a better reinforcement effect. Traditional methods mainly include silane coupling agent modification, titanate coupling agent modification, etc. The present invention uses hyperbranched polyether amide to graft modify glass fiber to enhance the mechanical properties and hydrophilic properties of nylon 6 materials. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The invention solves the problems of low strength and poor hydrophilicity of nylon materials.
[0006] (II) Technical solution
[0007] A preparation process of a hyperbranched polyetheramide modified glass fiber reinforced nylon composite material comprises the following steps:
[0008] Step S1, add N, N-dimethylacetamide, ethylene glycol dimethacrylate, and mercapto ether amide polymerization monomer into a reaction container, stir and dissolve, then introduce nitrogen, add photoinitiator 2959, use a 300-800W high-pressure mercury lamp as an ultraviolet light source, irradiate and stir to react for 60-90 minutes, then add KH570 modified glass fiber, stir and react for 20-40 minutes, add methanol to the solution to precipitate, filter, wash with ethanol, and dry to obtain hyperbranched polyether amide modified glass fiber.
[0009] The structural formula of the mercaptoetheramide polymerization monomer is:
[0010]
[0011] Step S2, placing nylon 6, hyperbranched polyether amide modified glass fiber, and an antioxidant in a twin-screw extruder, with a barrel temperature of 210-250° C., a nozzle temperature of 240-250° C., and a screw speed of 60-120 r / min, blending and extruding, and then injection molding in an injection molding machine, with a mold temperature of the injection molding machine of 80-90° C. and an injection molding pressure of 80-100 MPa, to obtain a hyperbranched polyether amide modified glass fiber reinforced nylon composite material.
[0012] Furthermore, the ratio of ethylene glycol dimethacrylate, mercapto ether amide polymerization monomer, and KH570 modified glass fiber in S1 is (1.2-1.4) mol:1 mol:(300-600) g.
[0013] Furthermore, the ratio of the hyperbranched polyetheramide modified glass fiber to nylon 6 in S2 is 1 kg:(100-600) g.
[0014] Step (1), add ethanol, trimesic acid and 1-amino-3,6,9-trioxaundecane-11-ol in a ratio of 1 mol:(3.6-4.2) mol to a reaction vessel, add glacial acetic acid dropwise, heat to 75-80° C., condense and reflux for 18-24 hours, concentrate the solvent until a precipitate is precipitated, filter, wash with acetone, and dry to obtain an intermediate.
[0015] Step (2), adding tetrahydrofuran, the intermediate in a ratio of 1 mol:(3.3-3.9) mol:(3.3-3.9) mol, thioglycolic acid, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into a reaction container, reacting at room temperature for 10-15 hours, concentrating the solvent until a precipitate is precipitated, filtering, washing with acetone, and drying to obtain a thiol ether amide polymerization monomer.
[0016] Furthermore, the preparation process of KH570 modified glass fiber is as follows: add ethanol and KH570 into a reaction container, stir to dissolve and then add glass fiber, mix well and place the solution in an oven, dry at 100-120°C for 2-3h, wash with ethanol, and dry to obtain KH570 modified glass fiber.
[0017] (III) Technical effect: The present invention utilizes ethylene glycol dimethacrylate containing two alkenyl groups and mercapto ether amide polymerization monomers containing three mercapto groups to carry out mercapto-ene hyperbranching reaction, and adjusts the reaction ratio to obtain a hyperbranched polyether amide with terminal mercapto groups, and then the terminal mercapto groups react with the alkenyl groups of KH570 modified glass fibers to obtain hyperbranched polyether amide modified glass fibers.
[0018] The invention utilizes hyperbranched polyetheramide modified glass fiber as filler to fill and modify nylon 6. The hyperbranched polyetheramide contains branched molecular chains of three-dimensional flexible ether bonds, which form spatial physical crosslinking with nylon fibers. When subjected to external force, stress can be well dispersed and transferred, stress concentration can be reduced, and microcracks generated in the nylon matrix can be overcome, thereby achieving a good toughening effect and significantly improving the elongation at break and impact strength of the nylon material. In addition, the hyperbranched polyetheramide contains amide structural units, which have good interface bonding with the polyamide molecular chains of nylon 6. After the glass fiber is grafted and modified, the compatibility between the glass fiber and nylon 6 is significantly improved, so that the glass fiber plays a good reinforcing role and improves the tensile strength and bending performance of the nylon 6 material.
