Laminated modified perfluorosulfonic acid ion exchange membrane and preparation method thereof
By adopting a laminated composite structure and phase conversion heat crosslinking process in the traditional perfluorosulfonic acid ion exchange membrane, the high swelling rate and high cost problems of the traditional membrane are solved, and the ultra-thinization and reliability of the functional layer are achieved. The ion transfer efficiency and energy efficiency of fuel cells and flow cells are improved.
Patent Information
- Application Number
- CN202410740369.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-06-08
AI Technical Summary
Traditional perfluorosulfonic acid ion exchange membranes have problems such as high swelling rate, large functional layer thickness, low ion transfer efficiency and high cost, which limits its application in fuel cells and flow batteries.
Using a laminated composite structure, the functional layer is ultra-thinized and defect self-repaired by the combination of a hydrophilic porous support film and a modified perfluorosulfonic acid ion exchange functional layer, and the phase conversion and heat crosslinking process are used to achieve ultra-thinization of the functional layer and self-repair of defects to reduce perfluorocarbon. The amount of sulfonic acid resin used and the bond strength between the materials is increased.
It significantly reduces the swelling rate and cost of the perfluorosulfonic acid ion exchange membrane, shortens the ion transfer path, improves the reliability and conductivity of the functional layer, and enhances the energy efficiency of the battery.
Smart Images

Figure CN118562191B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ion exchange membranes, in particular to a laminated modified perfluorosulfonic acid ion exchange membrane and a preparation method thereof. Background Art
[0002] Traditional perfluorosulfonic acid ion exchange membranes have two forms, one is a self-supporting form, that is, it is composed entirely of perfluorosulfonic acid resin, and the other is a polymer membrane or mesh supported form, called a "filled composite" ion exchange membrane, that is, the perfluorosulfonic acid resin is filled in the pores of the membrane or mesh and wrapped on both surfaces; traditional perfluorosulfonic acid ion exchange membrane preparation methods mainly include the salivation method and the hot melt method.
[0003] The common problems of perfluorosulfonic acid ion exchange membranes manufactured by prior art are: ① The swelling rate of the product is relatively high after being immersed in electrolyte or water, the swelling rate index of supported membrane or net is 4%-5%, and the swelling rate index of self-supporting membrane is 8%-12%. In actual application, the dry and wet dimensions of the membrane are unstable; ② The functional layer thickness of the perfluorosulfonic acid ion exchange membrane is large, and the hydrogen ion transfer path is long. For example, the thickness of the membrane functional layer used for fuel cells is 25μm-50μm, and the thickness of the membrane functional layer used for flow batteries is 50μm-100μm. Therefore, although the conductivity of the ion exchange membrane is not low, the efficiency of ion transfer is still not high; ③ The content of perfluorosulfonic acid resin per unit area of the ion exchange membrane is large. Perfluorosulfonic acid resin is a polymer material with a relatively complex synthesis process and a high market price. The resin content of the ion exchange membrane is generally 30g / m 2 -80g / m 2 The cost of a single perfluorosulfonic acid resin main material seriously restricts the large-scale promotion and use of this type of membrane.
[0004] In view of this, there is an urgent need to develop a laminated modified perfluorosulfonic acid ion exchange membrane and a preparation method thereof to overcome the above-mentioned defects. Summary of the invention
[0005] The purpose of the present invention is to disclose a laminated modified perfluorosulfonic acid ion exchange membrane and a preparation method thereof.
[0006] The first object of the present invention is to develop a laminated modified perfluorosulfonic acid ion exchange membrane.
[0007] The second object of the present invention is to develop a method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane.
[0008] To achieve the above first invention objective, the present invention provides a laminated modified perfluorosulfonic acid ion exchange membrane, comprising a hydrophilic porous support membrane and a modified perfluorosulfonic acid ion exchange functional layer disposed on the surface of the porous support membrane;
[0009] The modified perfluorosulfonic acid ion exchange functional layer is attached to one surface of the porous support membrane through phase conversion and thermal cross-linking processes.
[0010] Preferably, the porous support membrane is a polytetrafluoroethylene membrane or a polypropylene membrane;
[0011] The porous support membrane has a thickness of 20 μm-100 μm, a pore size of 0.02 μm-1.0 μm, a porosity of 35%-80%, and a water spontaneous wetting time of less than 5 seconds.
[0012] Preferably, the loading amount of the modified perfluorosulfonic acid ion exchange functional layer is 1 g / m 2 -5g / m 2 .
[0013] Preferably, the total thickness of the porous support membrane and the modified perfluorosulfonic acid ion exchange functional layer is 21 μm-103 μm.
