Preparation method and application of BFAN-based ceramic particles-PVDF polymer filled porous aerogel
Through the method of filling porous aerogels with BFAN-based ceramic particles and PVDF polymer, the problems of high hardness, low output performance and poor environmental friendliness of existing piezoelectric materials in wearable devices have been solved, and efficient piezoelectric sensor preparation has been achieved. , has good recoverability and sensing functions, and is suitable for use in the medical care field.
Patent Information
- Application Number
- CN202411056113.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Existing piezoelectric materials in wearable electronic devices have problems such as high hardness, low breakdown electric field, high lead content, unfriendly environment, low output performance, and difficulty in achieving power generation and pressure sensing at the same time.
Using the preparation method of BFAN-based ceramic particles-PVDF polymer filled porous aerogels, lead-free BFAN-based nanoceramic particles were prepared through the sol-gel method, and mixed with PVDF polymer and ball milled, combined with the porous aerogel framework structure , forming an efficient piezoelectric sensor.
It improves the recoverability of the material and the piezoelectric power generation output performance, realizes a highly stable piezoelectric sensor, combines the sensing function, extends the service life of the sensor, and shows great potential in the field of medical care.
Smart Images

Figure CN118562239B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of piezoelectric sensor preparation, and in particular to a preparation method and application of a BFAN-based ceramic particle-PVDF polymer filled porous aerogel. Background Art
[0002] With the continuous progress and development of economic and ecological civilization construction, human demand for energy continues to grow. In particular, traditional energy is inevitably facing problems such as environmental pollution and increasing depletion. Therefore, people's demand for green new energy is becoming more and more urgent.
[0003] In recent years, piezoelectric materials have attracted wide attention in the field of self-powered and sensing due to their excellent electromechanical conversion performance. Piezoelectric materials are small in size, light in weight, and easy to integrate. They can collect various mechanical energies from the environment and biological movements and convert them into electrical energy, so they can be used in miniaturized electronic products. For example, sensors based on piezoelectric materials can detect and output mechanical vibrations and piezoelectricity in real time without external power supply.
[0004] Conventional piezoelectric ceramics have high hardness and low breakdown electric field, and most of the materials contain lead, which poses a threat to the human body and the environment and is not conducive to practical applications. Pure flexible polymer piezoelectric materials have low output performance and output power of only microwatts, which affects their applicability as a direct power source. In order to provide continuous power to wearable electronic devices, some researchers have combined traditional piezoelectric ceramics with flexible polymers to prepare flexible piezoelectric devices, but this type of flexible piezoelectric device faces difficulties such as high conductivity, low ductility, and structural collapse. In addition, current flexible piezoelectric sensors cannot simultaneously have the functions of power generation and pressure sensing. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a BFAN-based ceramic particle-PVDF polymer filled porous aerogel and its application. The prepared aerogel can improve the recoverability of the material and the output performance of piezoelectric power generation, and also has a sensing function, and can be used to prepare a high-stability piezoelectric sensor.
[0006] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:
[0007] A method for preparing a BFAN-based ceramic particle-PVDF polymer filled porous aerogel, the preparation method comprising the following steps:
[0008] S1, preparing a first solution by mixing polyvinyl alcohol, deionized water and borax in a mass ratio of 15:100:1.5 for standby use;
[0009] S2, mixing the first solution with the cellulose nanofiber solution, stirring and reacting at 75-85° C. for 2-5 minutes to obtain a colloidal slurry;
[0010] S3, coating the colloidal slurry and drying it to obtain a gel film, freeze-drying the gel film at -80°C for 10-14h, and then soaking and salting out with sodium persulfate to obtain a porous aerogel framework structure membrane;
[0011] S4, preparing 0.9BiFeO3-0.1AgNbO3 BFAN-based nano-ceramic particles by sol-gel method;
[0012] S5, mixing polyvinylidene fluoride powder and N,N-dimethylformamide solvent at a ratio of 0.5 g:10 ml, and stirring at 50-60° C. for 16 minutes to obtain a transparent solution;
[0013] S6, adding 0wt%-60wt% of BFAN-based ceramic particles to the above transparent solution to prepare a PVDF-BFAN mixed solution, placing the mixed solvent in an agate ball milling jar and performing high-energy ball milling at a speed of 200-750 rpm for 30 minutes to obtain a mixed slurry;
[0014] S7. Immerse the porous aerogel framework structure membrane in the above mixed slurry, keep it warm in a vacuum drying oven at 70° C. for 5-10 hours, then take it out from the slurry and dry it to obtain a BFAN-based ceramic particle-PVDF polymer filled porous aerogel.