[0019] The hyperbranched polyetheramide modified glass fiber of the invention contains a large number of hydrophilic ether bonds, which can significantly improve the water absorption and hydrophilicity of nylon materials and expand the practical application of nylon materials in hydrophilic fibers and textiles. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a reaction route for preparing mercaptoetheramide polymerization monomers.
[0021] Figure 2 This is the reaction mechanism for the preparation of hyperbranched polyetheramide modified glass fiber. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] (1) Add 25 mL of ethanol, 4 mmol of trimesic acid, and 14.4 mmol of 1-amino-3,6,9-trioxaundecane-11-ol to a reaction vessel, add 1.5 mL of glacial acetic acid dropwise, heat to 75° C., condense and reflux for 24 h, concentrate the solvent until a precipitate is precipitated, filter, wash with acetone, and dry to obtain an intermediate.
[0025] (2) Add 10 mL of tetrahydrofuran, 4 mmol of the intermediate, 13.2 mmol of thioglycolic acid, and 15.6 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into a reaction container, react at room temperature for 12 h, concentrate the solvent until a precipitate is precipitated, filter, wash with acetone, and dry to obtain a thiol ether amide polymerization monomer.
[0026] (3) Add 50 mL of ethanol and 0.1 g of KH570 to a reaction container, stir to dissolve, then add 15 g of glass fiber, mix well, place the solution in an oven, dry at 120° C. for 2 h, wash with ethanol, and dry to obtain KH570-modified glass fiber.
[0027] (4) 150 mL of N,N-dimethylacetamide, 14 mmol of ethylene glycol dimethacrylate, and 10 mmol of mercapto ether amide polymerization monomer were added to a reaction container, and nitrogen was introduced after stirring and dissolving. 0.12 mmol of photoinitiator 2959 was added, and the mixture was irradiated under a 300 W high-pressure mercury lamp, and stirred for reaction for 60 min. Then 3 g of KH570 modified glass fiber was added, and stirred for reaction for 20 min. Methanol was added to the solution to precipitate a precipitate, which was filtered, washed with ethanol, and dried to obtain a hyperbranched polyether amide modified glass fiber.
[0028] (5) 1 kg of nylon 6, 100 g of hyperbranched polyether amide modified glass fiber, and 3 g of antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C, and 250°C, respectively, and a nozzle temperature of 240°C. The screw speed was 100 r / min, and the mixture was extruded and then injection molded in an injection molding machine with a mold temperature of 90°C and an injection pressure of 80 MPa to obtain a hyperbranched polyether amide modified glass fiber reinforced nylon composite material.
[0029] Example 2
[0030] (1) 150 mL of N,N-dimethylacetamide, 13 mmol of ethylene glycol dimethacrylate, and 10 mmol of mercapto ether amide polymerization monomer (the same as the preparation method in Example 1) were added to a reaction container, nitrogen was introduced after stirring and dissolving, 0.12 mmol of photoinitiator 2959 was added, and the mixture was irradiated under a 300 W high-pressure mercury lamp, stirred and reacted for 60 min, and then 4 g of KH570 modified glass fiber (the same as the preparation method in Example 1) was added, stirred and reacted for 20 min, methanol was added to the solution to precipitate a precipitate, filtered, washed with ethanol, and dried to obtain a hyperbranched polyether amide modified glass fiber.
[0031] (2) 1 kg of nylon 6, 250 g of hyperbranched polyether amide modified glass fiber, and 3 g of antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C, and 250°C, respectively, and a nozzle temperature of 250°C. The screw speed was 120 r / min, and the mixture was blended and extruded. The mixture was then injection molded in an injection molding machine with a mold temperature of 90°C and an injection pressure of 80 MPa to obtain a hyperbranched polyether amide modified glass fiber reinforced nylon composite material.
[0032] Example 3
[0033] (1) 200 mL of N,N-dimethylacetamide, 13 mmol of ethylene glycol dimethacrylate, and 10 mmol of mercapto ether amide polymerization monomer (the same as the preparation method in Example 1) were added to a reaction container, nitrogen was introduced after stirring and dissolving, 0.13 mmol of photoinitiator 2959 was added, and the mixture was irradiated under an 800 W high-pressure mercury lamp, and stirred for reaction for 90 min. Then 5 g of KH570 modified glass fiber (the same as the preparation method in Example 1) was added, and the mixture was stirred for reaction for 40 min. Methanol was added to the solution to precipitate a precipitate, which was filtered, washed with ethanol, and dried to obtain a hyperbranched polyether amide modified glass fiber.