[0014] Based on the same inventive principle, in order to achieve the above second inventive object, the present invention provides a method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane, comprising the following steps:
[0015] Step S1: immersing the hydrophilic porous support membrane into a perfluorosulfonic acid resin modified liquid having a mass ratio of 1% to 5%, and quantifying it with a scraper to obtain an impregnated membrane;
[0016] Step S2: Compounding a non-porous film on one surface of the impregnated membrane, and passing the compounded membrane through a first evaporation box, a second evaporation box, and a third evaporation box with increasing temperatures at a speed of 0.5 m / min-3 m / min, to evaporate the solvent in the perfluorosulfonic acid resin modified liquid on one side, thereby obtaining a composite membrane;
[0017] Step S3: the composite membrane passes through a reaction box at a temperature of 100° C. to 160° C. at a speed of 0.5 m / min to 3 m / min to be chemically cross-linked, and the non-porous film is peeled off to obtain a laminated modified perfluorosulfonic acid ion exchange membrane.
[0018] Based on the same inventive principle, in order to achieve the above second inventive object, the present invention also provides a method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane, comprising the following steps:
[0019] Step A1: coating a surface of a hydrophilic porous support membrane with a perfluorosulfonic acid resin modification liquid having a mass ratio of 1% to 5% to obtain a coating membrane;
[0020] Step A2: Compounding a non-porous film on one surface of the coating film, and passing the compounded film through a first evaporation box, a second evaporation box, and a third evaporation box with gradually increasing temperatures at a speed of 0.5 m / min-3 m / min, to evaporate the solvent in the perfluorosulfonic acid resin modified liquid on one side, thereby obtaining a composite film;
[0021] Step A3: The composite membrane passes through a reaction box at a temperature of 100° C. to 160° C. at a speed of 0.5 m / min to 3 m / min to be chemically cross-linked, and the non-porous film is peeled off to obtain a laminated modified perfluorosulfonic acid ion exchange membrane.
[0022] Preferably, the temperature of the first evaporator box is 30°C-45°C, the temperature of the second evaporator box is 50°C-65°C, the temperature of the third evaporator box is 70°C-85°C, the humidity of the first evaporator box, the second evaporator box and the third evaporator box is 5%-15%, and the wind speed is 0.5m / s-2m / s.
[0023] Preferably, the non-porous film is a PET non-porous film, a PP non-porous film or a stainless steel non-porous film.
[0024] Preferably, the loading amount of the perfluorosulfonic acid resin modified liquid on the porous support membrane is 40 ml / m 2 -150ml / m 2 .
[0025] Preferably, the perfluorosulfonic acid resin modified liquid comprises a perfluorosulfonic acid resin modified material and a solvent;
[0026] The perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water;
[0027] Or, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated titanium and glutaraldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water;
[0028] Alternatively, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and maleic acid in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) Compared with the existing "filling composite" structure of perfluorosulfonic acid ion exchange membrane, the present invention adopts a novel "stacked composite" structure to make the perfluorosulfonic acid ion exchange functional layer ultra-thin. Ultra-thinness helps to reduce the swelling rate of the perfluorosulfonic acid ion exchange membrane, greatly shorten the ion transfer path, and greatly reduce the amount of perfluorosulfonic acid ion resin used, thereby greatly reducing the cost of the perfluorosulfonic acid ion exchange membrane. At the same time, the film formation process of the perfluorosulfonic acid ion exchange functional layer is controlled by single-sided phase transformation and thermal cross-linking process, so that the perfluorosulfonic acid ion exchange functional layer can achieve defect self-repair and ensure the reliability of the ultra-thin perfluorosulfonic acid ion exchange functional layer.
[0031] (2) The functional groups carried by the mixture in the perfluorosulfonic acid resin modified liquid form coordination-complexation-pre-crosslinking effects, achieving the following technical effects: the self-assembly deposition of the perfluorosulfonic acid resin modified material enables the defects on the perfluorosulfonic acid ion exchange functional layer to be automatically repaired, significantly improving the reliability of the ultra-thin perfluorosulfonic acid ion exchange functional layer; the perfluorosulfonic acid ion exchange functional layer forms an indiscriminate, saturated point-like physical anchoring with the pore fibers on the surface of the hydrophilic porous support membrane, greatly increasing the bonding strength between the two materials and maximizing the effective transfer channel; the perfluorosulfonic acid resin modified material residue in the hydrophilic porous support membrane body is very low, and no new ion transfer resistance is generated. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a cross-sectional schematic diagram of the laminated modified perfluorosulfonic acid ion exchange membrane of the present invention.