[0015] Preferably, the concentration of the cellulose nanofiber solution in step S2 is 4%-8%, and the volume ratio of the first solution to the cellulose nanofiber solution is 1:1.
[0016] Preferably, the coating method in step S3 is spin coating at a rotation speed of 600 rpm, and the coating thickness is 200-300 μm, and the drying method is drying in a vacuum drying oven at 75-85° C. for 10-16 hours.
[0017] Preferably, the concentration of sodium persulfate in step S3 is 1 mol / L, and the soaking treatment time is 3-24 hours.
[0018] Preferably, the method for preparing BFAN-based nano-ceramic particles in step S4 comprises the following steps:
[0019] S4-1. Weigh bismuth nitrate, iron nitrate, niobium ethoxide, and silver nitrate according to the stoichiometric ratio of the molecular formula 0.9BiFeO3-0.1AgNbO3;
[0020] S4-2, dissolve ferric nitrate and niobium ethoxide in ethylene glycol methyl ether, dissolve bismuth nitrate and silver nitrate in acetic acid to prepare two solutions, stir the two solutions at 50-80°C for 10-20 minutes and then mix them, add stabilizer acetylacetone, and continue stirring at 50-80°C until a yellow-brown transparent solution is obtained, and adjust the pH value to 4-6 with ammonia water to obtain a mixed solution for use;
[0021] S4-3. The mixed solution is placed in a vacuum drying oven and dried at 100-110°C to obtain a gel. The gel is transferred to a tubular furnace and heated to 400°C at 3°C / min and kept warm for 20 minutes. The temperature is then raised to 500-600°C and calcined for 2-3 hours. After cooling, the mixture is ground for 15-20 minutes to obtain BFAN-based ceramic particles.
[0022] Preferably, the concentration of the mixed solution in step S4-2 is 0.2M, and the volume ratio of each solvent is acetic acid:ethylene glycol methyl ether:acetylacetone solution=15-20:15-20:1.
[0023] BFAN-based ceramic particles-PVDF polymer filled porous aerogel is used in the preparation of piezoelectric sensors; the application method comprises the following steps:
[0024] (1) Using BFAN-based ceramic particles-PVDF polymer filled porous aerogel as a piezoelectric thick film, pasting ITO / PET transparent conductive films on the upper and lower surfaces of the piezoelectric thick film, and then using copper wire as the lead electrode, and then hot pressing to compact and flatten, to obtain a piezoelectric composite film;
[0025] (2) The piezoelectric composite film is polarized at an electric field of 10-20 kV / mm and a temperature of 50° C. for 10-30 min, and then connected to an external circuit to prepare a piezoelectric sensor.
[0026] Preferably, in the step (1), when the ITO / PET transparent conductive film is attached to the piezoelectric thick film, the conductive side is in contact with the piezoelectric thick film.
[0027] Preferably, in step (1), the hot pressing pressure of the hot pressing machine is 10 MPa, the temperature is 60° C., and the hot pressing time is 30 min.
[0028] The present invention provides a preparation method and application of a BFAN-based ceramic particle-PVDF polymer filled porous aerogel, which has the following advantages over the prior art:
[0029] The PVA-CNF porous aerogel frame prepared by the present invention has excellent mechanical properties and recoverability, and prolongs the service life of the sensor; the BFAN-based lead-free ceramic particles prepared by the sol-gel method can reduce the conductivity, and obtain excellent lead-free piezoelectric ceramic particles, which are environmentally friendly; the BFAN-based ceramic particles are mixed with PVDF polymers for ball milling, and the high-energy ball milling produces a "drag effect", which helps the α crystal phase in the PVDF polymer to transform into the β crystal phase with higher piezoelectric performance, and the obtained slurry has strong piezoelectric properties; the aerogel frame is filled with it, and the obtained composite film has the advantages of high ductility and good recoverability. The piezoelectric sensor of the BFAN-based-PVDF polymer filled porous aerogel has a larger output performance than the existing flexible piezoelectric power generation materials and has a sensing function, and has great potential in the field of medical care. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 (a) is a surface SEM photo of the porous aerogel frame of Example 4; (b) is a surface SEM photo of the composite membrane after filling in Example 4; (c) is a schematic diagram of the piezoelectric sensor structure of the BFAN-based-PVDF polymer filled porous aerogel; (d) is an external rectifier circuit of the piezoelectric composite membrane;
[0031] Figure 2 This is a schematic flow chart of the method for preparing a piezoelectric sensor of the present invention using a porous aerogel filled with a BFAN-based PVDF polymer;
[0032] Figure 3 The output voltage performance comparison of each embodiment of the piezoelectric sensor of the BFAN-based-PVDF polymer filled porous aerogel of each embodiment of the present invention;
[0033] Figure 4 The piezoelectric sensor of the BFAN-based-PVDF polymer filled porous aerogel of Example 4 of the present invention is used for human health monitoring, and the output signal comparison between walking, falling, running and jumping actions is obtained;
[0034] Figure 5 This is an output power-load relationship diagram of the piezoelectric sensor of the BFAN-based-PVDF polymer filled porous aerogel of Example 4 of the present invention under the application of fixed frequency and pressure.