[0034] (2) 1 kg of nylon 6, 400 g of hyperbranched polyether amide modified glass fiber, and 3 g of antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C, and 250°C, respectively, and a nozzle temperature of 240°C. The screw speed was 60 r / min, and the mixture was extruded and then injection molded in an injection molding machine with a mold temperature of 90°C and an injection pressure of 80 MPa to obtain a hyperbranched polyether amide modified glass fiber reinforced nylon composite material.
[0035] Example 4
[0036] (1) 200 mL of N,N-dimethylacetamide, 12 mmol of ethylene glycol dimethacrylate, and 10 mmol of mercapto ether amide polymerization monomer (the same as the preparation method in Example 1) were added to a reaction container, nitrogen was introduced after stirring and dissolving, 0.12 mmol of photoinitiator 2959 was added, and the mixture was irradiated under a high-pressure mercury lamp of 800 W, and stirred for reaction for 60 min. Then 6 g of KH570 modified glass fiber (the same as the preparation method in Example 1) was added, and the mixture was stirred for reaction for 40 min. Methanol was added to the solution to precipitate a precipitate, which was filtered, washed with ethanol, and dried to obtain a hyperbranched polyether amide modified glass fiber.
[0037] (2) 1 kg of nylon 6, 600 g of hyperbranched polyether amide modified glass fiber, and 3 g of antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C, and 250°C, respectively, and a nozzle temperature of 250°C. The screw speed was 60 r / min, and the mixture was extruded and then injection molded in an injection molding machine with a mold temperature of 85°C and an injection pressure of 100 MPa to obtain a hyperbranched polyether amide modified glass fiber reinforced nylon composite material.
[0038] Comparative Example 1
[0039] (1) 1 kg of nylon 6 and 3 g of antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C, and 250°C, respectively, and a nozzle temperature of 240°C. The screw speed was 100 r / min, and the mixture was extruded and then injection molded in an injection molding machine with a mold temperature of 90°C and an injection pressure of 80 MPa to obtain a nylon composite material.
[0040] Comparative Example 2
[0041] (1) 150 mL of N,N-dimethylacetamide, 14 mmol of ethylene glycol dimethacrylate, and 10 mmol of mercapto ether amide polymerization monomer (the same preparation method as in Example 1) were added to a reaction container, and nitrogen was introduced after stirring and dissolving. 0.12 mmol of photoinitiator 2959 was added, and the mixture was irradiated under a 300 W high-pressure mercury lamp and stirred for reaction for 60 min to obtain a hyperbranched polyether amide.
[0042] (2) 1 kg of nylon 6, 100 g of hyperbranched polyether amide, and 3 g of antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C, and 250°C, respectively, and a nozzle temperature of 240°C. The screw speed was 100 r / min, and the mixture was extruded and then injection molded in an injection molding machine with a mold temperature of 90°C and an injection pressure of 80 MPa to obtain a nylon composite material.
[0043] Comparative Example 3
[0044] 1kg nylon 6, 100g KH570 modified glass fiber and 3g antioxidant 1010 were placed in a twin-screw extruder with barrel temperatures of 210°C, 235°C and 250°C, respectively, and a nozzle temperature of 240°C. The screw speed was 100r / min, and the mixture was extruded and then injection molded in an injection molding machine with a mold temperature of 90°C and an injection pressure of 80MPa to obtain a nylon composite material.
[0045] Table 1 Performance test of nylon composite materials
[0046]
[0047] After testing, the nylon composite materials of Examples 1-4 added with hyperbranched polyetheramide modified glass fibers have a good toughening and strengthening modification effect. The tensile strength is 98.3-125.0MPa, the elongation at break is 24.8-43.9%, and the notched impact strength is 22.0-35.4kJ / m 2 The bending strength is 144.5-186.1MPa, and the bending modulus is 3.95-9.80GPa. Compared with the pure nylon material in comparative example 1, the mechanical properties are significantly improved.
[0048] In comparative example 2, only hyperbranched polyetheramide was added without glass fiber, and the tensile and flexural strengths of the nylon material increased slightly, but the elongation at break and the notched impact strength were significantly improved. The toughening effect was very good.
[0049] In Comparative Example 3, only KH570-modified glass fiber is added. Although the glass fiber is modified by KH570, the interface bonding performance between KH570 and nylon 6 material is poor, so the compatibility between the glass fiber and nylon 6 is not well improved, resulting in the glass fiber not enhancing the mechanical strength of the nylon material.
