A kind of EVA photovoltaic encapsulation film and its preparation method and application

By introducing one-dimensional organic polymer nanomaterials and two-dimensional layered nanomaterials of specific biomass into the EVA photovoltaic packaging film, the EVA packaging film is solved by combining with silane coupling agent to form anti-PID masterbatches, and the EVA packaging film is solved at high temperature and high humidity. The aging problem in the environment improves its thermal stability and PID resistance, and extends the service life of photovoltaic modules.

CN118562412BActive Publication Date: 2024-11-26JIANGSU ZHONGLAI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027361.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-26
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

EVA photovoltaic packaging film is prone to aging and decomposition in high temperature and high humidity environments, resulting in degradation of battery performance, contact adhesion loss and PID effect, affecting the long-term performance of photovoltaic modules.

Method used

Introduce one-dimensional organic polymer nanomaterials and two-dimensional layered nanomaterials with specific biomass, combined with silane coupling agents, to form anti-PID masterbatches, improve the thermal stability, barrier properties and anti-PID performance of EVA packaging films, through Hydrogen bonds reduce the polarity of EVA molecular chains, improve mechanical strength and humidity and heat resistance.

Benefits of technology

It improves the aging resistance, mechanical strength and PID resistance of the EVA packaging film, extends the service life of photovoltaic modules, reduces the PID attenuation phenomenon, and enhances the photoelectric conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of photovoltaic encapsulation films, and specifically discloses an EVA photovoltaic encapsulation film and its preparation method and application. The EVA photovoltaic encapsulation film comprises: a specific weight portion of ethylene-vinyl acetate copolymer, an anti-PID masterbatch, a main cross-linking agent, an auxiliary cross-linking agent and an antioxidant; the anti-PID masterbatch comprises: a specific weight portion of ethylene-vinyl acetate copolymer, a one-dimensional organic polymer nanomaterial, a two-dimensional layered nanomaterial and a silane coupling agent; the one-dimensional organic polymer nanomaterial is at least one of cellulose nanofibrils, cellulose nanocrystals and bacterial cellulose with multiple hydroxyls; the two-dimensional layered nanomaterial is organic sodium montmorillonite. The EVA photovoltaic encapsulation film of the present invention can improve its aging resistance and mechanical strength when applied at the end of a photovoltaic module, reduce the PID attenuation phenomenon, and has a low water vapor permeability, which helps to extend the service life of the battery cell and improve the photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic encapsulation adhesive films, and in particular to an EVA photovoltaic encapsulation adhesive film and a preparation method and application thereof. Background Art

[0002] Photovoltaic encapsulation film provides a barrier structure for photovoltaic modules to limit the penetration of oxygen and moisture. While playing an important role in bonding the cell to the photovoltaic front panel (such as photovoltaic glass), and the cell to the photovoltaic back panel, it also has multiple functions such as providing mechanical buffering, protection, and anti-PID performance for photovoltaic modules (PID refers to induced potential difference attenuation. In practice, the anti-PID performance of POE encapsulation film is better than that of EVA encapsulation film) and providing anti-ultraviolet protection for the photovoltaic back panel. Therefore, photovoltaic encapsulation film plays an important role in extending the service life of photovoltaic modules.

[0003] As shown in publication number CN117417712A, as mainstream photovoltaic encapsulation films, single-layer EVA (ethylene-vinyl acetate copolymer) encapsulation films or three-layer co-extruded EPE encapsulation films are widely used in mainstream photovoltaic cells in the market (such as PERC cells, TOPCon cells and HJT cells) and photovoltaic modules corresponding to these photovoltaic cells; this is because EVA encapsulation films have many advantages such as low cost, good light transmittance, high elasticity, low processing temperature, good melt fluidity and high adhesion.

[0004] However, the stability of EVA encapsulation film is greatly affected by the environment. Light, heat and humidity can cause it to age, which can lead to adverse effects such as loss of battery performance and contact adhesion, increase in contact resistance and formation of visible dark areas in electroluminescence (EL) imaging. Especially in high temperature and high humidity environments, EVA encapsulation film is prone to aging and decomposition to produce acetic acid, which in turn accelerates the oxidation rate of aluminum in the silver aluminum paste of the TOPCon battery, resulting in electron loss and affecting the photoelectric conversion efficiency of the photovoltaic module (specifically manifested in the photovoltaic module: after the wet heat test, the photovoltaic module will show obvious power attenuation); moreover, the acetate ions produced will also cause Na+ migration in the glass layer of the photovoltaic module (such as photovoltaic glass), thereby inducing the PID-s effect, further causing PID power attenuation in the photovoltaic module, affecting its long-term anti-PID performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide an EVA photovoltaic encapsulation film and a preparation method and application thereof.