[0035] Figure 6 This is a durability test diagram of the piezoelectric sensor of the BFAN-based PVDF polymer filled porous aerogel of Example 4 of the present invention. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Embodiment 1:
[0038] The preparation of a conventional porous aerogel piezoelectric sensor (without filling the aerogel microcavities with a mixed slurry) includes the following steps:
[0039] 1. Preparation of porous aerogel framework:
[0040] 1.1. Dissolve 7.5 g of polyvinyl alcohol powder in 50 ml of deionized water to prepare a PVA solution, and dissolve 0.75 g of borax in the PVA solution to prepare a first mixed solution;
[0041] 1.2. 50 ml of 6% cellulose nanofiber solution was mixed with the first mixed solution and stirred at 80° C. for 3 min to obtain a colloidal slurry;
[0042] 1.3. Spin the colloidal slurry onto a glass substrate at a spin coating speed of 600 rpm, control the film thickness to be 200 μm, and then dry it in a vacuum drying oven at 80° C. for 12 h to obtain a gel film;
[0043] 1.4. Freeze the above gel film in a freeze dryer at -80°C for 12 hours; then transfer it to a 1 mol / L sodium persulfate solution and soak it for salting out for 24 hours, then rinse it with deionized water for 3 times, and freeze it again at -80°C for 12 hours to obtain a porous aerogel thick film;
[0044] 2. Covering electrodes and hot pressing treatment:
[0045] ITO / PET transparent conductive films were attached to the upper and lower surfaces of the porous aerogel thick film, and the conductive side of the ITO / PET transparent conductive film was in contact with the porous aerogel thick film. Finally, it was cut into a 4cm×5cm rectangle and copper wire was used as the lead-out electrode. Then, a hot press was used at a pressure of 10MPa and a temperature of 60℃ for 30min and then taken out to obtain a piezoelectric composite film.
[0046] 3. Polarization treatment and connection to external circuit:
[0047] The piezoelectric composite film was polarized for 20 minutes under the conditions of a polarization electric field of 15 kV / mm and a temperature of 50°C to obtain a pressure sensor, which was then connected to an external circuit and the output of the sensor was achieved after rectification.
[0048] Embodiment 2:
[0049] The preparation of a piezoelectric sensor of a BFAN-based PVDF polymer filled porous aerogel comprises the following steps:
[0050] 1. Preparation of porous aerogel framework:
[0051] 1.1. Dissolve 7.5 g of polyvinyl alcohol powder in 50 ml of deionized water to prepare a PVA solution, and dissolve 0.75 g of borax in the PVA solution to prepare a first mixed solution;
[0052] 1.2. 50 ml of 6% cellulose nanofiber solution was mixed with the first mixed solution and stirred at 80° C. for 3 min to obtain a colloidal slurry;
[0053] 1.3. Spin the colloidal slurry onto a glass substrate at a spin coating speed of 600 rpm, control the film thickness to be 200 μm, and then dry it in a vacuum drying oven at 80° C. for 12 h to obtain a gel film;
[0054] 1.4. Freeze the above gel film in a freeze dryer at -80°C for 12 hours; then transfer it to a 1 mol / L sodium persulfate solution and soak it for salting out for 24 hours, then rinse it with deionized water for 3 times, and freeze it again at -80°C for 12 hours to obtain a porous aerogel thick film;
[0055] 2. Preparation of BFAN-based nano-ceramic particles:
[0056] 2.1. Weigh bismuth nitrate, iron nitrate, niobium ethoxide, and silver nitrate in the stoichiometric ratio of the molecular formula 0.9BiFeO3–0.1AgNbO3 (BFAN):
[0057] 2.2. Dissolve ferric nitrate and niobium ethoxide in ethylene glycol methyl ether, and dissolve bismuth nitrate and silver nitrate in acetic acid. Stir the two solutions at 80°C for 20 minutes and then mix them. Add stabilizer acetylacetone and continue stirring at 80°C until it becomes a yellow-brown transparent solution. At the same time, adjust the pH value to 6 with ammonia water (the concentration after preparation is controlled to be 0.2M, and the volume ratio of acetic acid, ethylene glycol methyl ether and acetylacetone solution is 15:15:1). Then put the solution into a vacuum drying oven and dry it at 100°C to obtain a gel.