[0050] The nylon composite material was dried and weighed, and then immersed in distilled water for 24 hours. After being taken out, the surface moisture was wiped dry, and the weight was weighed to calculate the water absorption rate.
[0051] Water absorption rate W = (m-m0) / m0×100%. m is the mass of the nylon material after absorbing water. m is the mass before absorbing water.
[0052] Table 1 Hydrophilic properties test of nylon materials
[0053] Water absorption (%) Example 1 7.9 Example 2 8.3 Example 3 9.6 Example 4 9.2 Comparative Example 1 7.4 Comparative Example 2 8.8 Comparative Example 3 7.0
[0054] The nylon composite materials of Examples 1-4 are added with hyperbranched polyetheramide modified glass fibers, which contain more hydrophilic ether bonds and can significantly improve the water absorption and hydrophilicity of the nylon material.
[0055] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A preparation process of a hyperbranched polyetheramide modified glass fiber reinforced nylon composite material, characterized in that: The preparation process comprises the following steps: Step S1, adding N,N-dimethylacetamide, ethylene glycol dimethacrylate, and mercapto ether amide polymerization monomer into a reaction container, stirring and dissolving, introducing nitrogen, adding photoinitiator 2959, irradiating under an ultraviolet light source, stirring and reacting for 60-90 minutes, then adding KH570 modified glass fiber, stirring and reacting for 20-40 minutes, adding methanol to the solution to precipitate a precipitate, filtering, washing with ethanol, and drying to obtain a hyperbranched polyether amide modified glass fiber; The structural formula of the mercaptoetheramide polymerization monomer is: ; Step S2, placing nylon 6, hyperbranched polyether amide modified glass fiber, and an antioxidant in a twin-screw extruder, blending and extruding, and then injection molding in an injection molding machine to obtain a hyperbranched polyether amide modified glass fiber reinforced nylon composite material; The preparation process of the mercapto ether amide polymerization monomer is: Step (1), adding ethanol, trimesic acid, and 1-amino-3,6,9-trioxaundecane-11-ol to a reaction vessel, adding glacial acetic acid dropwise, heating to 75-80° C., condensing and refluxing for 18-24 hours, concentrating the solvent until a precipitate is precipitated, filtering, washing with acetone, and drying to obtain an intermediate; Step (2), adding tetrahydrofuran, the intermediate, thioglycolic acid, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into a reaction vessel, reacting at room temperature for 10-15 hours, concentrating the solvent until a precipitate is precipitated, filtering, washing with acetone, and drying to obtain a thiol ether amide polymerization monomer; In the step (1), the ratio of trimesaldehyde to 1-amino-3,6,9-trioxaundecane-11-ol is 1 mol: (3.6-4.2) mol; In the step (2), the ratio of the intermediate, thioglycolic acid, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride is 1 mol: (3.3-3.9) mol: (3.3-3.9) mol; The preparation process of the KH570 modified glass fiber is as follows: add ethanol and KH570 into a reaction container, stir to dissolve, then add glass fiber, mix well, place the solution in an oven, dry at 100-120° C. for 2-3 hours, wash with ethanol, and dry to obtain the KH570 modified glass fiber.
2. The preparation process of the hyperbranched polyetheramide modified glass fiber reinforced nylon composite material according to claim 1, characterized in that: The ratio of ethylene glycol dimethacrylate, mercapto ether amide polymerization monomer, and KH570 modified glass fiber in the S1 is (1.2-1.4) mol: 1 mol: (300-600) g.
3. The preparation process of the hyperbranched polyetheramide modified glass fiber reinforced nylon composite material according to claim 1, characterized in that: The ultraviolet lamp source in S1 is a 300-800W high-pressure mercury lamp.
4. The preparation process of the hyperbranched polyetheramide modified glass fiber reinforced nylon composite material according to claim 1, characterized in that: The ratio of the hyperbranched polyetheramide modified glass fiber to nylon 6 in S2 is 1kg:(100-600)g.
5. The preparation process of the hyperbranched polyetheramide modified glass fiber reinforced nylon composite material according to claim 1, characterized in that: The barrel temperature of the twin-screw extruder in S2 is 210-250°C, the nozzle temperature is 240-250°C, and the screw speed is 60-120r / min.
6. The preparation process of the hyperbranched polyetheramide modified glass fiber reinforced nylon composite material according to claim 1, characterized in that: The mold temperature of the injection molding machine in S2 is 80-90° C., and the injection pressure is 80-100 MPa.