[0033] Figure 2 The present invention is a flow chart of the method for preparing the laminated modified perfluorosulfonic acid ion exchange membrane.
[0034] Figure 3 The figure is a schematic diagram of the cross-linking principle of the modified perfluorosulfonic acid ion exchange functional layer of the present invention.
[0035] Figure 4 The present invention is a flow chart of the method for preparing the laminated modified perfluorosulfonic acid ion exchange membrane.
[0036] Figure 5 This is an electron microscope image of the surface of the hydrophilic polytetrafluoroethylene membrane of the present invention.
[0037] Figure 6 This is an electron microscope image of the surface of the modified perfluorosulfonic acid ion exchange functional layer of the present invention.
[0038] Among them, 1. a porous support membrane; 2. a modified perfluorosulfonic acid ion exchange functional layer. DETAILED DESCRIPTION
[0039] The present invention is described in detail below in conjunction with the various embodiments shown in the accompanying drawings, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0040] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0041] The specific implementation process of the present invention is described below through multiple embodiments.
[0042] Embodiment 1:
[0043] See also Figure 1 This embodiment discloses a laminated modified perfluorosulfonic acid ion exchange membrane, comprising a hydrophilic porous support membrane 1 and a modified perfluorosulfonic acid ion exchange functional layer 2 arranged on the surface of the porous support membrane 1; the modified perfluorosulfonic acid ion exchange functional layer 2 is attached to one surface of the porous support membrane 1 through phase inversion and thermal cross-linking processes.
[0044] Specifically, the porous support membrane 1 is a polytetrafluoroethylene membrane or a polypropylene membrane, the porous support membrane has a thickness of 20 μm-100 μm, a pore size of 0.02 μm-1.0 μm, a porosity of 35%-80%, a water spontaneous wetting time of less than 5 s, and a loading amount of the modified perfluorosulfonic acid ion exchange functional layer of 1 g / m 2 -5g / m 2 The total thickness of the porous support membrane and the modified perfluorosulfonic acid ion exchange functional layer is 21 μm-103 μm.
[0045] See Table 1, which shows the parameter test values of the laminated modified perfluorosulfonic acid ion exchange membrane. The indicators of the porous support membranes of Examples 1 to 4 are: pore size 0.05 μm, porosity 40%-65%, and water spontaneous wetting time 3 s; Comparative Examples 1 and 2 adopt a "filling composite" structure, and the perfluorosulfonic acid resin not only exists on the surface of the porous support membrane, but also fills the pores of the porous support membrane, so that the entire exchange membrane has an ion interaction function, that is, the entire exchange membrane becomes an ion exchange functional layer. In Examples 1 to 4, the water swelling rate of the stacked modified perfluorosulfonic acid ion exchange membrane is less than 1%, the water swelling rate of Comparative Examples 1 and 2 is 3.57% and 1.13%, respectively, the dimensional stability is lower than that of the exchange membranes of Examples 1 to 4, and the functional layer loading of Comparative Examples 1 to 2 is 12 to 28 times higher than that of Examples 1 to 4. The cost of the perfluorosulfonic acid resin modified material used in Comparative Examples 1 to 2 is much higher than that of the exchange membranes of Examples 1 to 4. The thickness of the perfluorosulfonic acid ion exchange functional layer of the exchange membranes of Examples 1 to 4 is only 1 μm-3 μm, while the thickness of the ion exchange functional layer of Comparative Examples 1 to 2 is 36 μm and 65 μm, which is much larger than the thickness of the ion exchange functional layer of Examples 1 to 4. Through this embodiment, the ultra-thin ion exchange functional layer greatly reduces the ion exchange path.
[0046] Table 1 Parameter test values of laminated modified perfluorosulfonic acid ion exchange membrane
[0047]
[0048] See Table 2, which shows the application performance test values of the laminated modified perfluorosulfonic acid ion exchange membrane.