[0058] 2.3. The dried gel was transferred to a tube furnace and heated to 400°C at a rate of 3°C / min and kept at that temperature for 20 min to remove residual impurities. The temperature was then raised to 600°C and calcined for 3 h. After cooling, the ceramic particles were ground for 20 min to obtain BFAN-based ceramic particles.
[0059] 3. Preparation of BFAN-based-PVDF polymer mixed slurry:
[0060] 3.1. Dissolve 5 g of polyvinylidene fluoride powder in 100 ml of N,N-dimethylformamide solvent and stir at 60°C for 16 minutes to obtain a transparent solution.
[0061] 3.2. Add BFAN-based ceramic particles to the transparent solution to obtain a PVDF-BFAN-0 solution, in which the BFAN-based ceramic particles account for 0wt% of the PVDF mass. Put the PVDF-BFAN-0 solution into an agate ball mill for high-energy ball milling at a ball milling speed of 600 rpm. Take out after 30 minutes to obtain a mixed slurry with high piezoelectricity;
[0062] 4. Preparation of piezoelectric thick film by filling porous aerogel framework with BFAN-based PVDF polymer:
[0063] The porous aerogel thick film was immersed in the mixed slurry prepared in step 3, kept warm in a vacuum drying oven at 70°C for 8 hours, and then the composite piezoelectric thick film was taken out from the slurry and continued to dry for 30 minutes to obtain a BFAN-based ceramic particle-PVDF polymer filled porous aerogel film.
[0064] 5. Covering electrode and hot pressing treatment:
[0065] ITO / PET transparent conductive films were attached to the upper and lower surfaces of the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane, and the conductive side of the ITO / PET transparent conductive film was in contact with the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane. Finally, it was cut into a 4cm×5cm rectangle and copper wire was used as the lead-out electrode. Then, a hot press was used at a pressure of 10MPa and a temperature of 60°C for 30 minutes, and then it was taken out to obtain a piezoelectric composite membrane.
[0066] 6. Polarization treatment and connection to external circuit:
[0067] The piezoelectric composite film was polarized for 20 minutes under the conditions of a polarization electric field of 15 kV / mm and a temperature of 50°C to obtain a pressure sensor, which was then connected to an external circuit and the output of the sensor was achieved after rectification.
[0068] Embodiment 3:
[0069] The preparation of a piezoelectric sensor of a BFAN-based PVDF polymer filled porous aerogel comprises the following steps:
[0070] 1. Preparation of porous aerogel framework:
[0071] 1.1. Dissolve 7.5 g of polyvinyl alcohol powder in 50 ml of deionized water to prepare a PVA solution, and dissolve 0.75 g of borax in the PVA solution to prepare a first mixed solution;
[0072] 1.2. 50 ml of 6% cellulose nanofiber solution was mixed with the first mixed solution and stirred at 80° C. for 3 min to obtain a colloidal slurry;
[0073] 1.3. Spin the colloidal slurry onto a glass substrate at a spin coating speed of 600 rpm, control the film thickness to be 200 μm, and then dry it in a vacuum drying oven at 80° C. for 12 h to obtain a gel film;
[0074] 1.4. Freeze the above gel film in a freeze dryer at -80°C for 12 hours; then transfer it to a 1 mol / L sodium persulfate solution and soak it for salting out for 24 hours, then rinse it with deionized water for 3 times, and freeze it again at -80°C for 12 hours to obtain a porous aerogel thick film;
[0075] 2. Preparation of BFAN-based nano-ceramic particles:
[0076] 2.1. Weigh bismuth nitrate, iron nitrate, niobium ethoxide, and silver nitrate in the stoichiometric ratio of the molecular formula 0.9BiFeO3–0.1AgNbO3 (BFAN):
[0077] 2.2. Dissolve ferric nitrate and niobium ethoxide in ethylene glycol methyl ether, and dissolve bismuth nitrate and silver nitrate in acetic acid. Stir the two solutions at 80°C for 20 minutes and then mix them. Add stabilizer acetylacetone and continue stirring at 80°C until it becomes a yellow-brown transparent solution. At the same time, adjust the pH value to 6 with ammonia water (the concentration after preparation is controlled to be 0.2M, and the volume ratio of acetic acid, ethylene glycol methyl ether and acetylacetone solution is 15:15:1). Then put the solution into a vacuum drying oven and dry it at 100°C to obtain a gel.