[0049] Table 2 Application performance test values of laminated modified perfluorosulfonic acid ion exchange membrane
[0050]
[0051] The existing perfluorosulfonic acid ion exchange membrane has a "filling composite" structure, in which the inside and both surfaces of the supporting membrane have perfluorosulfonic acid ion exchange functional materials, resulting in a long ion transfer path, high cost and high water absorption and swelling rate. To overcome the above defects, this embodiment adopts a new "stacked composite" structure to make the perfluorosulfonic acid ion exchange functional layer ultra-thin, and the loading amount of the perfluorosulfonic acid ion exchange functional layer is only 1g / m 2 -5g / m 2The thickness of the functional layer does not exceed 3μm. Ultra-thinning helps to reduce the swelling rate of the perfluorosulfonic acid ion exchange membrane, which is below 1%. The size is stable, the ion transfer path is greatly shortened, and the use of perfluorosulfonic acid ion resin is greatly reduced, thereby greatly reducing the cost of the perfluorosulfonic acid ion exchange membrane. At the same time, the film formation process of the perfluorosulfonic acid ion exchange functional layer is controlled by single-sided phase transformation and thermal cross-linking process, so that the perfluorosulfonic acid ion exchange functional layer can achieve defect self-repair and ensure the reliability of the use of the ultra-thin perfluorosulfonic acid ion exchange functional layer.
[0052] According to the methods specified in GB / T 20042.3-2022 Proton Exchange Membrane Fuel Cell Part 3: Proton Exchange Membrane Test Methods and NB / T 42080-2023 General Technical Requirements and Test Methods for Ion Conducting Membranes for All-vanadium Redox Flow Batteries, the test data is shown in Table 1. After testing, the thickness of the laminated modified perfluorosulfonic acid ion exchange membrane is 20μm-100μm, and the modified material loading is 1g / m 2 -5 g / m 2 , longitudinal and transverse tensile strength, longitudinal and transverse elongation at break, water swelling rate 0.75%, longitudinal and transverse thermal deformation and other indicators are shown in Table 1. The laminated modified perfluorosulfonic acid ion exchange membrane was used as the diaphragm of the iron-chromium flow battery for charge and discharge tests. The test results are shown in Table 2, where the positive and negative electrolytes are equal volumes of FeCl2 / CrCl3 / HCl, the positive and negative electrodes are treated graphite carbon felt, and the charge and discharge current is 100mA / cm 2 , charging cut-off voltage 1.25V, discharging cut-off voltage 0.3V, battery coulombic efficiency 96.3%-96.6%, voltage efficiency 82.6%-86.5%, it can be seen that although Example 1 and Example 2 use less functional layer loading than Example 2, the energy efficiency (product of coulombic efficiency and voltage efficiency) of the assembled battery is improved at the same time, indicating that Example 1 and Example 2 have the advantages of low cost and high energy efficiency; stacked modified perfluorosulfonic acid ion exchange membrane is used as the diaphragm of vanadium liquid flow battery for charge and discharge test, the test results are shown in Table 2, wherein the positive and negative electrolytes are equal volumes of VO2 + / VO2 + / H2SO4 / / V3 + / V2 + / H2SO4, the positive and negative electrodes are treated graphite carbon felt, the charge and discharge current is 50mA / cm 2 , the charging cut-off voltage is 1.85V, the discharging cut-off voltage is 0.8V, the coulombic efficiency of the battery is 96.1%-96.7%, and the voltage efficiency is 82.2%-85.6%. It can be seen that although Examples 3 and 4 use less functional layer loading than Example 1, the energy efficiency (the product of coulombic efficiency and voltage efficiency) of the assembled batteries is basically the same, indicating that Examples 3 and 4 have the advantage of low cost.
[0053] Embodiment 2:
[0054] See also Figure 2 This embodiment discloses a method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane, comprising the following steps:
[0055] Step S1: immersing a hydrophilic porous support membrane into a perfluorosulfonic acid resin modification liquid with a mass ratio of 1%-5%, and quantifying it with a scraper to obtain an impregnated membrane; specifically, the hydrophilic porous support membrane is preferably a hydrophilic polytetrafluoroethylene membrane or a hydrophilic polypropylene membrane, the porous support membrane has a thickness of 20μm-100μm, a pore size of 0.02μm-1.0μm, a porosity of 35%-80%, and a water spontaneous wetting time of less than 5s; the perfluorosulfonic acid resin modification liquid includes a perfluorosulfonic acid resin modification material and a solvent; the perfluorosulfonic acid resin modification material includes a perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), the solvent includes ethanol, dimethyl sulfoxide and water, the triethanolamine chelated zirconium can also be replaced by triethanolamine chelated titanium, and the terephthalaldehyde can also be replaced by glutaraldehyde or maleic acid.
[0056] The preparation process of the perfluorosulfonic acid resin modified liquid with a mass ratio of 1%-5% is as follows:
[0057] Step B1: adding water and dimethyl sulfoxide in a mass ratio of 100:(5-25) to a first corrosion-resistant reaction kettle, and slowly adding polyvinyl alcohol in a mass ratio of 0.4%-0.8% under stirring, stirring for 30min-60min and then standing to swell for 2h-3h; heating to 70°C-90°C under stirring until the polyvinyl alcohol solution is completely transparent, continuing to stir for 1h-2h and cooling the polyvinyl alcohol solution to 30°C to prepare a first component;
[0058] Step B2: Add ethanol, terephthalaldehyde, and triethanolamine chelated zirconium alcohol solution in a mass ratio of 100: (0.105-0.320): (0.160-0.480) to the second corrosion-resistant reaction kettle, slowly add water and perfluorosulfonic acid alcohol aqueous solution after complete dissolution, and stir for 2h-3h to prepare the second component;
[0059] Step B3: Stir the first component and slowly add the second component into the first component, and continue stirring for 2h-3h;
[0060] Step B4: Filter with a filter with a precision of 3 μm-10 μm to obtain a perfluorosulfonic acid resin modified liquid with a mass fraction of 1%-5%.
[0061] In step S1, perfluorosulfonic acid resin is used as the main polymer, polyvinyl alcohol is used as the compound polymer, triethanolamine chelated zirconium or triethanolamine chelated titanium is used as the first cross-linking agent, and terephthalaldehyde, glutaraldehyde or maleic acid is used as the second cross-linking agent. The above substances are fully dissolved and dispersed in the modified liquid, and the functional groups they carry form coordination-complexation-pre-cross-linking effects. The hydroxyl groups in polyvinyl alcohol interact with the sulfonic acid groups in the perfluorosulfonic acid resin to form a hydrogen bond pre-cross-linking network, and the triethanolamine chelated zirconium / titanium has a strong affinity with the perfluorosulfonic acid resin and polyvinyl alcohol, which can form a stable coordination-complexation, and further a chemical cross-linking reaction can be carried out; on the other hand, polyvinyl alcohol can make the modified perfluorosulfonic acid ion exchange functional layer have higher proton conductivity and defect self-repairing ability, triethanolamine chelated zirconium / titanium has delayed cross-linking performance and has a strong chelation effect with the hydrophilic surface of the polytetrafluoroethylene microporous membrane, and the high boiling point of terephthalaldehyde / maleic acid can effectively increase the temperature of the subsequent cross-linking reaction and shorten the reaction time; the above effects and characteristics are in the perfluorosulfonic acid The acid resin modified liquid is stable during the single-sided phase transformation and chemical cross-linking film-forming process, and has an indispensable preset effect on the subsequent solid-state chemical cross-linking; the solvent includes ethanol, dimethyl sulfoxide, and water. The solvent is used as a carrier of the modified material. The primary function is to fully dissolve the modified material. Therefore, a composite solvent is used. The basis for adjusting the ratio is to fully stretch the polymer chain segments, increase the freedom of assembly-coordination-complexation between functional groups, improve the permeability of the polymer solution to the base membrane, facilitate programmed evaporation, facilitate coating uniformity, and ensure the solution replacement defoaming ability. The perfluorosulfonic acid resin modified liquid adopts a low concentration strategy, and the mass concentration of the perfluorosulfonic acid resin modified material is controlled at 1-5%.
[0062] Step S2: Compounding a non-porous film on one surface of the impregnated membrane, and passing the compounded membrane through a first evaporation box, a second evaporation box, and a third evaporation box with increasing temperatures at a speed of 0.5 m / min-3 m / min, to evaporate the solvent in the perfluorosulfonic acid resin modified liquid on one side, thereby obtaining a composite membrane;
[0063] Specifically, since the porous support membrane and the perfluorosulfonic acid resin modified liquid have a very low contact angle, when the hydrophilic porous support membrane is immersed in the perfluorosulfonic acid resin modified liquid, the perfluorosulfonic acid resin modified liquid is quickly filled into the porous support membrane under the strong capillary force of the porous support membrane. After the impregnation is completed, the perfluorosulfonic acid resin modified liquid is evenly laid on the inside and both surfaces of the porous support membrane, and the impregnated membrane is formed under the quantitative operation of the scraper. The loading amount of the perfluorosulfonic acid resin modified liquid on both surfaces of the impregnated membrane is 40ml / m 2 -150ml / m 2The non-porous film is a PET non-porous film, a PP non-porous film or a stainless steel non-porous film. The non-porous film is taken as an example for explanation. A surface evaporation mass transfer method is adopted. The impregnated membrane makes the solvent in the perfluorosulfonic acid resin modified liquid evaporate according to a predetermined procedure in a space where the temperature, humidity and wind speed are controlled, so as to realize phase transformation into a membrane. Specifically, a non-porous film is composited on one surface of the impregnated membrane. The non-porous film limits the evaporation of the solvent on this surface, and drives the solvent to evaporate through a surface without the composite non-porous film. During the single-surface solvent evaporation process, the perfluorosulfonic acid resin modified liquid continuously migrates to the evaporation surface through the membrane pores of the porous support membrane under the action of the capillary attraction (effect) generated by the micropores of the porous support membrane, and finally gathers on a surface with evaporation. After the solvent evaporation is completed, a laminated modified perfluorosulfonic acid ion exchange membrane is obtained.