[0078] 2.3. The dried gel was transferred to a tube furnace and heated to 400°C at a rate of 3°C / min and kept at that temperature for 20 min to remove residual impurities. The temperature was then raised to 600°C and calcined for 3 h. After cooling, the ceramic particles were ground for 20 min to obtain BFAN-based ceramic particles.
[0079] 3. Preparation of BFAN-based-PVDF polymer mixed slurry:
[0080] 3.1. Dissolve 5 g of polyvinylidene fluoride powder in 100 ml of N,N-dimethylformamide solvent and stir at 60°C for 16 minutes to obtain a transparent solution.
[0081] 3.2. Add BFAN-based ceramic particles to the transparent solution to obtain a PVDF-BFAN-20 solution, in which the BFAN-based ceramic particles account for 20wt% of the PVDF mass. Put the PVDF-BFAN-20 solution into an agate ball mill for high-energy ball milling at a ball milling speed of 600rpm. Take out the mixed slurry with high piezoelectricity after 30 minutes.
[0082] 4. Preparation of piezoelectric thick film by filling porous aerogel framework with BFAN-based PVDF polymer:
[0083] The porous aerogel thick film was immersed in the mixed slurry prepared in step 3, kept warm in a vacuum drying oven at 70°C for 8 hours, and then the composite piezoelectric thick film was taken out from the slurry and continued to dry for 30 minutes to obtain a BFAN-based ceramic particle-PVDF polymer filled porous aerogel film.
[0084] 5. Covering electrode and hot pressing treatment:
[0085] ITO / PET transparent conductive films were attached to the upper and lower surfaces of the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane, and the conductive side of the ITO / PET transparent conductive film was in contact with the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane. Finally, it was cut into a 4cm×5cm rectangle and copper wire was used as the lead-out electrode. Then, a hot press was used at a pressure of 10MPa and a temperature of 60°C for 30 minutes, and then it was taken out to obtain a piezoelectric composite membrane.
[0086] 6. Polarization treatment and connection to external circuit:
[0087] The piezoelectric composite film was polarized for 20 minutes under the conditions of a polarization electric field of 15 kV / mm and a temperature of 50°C to obtain a pressure sensor, which was then connected to an external circuit and the output of the sensor was achieved after rectification.
[0088] Embodiment 4:
[0089] The preparation of a piezoelectric sensor of a BFAN-based PVDF polymer filled porous aerogel comprises the following steps:
[0090] 1. Preparation of porous aerogel framework:
[0091] 1.1. Dissolve 7.5 g of polyvinyl alcohol powder in 50 ml of deionized water to prepare a PVA solution, and dissolve 0.75 g of borax in the PVA solution to prepare a first mixed solution;
[0092] 1.2. 50 ml of 6% cellulose nanofiber solution was mixed with the first mixed solution and stirred at 80° C. for 3 min to obtain a colloidal slurry;
[0093] 1.3. Spin the colloidal slurry onto a glass substrate at a spin coating speed of 600 rpm, control the film thickness to be 200 μm, and then dry it in a vacuum drying oven at 80° C. for 12 h to obtain a gel film;
[0094] 1.4. Freeze the above gel film in a freeze dryer at -80°C for 12 hours; then transfer it to a 1 mol / L sodium persulfate solution and soak it for salting out for 24 hours, then rinse it with deionized water for 3 times, and freeze it again at -80°C for 12 hours to obtain a porous aerogel thick film;
[0095] 2. Preparation of BFAN-based nano-ceramic particles:
[0096] 2.1. Weigh bismuth nitrate, iron nitrate, niobium ethoxide, and silver nitrate in the stoichiometric ratio of the molecular formula 0.9BiFeO3–0.1AgNbO3 (BFAN):
[0097] 2.2. Dissolve ferric nitrate and niobium ethoxide in ethylene glycol methyl ether, and dissolve bismuth nitrate and silver nitrate in acetic acid. Stir the two solutions at 80°C for 20 minutes and then mix them. Add stabilizer acetylacetone and continue stirring at 80°C until it becomes a yellow-brown transparent solution. At the same time, adjust the pH value to 6 with ammonia water (the concentration after preparation is controlled to be 0.2M, and the volume ratio of acetic acid, ethylene glycol methyl ether and acetylacetone solution is 15:15:1). Then put the solution into a vacuum drying oven and dry it at 100°C to obtain a gel.
[0098] 2.3. The dried gel was transferred to a tube furnace and heated to 400°C at a rate of 3°C / min and kept at that temperature for 20 min to remove residual impurities. The temperature was then raised to 600°C and calcined for 3 h. After cooling, the ceramic particles were ground for 20 min to obtain BFAN-based ceramic particles.
[0099] 3. Preparation of BFAN-based-PVDF polymer mixed slurry:
[0100] 3.1. Dissolve 5 g of polyvinylidene fluoride powder in 100 ml of N,N-dimethylformamide solvent and stir at 60°C for 16 minutes to obtain a transparent solution.
[0101] 3.2. Add BFAN-based ceramic particles to the transparent solution to obtain a PVDF-BFAN-40 solution, in which the BFAN-based ceramic particles account for 40wt% of the PVDF mass. Put the PVDF-BFAN-40 solution into an agate ball mill for high-energy ball milling at a ball milling speed of 600rpm. Take out the mixed slurry with high piezoelectricity after 30 minutes.
[0102] 4. Preparation of piezoelectric thick film by filling porous aerogel framework with BFAN-based PVDF polymer:
[0103] The porous aerogel thick film was immersed in the mixed slurry prepared in step 3, kept warm in a vacuum drying oven at 70°C for 8 hours, and then the composite piezoelectric thick film was taken out from the slurry and continued to dry for 30 minutes to obtain a BFAN-based ceramic particle-PVDF polymer filled porous aerogel film.
[0104] 5. Covering electrode and hot pressing treatment:
[0105] ITO / PET transparent conductive films were attached to the upper and lower surfaces of the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane, and the conductive side of the ITO / PET transparent conductive film was in contact with the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane. Finally, it was cut into a 4cm×5cm rectangle and copper wire was used as the lead-out electrode. Then, a hot press was used at a pressure of 10MPa and a temperature of 60°C for 30 minutes, and then it was taken out to obtain a piezoelectric composite membrane.
[0106] 6. Polarization treatment and connection to external circuit:
[0107] The piezoelectric composite film was polarized for 20 minutes under the conditions of a polarization electric field of 15 kV / mm and a temperature of 50°C to obtain a pressure sensor, which was then connected to an external circuit and the output of the sensor was achieved after rectification.
[0108] Embodiment 5:
[0109] The preparation of a piezoelectric sensor of a BFAN-based PVDF polymer filled porous aerogel comprises the following steps:
[0110] 1. Preparation of porous aerogel framework:
[0111] 1.1. Dissolve 7.5 g of polyvinyl alcohol powder in 50 ml of deionized water to prepare a PVA solution, and dissolve 0.75 g of borax in the PVA solution to prepare a first mixed solution;
[0112] 1.2. 50 ml of 6% cellulose nanofiber solution was mixed with the first mixed solution and stirred at 80° C. for 3 min to obtain a colloidal slurry;
[0113] 1.3. Spin the colloidal slurry onto a glass substrate at a spin coating speed of 600 rpm, control the film thickness to be 200 μm, and then dry it in a vacuum drying oven at 80° C. for 12 h to obtain a gel film;
[0114] 1.4. Freeze the above gel film in a freeze dryer at -80°C for 12 hours; then transfer it to a 1 mol / L sodium persulfate solution and soak it for salting out for 24 hours, then rinse it with deionized water for 3 times, and freeze it again at -80°C for 12 hours to obtain a porous aerogel thick film;
[0115] 2. Preparation of BFAN-based nano-ceramic particles:
[0116] 2.1. Weigh bismuth nitrate, iron nitrate, niobium ethoxide, and silver nitrate in the stoichiometric ratio of the molecular formula 0.9BiFeO3–0.1AgNbO3 (BFAN):
[0117] 2.2. Dissolve ferric nitrate and niobium ethoxide in ethylene glycol methyl ether, and dissolve bismuth nitrate and silver nitrate in acetic acid. Stir the two solutions at 80°C for 20 minutes and then mix them. Add stabilizer acetylacetone and continue stirring at 80°C until it becomes a yellow-brown transparent solution. At the same time, adjust the pH value to 6 with ammonia water (the concentration after preparation is controlled to be 0.2M, and the volume ratio of acetic acid, ethylene glycol methyl ether and acetylacetone solution is 15:15:1). Then put the solution into a vacuum drying oven and dry it at 100°C to obtain a gel.