[0064] Specifically, the temperature of the first evaporation box is 30°C-45°C, the temperature of the second evaporation box is 50°C-65°C, the temperature of the third evaporation box is 70°C-85°C, the humidity of the first evaporation box, the second evaporation box and the third evaporation box is 5%-15%, and the wind speed is 0.5m / s-2m / s; the composite film passes through the first evaporation box, the second evaporation box and the third evaporation box with increasing temperatures at a speed of 0.5m / min-3m / min, and the solvent on the single surface of the composite film evaporates first, so that the whole film is The surface of the fluorosulfonic acid resin modified liquid rapidly undergoes phase transformation to form a cortex of the perfluorosulfonic acid modified material. The solvent in the main body of the perfluorosulfonic acid resin modified liquid continuously diffuses into the cortex under the driving force of the concentration difference, causing the perfluorosulfonic acid resin modified material to continuously undergo phase transformation on the inner surface of the cortex, forming a self-assembled deposition of the perfluorosulfonic acid resin modified material. The perfluorosulfonic acid resin modified liquid continuously migrates and is transported to the surface where the phase transformation occurs under the capillary attraction of the hydrophilic polytetrafluoroethylene membrane pores, ultimately achieving layered superposition and aggregation of the perfluorosulfonic acid resin modified material. The loading amount of the perfluorosulfonic acid resin modified material is controlled at 1g / m 2 -5g / m 2 Compared with the existing "filling composite" structure of perfluorosulfonic acid resin, the amount of perfluorosulfonic acid resin used is reduced by at least 10 times, which has a very high cost-effectiveness. The single-sided phase transformation produces at least the following three beneficial results: ① The self-assembly deposition of the perfluorosulfonic acid resin modified material automatically repairs the defects of the modified perfluorosulfonic acid ion exchange functional layer, which significantly improves the reliability of the ultra-thin functional layer; ② The modified perfluorosulfonic acid ion exchange functional layer forms an indifferent, saturated point-like physical anchor with the surface pore fibers of the hydrophilic polytetrafluoroethylene microporous membrane, which greatly increases the bonding strength between the two materials and maximizes the effective transmission channel; ③ The amount of perfluorosulfonic acid modified material remaining in the main body of the hydrophilic polytetrafluoroethylene microporous membrane is very low, and no new transmission resistance is generated.
[0065] Step S3: The composite membrane passes through a reaction box with a temperature of 100℃-160℃ at a speed of 0.5m / min-3m / min, undergoes chemical crosslinking, and peels off the non-porous film to obtain a laminated modified perfluorosulfonic acid ion exchange membrane. Specifically, perfluorosulfonic acid resin and polyvinyl alcohol are the two central substances of the molecular crosslinking structure, triethanolamine chelated zirconium and terephthalaldehyde are a group of composite crosslinking agents, and the chemical crosslinking reaction is initiated by heating. The water, alcohol products produced during the crosslinking reaction and a small amount of solvent remaining in the phase-converted membrane are discharged from the modified perfluorosulfonic acid ion exchange functional layer by diffusion. Since high-boiling-point dimethyl sulfoxide is added to the perfluorosulfonic acid resin modified liquid, the crosslinking reaction presents three processes: semi-solid phase thermal chemical crosslinking, solid phase thermal chemical crosslinking and stress relief. Since the composition, distribution and interaction of the four substances, namely, perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde, have been preset in the preparation of perfluorosulfonic acid resin modified liquid and the phase transformation film-forming process, the cross-linking reaction is highly controllable, the reaction product is uniform, and the process is convenient and simple.