[0118] 2.3. The dried gel was transferred to a tube furnace and heated to 400°C at a rate of 3°C / min and kept at that temperature for 20 min to remove residual impurities. The temperature was then raised to 600°C and calcined for 3 h. After cooling, the ceramic particles were ground for 20 min to obtain BFAN-based ceramic particles.
[0119] 3. Preparation of BFAN-based-PVDF polymer mixed slurry:
[0120] 3.1. Dissolve 5 g of polyvinylidene fluoride powder in 100 ml of N,N-dimethylformamide solvent and stir at 60°C for 16 minutes to obtain a transparent solution.
[0121] 3.2. Add BFAN-based ceramic particles to the transparent solution to obtain a PVDF-BFAN-60 solution, in which the BFAN-based ceramic particles account for 60wt% of the PVDF mass. Put the PVDF-BFAN-60 solution into an agate ball mill for high-energy ball milling at a ball milling speed of 600rpm. Take out the mixed slurry with high piezoelectricity after 30 minutes.
[0122] 4. Preparation of piezoelectric thick film by filling porous aerogel framework with BFAN-based PVDF polymer:
[0123] The porous aerogel thick film was immersed in the mixed slurry prepared in step 3, kept warm in a vacuum drying oven at 70°C for 8 hours, and then the composite piezoelectric thick film was taken out from the slurry and continued to dry for 30 minutes to obtain a BFAN-based ceramic particle-PVDF polymer filled porous aerogel film.
[0124] 5. Covering electrode and hot pressing treatment:
[0125] ITO / PET transparent conductive films were attached to the upper and lower surfaces of the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane, and the conductive side of the ITO / PET transparent conductive film was in contact with the BFAN-based ceramic particle-PVDF polymer filled porous aerogel membrane. Finally, it was cut into a 4cm×5cm rectangle and copper wire was used as the lead-out electrode. Then, a hot press was used at a pressure of 10MPa and a temperature of 60°C for 30 minutes, and then it was taken out to obtain a piezoelectric composite membrane.
[0126] 6. Polarization treatment and connection to external circuit:
[0127] The piezoelectric composite film was polarized for 20 minutes under the conditions of a polarization electric field of 15 kV / mm and a temperature of 50°C to obtain a pressure sensor, which was then connected to an external circuit and the output of the sensor was achieved after rectification.
[0128] Detection:
[0129] The electrical performance tests of the piezoelectric sensors of Examples 1-5 were performed:
[0130] Figure 3 The output voltage performance comparison of the piezoelectric sensor of the BFAN-based-PVDF polymer filled porous aerogel according to various embodiments of the present invention is shown.
[0131] Apply a periodic pressure with a frequency of 1 Hz and a pressure of 50 kPa:
[0132] In Example 1, the piezoelectric sensor prepared by using only the aerogel frame structure without filling the piezoelectric mixed slurry has low output performance and the voltage peak reaches 15V;
[0133] Example 2: The piezoelectric sensor prepared by filling the aerogel frame structure with PVDF-BFAN-0 solution has improved output performance and the voltage peak reaches 20V;
[0134] The piezoelectric sensor of Example 4 has the best output capability, that is, when the BFAN-based ceramic accounts for 40 wt % of the PVDF, the maximum output voltage is 62 V.
[0135] Figure 4 A piezoelectric sensor of a BFAN-based PVDF polymer filled porous aerogel according to Example 4 of the present invention is used for output signal comparison between walking, falling, running and jumping actions in human health monitoring.
[0136] The output voltage is about 30V when walking, and it decreases to 15V when falling. The frequency increases and the pressure increases when running, and the output voltage is about 60V. The pressure is greater when jumping, and the output voltage is about 80V.
[0137] Figure 5This is a graph showing the output power-load relationship of a piezoelectric sensor of a BFAN-based PVDF polymer-filled porous aerogel under a fixed frequency and pressure applied in Example 4 of the present invention. The frequency of the applied pressure is 1 Hz and the pressure is 50 kPa. When the load resistance is 10 MΩ, the maximum output power density is about 0.54 W / m 2 .
[0138] Figure 6 This is a durability test diagram of a piezoelectric sensor of a BFAN-based PVDF polymer filled porous aerogel in Example 4 of the present invention: a curve of the relationship between the number of times and the output voltage. A periodic pressure of 1 Hz and 50 kPa was applied. After 10 6 After a pressure cycle, the output voltage remains basically unchanged, and the variation range is kept within ±2%, indicating that the piezoelectric sensor has good recoverability and long service life.
[0139] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a BFAN-based ceramic particle-PVDF polymer filled porous aerogel, characterized in that: The preparation method comprises the following steps: S1, preparing a first solution by mixing polyvinyl alcohol, deionized water and borax in a mass ratio of 15:100:1.5 for standby use; S2, mixing the first solution with the cellulose nanofiber solution, stirring and reacting at 75-85° C. for 2-5 minutes to obtain a colloidal slurry; S3, coating the colloidal slurry and drying it to obtain a gel film, freeze-drying the gel film at -80°C for 10-14h, and then soaking and salting out with sodium persulfate to obtain a porous aerogel framework structure membrane; S4, preparing 0.9BiFeO3-0.1AgNbO3 BFAN-based nano-ceramic particles by sol-gel method; S5, mixing polyvinylidene fluoride powder and N,N-dimethylformamide solvent at a ratio of 0.5 g:10 ml, and stirring at 50-60° C. for 16 minutes to obtain a transparent solution; S6, adding 20wt%-60wt% of BFAN-based ceramic particles to the above transparent solution to prepare a PVDF-BFAN mixed solution, placing the mixed solvent in an agate ball milling jar and performing high-energy ball milling at a speed of 200-750rpm for 30min to obtain a mixed slurry; S7. Immerse the porous aerogel framework structure membrane in the above mixed slurry, keep it warm in a vacuum drying oven at 70° C. for 5-10 hours, then take it out from the slurry and dry it to obtain a BFAN-based ceramic particle-PVDF polymer filled porous aerogel.
2. The preparation method according to claim 1, characterized in that: In step S2, the concentration of the cellulose nanofiber solution is 4%-8%, and the volume ratio of the first solution and the cellulose nanofiber solution is 1:
1.
3. The preparation method according to claim 1, characterized in that: The coating method in step S3 is spin coating at a rotation speed of 600 rpm, and the coating thickness is 200-300 μm, and the drying method is drying in a vacuum drying oven at 75-85° C. for 10-16 hours.
4. The preparation method according to claim 1, characterized in that: In step S3, the concentration of sodium persulfate is 1 mol / L, and the soaking time is 3-24 hours.
5. The preparation method according to claim 1, characterized in that: The method for preparing BFAN-based nano-ceramic particles in step S4 comprises the following steps: S4-1. Weigh bismuth nitrate, iron nitrate, niobium ethoxide, and silver nitrate according to the stoichiometric ratio of the molecular formula 0.9BiFeO3-0.1AgNbO3; S4-2, dissolve ferric nitrate and niobium ethoxide in ethylene glycol methyl ether, dissolve bismuth nitrate and silver nitrate in acetic acid to prepare two solutions, stir the two solutions at 50-80°C for 10-20 minutes and then mix them, add stabilizer acetylacetone, and continue stirring at 50-80°C until a yellow-brown transparent solution is obtained, and adjust the pH value to 4-6 with ammonia water to obtain a mixed solution for use; S4-3. The mixed solution is placed in a vacuum drying oven and dried at 100-110°C to obtain a gel. The gel is transferred to a tubular furnace and heated to 400°C at 3°C / min and kept warm for 20 minutes. The temperature is then raised to 500-600°C and calcined for 2-3 hours. After cooling, the mixture is ground for 15-20 minutes to obtain BFAN-based ceramic particles.
6. The preparation method according to claim 5, characterized in that: The concentration of the mixed solution in step S4-2 is 0.2M, and the volume ratio of each solvent is acetic acid:ethylene glycol methyl ether:acetylacetone solution=15-20:15-20:
1.
7. Use of the BFAN-based ceramic particle-PVDF polymer filled porous aerogel obtained by the preparation method according to any one of claims 1 to 6 in a piezoelectric sensor.
8. The use according to claim 7, characterized in that: The application method comprises the following steps: (1) Using BFAN-based ceramic particles-PVDF polymer filled porous aerogel as a piezoelectric thick film, pasting ITO / PET transparent conductive films on the upper and lower surfaces of the piezoelectric thick film, and then using copper wire as the lead electrode, and then hot pressing to compact and flatten, to obtain a piezoelectric composite film; (2) The piezoelectric composite film is polarized at an electric field of 10-20 kV / mm and a temperature of 50° C. for 10-30 min, and then connected to an external circuit to prepare a piezoelectric sensor.
9. The use according to claim 8, characterized in that: In the step (1), when the ITO / PET transparent conductive film is attached to the piezoelectric thick film, the conductive side is in contact with the piezoelectric thick film.
10. The use according to claim 8, characterized in that: In step (1), the hot pressing pressure of the hot pressing machine is 10 MPa, the temperature is 60° C., and the hot pressing time is 30 min.