[0066] Through steps S1 to S3, a laminated modified perfluorosulfonic acid ion exchange membrane as shown in Example 1 is prepared. In Example 1, the perfluorosulfonic acid resin modified material includes perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde in a mass ratio of 100:9:5:3; in Example 2, the perfluorosulfonic acid resin modified material includes perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated titanium and glutaraldehyde in a mass ratio of 100:10:6:6; in Example 3, the perfluorosulfonic acid resin modified material includes perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated titanium and glutaraldehyde in a mass ratio of 100:11:7:5 Acid resin, polyvinyl alcohol, triethanolamine chelated titanium and maleic acid; in Example 4, the perfluorosulfonic acid resin modified material includes perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and maleic acid in a mass ratio of 100:8:4:2; the parameter test values of the laminated modified perfluorosulfonic acid ion exchange membrane are shown in Table 1, and the application performance test values of the laminated modified perfluorosulfonic acid ion exchange membrane are shown in Table 2. Taking the porous support membrane parameters of Example 1 in Table 1 as an example, the porous support membrane is a hydrophilic polytetrafluoroethylene membrane, and the electron microscope image of the surface of the hydrophilic polytetrafluoroethylene membrane in Example 1 is shown in Figure 5 The cross-linking principle of the modified perfluorosulfonic acid ion exchange functional layer after cross-linking can be found in Figure 3 , Figure 3 In the invention, the composite crosslinking agent is triethanolamine chelated zirconium and terephthalaldehyde, and R1, R2 and R3 are independent long-chain fluoroalkyl groups. Figure 3 The chemical formula structure in the modified perfluorosulfonic acid ion exchange functional layer forms a three-dimensional network structure. Therefore, the swelling rate of the modified perfluorosulfonic acid ion exchange functional layer is low. At the same time, polyvinyl alcohol not only provides a monomer component for cross-linking, but also acts as a "medium" for cross-linking of other components, which is beneficial to improving proton conductivity and defect self-repair. The electron microscope image of the surface of the modified perfluorosulfonic acid ion exchange functional layer can be found in Figure 6 ,from Figure 6 It can be seen that the surface of the modified perfluorosulfonic acid ion exchange functional layer is complete and uniform, indicating that the method for preparing the laminated modified perfluorosulfonic acid ion exchange membrane of Example 2 is stable and reliable.
[0067] Embodiment three:
[0068] See also Figure 4 This embodiment discloses a method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane, comprising the following steps:
[0069] Step A1: coating a surface of a hydrophilic porous support membrane with a perfluorosulfonic acid resin modification liquid having a mass ratio of 1% to 5% to obtain a coating membrane;
[0070] Step A2: Compounding a non-porous film on one surface of the coating film, and passing the compounded film through a first evaporation box, a second evaporation box, and a third evaporation box with gradually increasing temperatures at a speed of 0.5 m / min-3 m / min, to evaporate the solvent in the perfluorosulfonic acid resin modified liquid on one side, thereby obtaining a composite film;
[0071] Step A3: The composite membrane passes through a reaction box at a temperature of 100° C. to 160° C. at a speed of 0.5 m / min to 3 m / min to be chemically cross-linked, and the non-porous film is peeled off to obtain a laminated modified perfluorosulfonic acid ion exchange membrane.
[0072] The difference from Example 2 is that Example 3 does not adopt an immersion method, but a coating method, that is, in step A1, a perfluorosulfonic acid resin modified liquid with a mass ratio of 1%-5% is coated on one surface of the hydrophilic porous support membrane. Since the porous support membrane is a hydrophilic membrane and has abundant pores, the coated perfluorosulfonic acid resin modified liquid will penetrate into the other surface, and finally both surfaces of the porous support membrane are coated with the perfluorosulfonic acid resin modified liquid. Compared with the immersion method, the coating method contains almost no bubbles in the perfluorosulfonic acid resin modified liquid, and a smaller amount of perfluorosulfonic acid resin modified liquid can also ensure the reliability of the use of the ion exchange membrane. Therefore, the amount of perfluorosulfonic acid resin modified liquid used is less and the preparation cost is lower; the preparation method of the perfluorosulfonic acid resin modified liquid refers to steps B1 to B4 of Example 1, and the subsequent A2 and step S2 adopt the same single-sided phase transformation method, and the subsequent A3 and step S3 adopt the same chemical cross-linking method, and the same parts are not repeated.
[0073] The method for preparing the laminated modified perfluorosulfonic acid ion exchange membrane disclosed in this embodiment has the same technical solution as that in the second embodiment. Please refer to the second embodiment and will not be described in detail here.
Claims
1. Laminated modified perfluorosulfonic acid ion exchange membrane, It is characterized in that It comprises a hydrophilic porous support membrane and a modified perfluorosulfonic acid ion exchange functional layer arranged on the surface of the porous support membrane; The modified perfluorosulfonic acid ion exchange functional layer is attached to one surface of the porous support membrane through phase conversion of perfluorosulfonic acid resin modified liquid and thermal crosslinking process; The thickness of the modified perfluorosulfonic acid ion exchange functional layer does not exceed 3 μm; The loading amount of the modified perfluorosulfonic acid ion exchange functional layer is 1 g / m 2 -5g / m 2 ; The perfluorosulfonic acid resin modified liquid comprises a perfluorosulfonic acid resin modified material and a solvent; The perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water; Or, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated titanium and glutaraldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water; Alternatively, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and maleic acid in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water.
2. The laminated modified perfluorosulfonic acid ion exchange membrane according to claim 1, It is characterized in that The porous support membrane is a polytetrafluoroethylene membrane or a polypropylene membrane; The porous support membrane has a thickness of 20 μm-100 μm, a pore size of 0.02 μm-1.0 μm, a porosity of 35%-80%, and a spontaneous water wetting time of less than 5 seconds.
3. The laminated modified perfluorosulfonic acid ion exchange membrane according to claim 1 or 2, It is characterized in that The total thickness of the porous support membrane and the modified perfluorosulfonic acid ion exchange functional layer is 21 μm-103 μm.
4. Preparation method of laminated modified perfluorosulfonic acid ion exchange membrane, It is characterized in that The following steps are involved: Step S1: immersing the hydrophilic porous support membrane into a perfluorosulfonic acid resin modification liquid having a mass ratio of 1% to 5%, and quantifying it with a scraper to obtain an impregnated membrane; Step S2: Compounding a non-porous film on one surface of the impregnated membrane, and passing the compounded membrane through a first evaporation box, a second evaporation box, and a third evaporation box with increasing temperatures at a speed of 0.5 m / min-3 m / min, to evaporate the solvent in the perfluorosulfonic acid resin modified liquid on one side, thereby obtaining a composite membrane; Step S3: the composite membrane passes through a reaction box at a temperature of 100° C. to 160° C. at a speed of 0.5 m / min to 3 m / min to be chemically cross-linked, and the non-porous film is peeled off to obtain a laminated modified perfluorosulfonic acid ion exchange membrane; The loading amount of the perfluorosulfonic acid resin modified liquid on the porous support membrane is 40 ml / m 2 -150ml / m 2 ; The perfluorosulfonic acid resin modified liquid comprises a perfluorosulfonic acid resin modified material and a solvent; The perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water; Or, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated titanium and glutaraldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water; Alternatively, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and maleic acid in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water.
5. Preparation method of laminated modified perfluorosulfonic acid ion exchange membrane, It is characterized in that The following steps are involved: Step A1: coating a surface of a hydrophilic porous support membrane with a perfluorosulfonic acid resin modification liquid having a mass ratio of 1% to 5% to obtain a coating membrane; Step A2: Compounding a non-porous film on one surface of the coating film, and passing the compounded film through a first evaporation box, a second evaporation box, and a third evaporation box with gradually increasing temperatures at a speed of 0.5 m / min-3 m / min, to evaporate the solvent in the perfluorosulfonic acid resin modified liquid on one side, thereby obtaining a composite film; Step A3: the composite membrane passes through a reaction box at a temperature of 100° C. to 160° C. at a speed of 0.5 m / min to 3 m / min to be chemically cross-linked, and the non-porous film is peeled off to obtain a laminated modified perfluorosulfonic acid ion exchange membrane; The loading amount of the perfluorosulfonic acid resin modified liquid on the porous support membrane is 40 ml / m 2 -150ml / m 2 ; The perfluorosulfonic acid resin modified liquid comprises a perfluorosulfonic acid resin modified material and a solvent; The perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and terephthalaldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water; Or, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated titanium and glutaraldehyde in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water; Alternatively, the perfluorosulfonic acid resin modified material comprises perfluorosulfonic acid resin, polyvinyl alcohol, triethanolamine chelated zirconium and maleic acid in a mass ratio of 100:(5-15):(4-8):(2-6), and the solvent comprises ethanol, dimethyl sulfoxide and water.
6. The method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane according to claim 4 or 5, It is characterized in that The temperature of the first evaporator box is 30°C-45°C, the temperature of the second evaporator box is 50°C-65°C, the temperature of the third evaporator box is 70°C-85°C, the humidity of the first evaporator box, the second evaporator box and the third evaporator box is 5%-15%, and the wind speed is 0.5m / s-2m / s.
7. The method for preparing a laminated modified perfluorosulfonic acid ion exchange membrane according to any one of claims 4 or 5, It is characterized in that The non-porous film is a PET non-porous film, a PP non-porous film or a stainless steel non-porous film.