[0006] Based on this, the present invention discloses an EVA photovoltaic encapsulation film, which includes the following raw materials in parts by weight:

[0007] 85-100 parts of ethylene-vinyl acetate copolymer, 1-15 parts of anti-PID masterbatch, 0.5-1 parts of main cross-linking agent, 0.1-0.8 parts of auxiliary cross-linking agent and 0.1-1 parts of antioxidant;

[0008] Wherein, the anti-PID masterbatch comprises the following raw materials in parts by weight:

[0009] 60-100 parts of ethylene-vinyl acetate copolymer, 1-20 parts of one-dimensional organic polymer nanomaterial, 1-10 parts of two-dimensional layered nanomaterial and 2-10 parts of silane coupling agent;

[0010] The one-dimensional organic polymer nanomaterial is at least one of cellulose nanofibrils (CNF), cellulose nanocrystals (CNC), and bacterial cellulose (BC) having multiple hydroxyl groups;

[0011] The two-dimensional layered nanomaterial is organic sodium montmorillonite (MMT).

[0012] Preferably, the aspect ratio of the cellulose nanofibrils is 20:1-40:1; the crystallinity of the cellulose nanocrystals is 75-85%; and the crystallinity of the bacterial cellulose is 80-85%.

[0013] Further preferably, the one-dimensional organic polymer nanomaterial is bacterial cellulose with a crystallinity of 80-85%.

[0014] Conventional EVA packaging films are prone to yellowing, deterioration, blistering and degumming under direct sunlight. After introducing a one-dimensional organic polymer nanomaterial of a specific biomass (such as cellulose nanofibrils with an aspect ratio of 20:1-40:1, cellulose nanocrystals with a crystallinity of 75-85%, and bacterial cellulose with a crystallinity of 80-85%) into the anti-PID masterbatch of the EVA packaging film of the present invention, the solvent resistance, weather resistance, high tensile modulus and good compatibility of the one-dimensional organic polymer nanomaterial of the specific biomass can be utilized to improve the above-mentioned phenomena of conventional EVA packaging films. At the same time, CNF can greatly reduce the harm caused by the above-mentioned phenomena of conventional EVA packaging films by absorbing ultraviolet rays.

[0015] Preferably, the organic sodium montmorillonite has an ion exchange capacity of 120-145, an aspect ratio of 300:500-150:200, and a pH of 9.0-10.5.

[0016] Further preferably, the organic sodium montmorillonite has an ion exchange capacity of 145 and an aspect ratio of 300:500-200:300.

[0017] Conventional EVA packaging films have poor barrier properties to water vapor and gas, and poor thermal stability, and these defects greatly reduce the service life of conventional EVA packaging films under outdoor or hot and humid conditions. However, after the anti-PID masterbatch of the EVA packaging film of the present invention is introduced with MMT, the thermal stability of the EVA packaging film is improved, and the barrier effect of the EVA packaging film to water vapor and oxygen is also improved, thereby broadening the application market of the EVA packaging film.

[0018] Further preferably, in the EVA photovoltaic encapsulation film, the weight ratio of ethylene-vinyl acetate copolymer: anti-PID masterbatch: main cross-linking agent: auxiliary cross-linking agent: antioxidant is 100:6-10:0.8:0.6:0.5;

[0019] In the anti-PID masterbatch, the weight ratio of ethylene-vinyl acetate copolymer: one-dimensional organic polymer nanomaterial: two-dimensional layered nanomaterial: silane coupling agent is 100:8-12:4-6:5.

[0020] Further preferably, the main cross-linking agent is one or more of tert-butyl peroxide-2-ethylhexyl carbonate, dibenzoyl peroxide, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, and 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane;

[0021] The auxiliary cross-linking agent is one or more of triallyl isocyanurate, diethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, triallyl cyanurate, and ethoxylated trimethylolpropane triacrylate;

[0022] The antioxidant is one or more of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris(2,4-di-tert-butylphenyl) phosphite, and bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate;

[0023] The silane coupling agent is one or more of γ-glycidyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane or γ-(methacryloyloxy)propyltrimethoxysilane.

[0024] The present invention also discloses a method for preparing an EVA photovoltaic encapsulation film, comprising the following preparation steps:

[0025] S1. Pre-treating the one-dimensional organic polymer nanomaterial and the two-dimensional layered nanomaterial respectively to obtain the one-dimensional organic polymer nanomaterial powder and the two-dimensional layered nanomaterial powder respectively; blending the formulated amount of ethylene-vinyl acetate copolymer, the pre-treated one-dimensional organic polymer nanomaterial powder, the pre-treated two-dimensional layered nanomaterial powder and the silane coupling agent, and granulating them in a molten state to obtain an anti-PID masterbatch;

[0026] S2. Blending the formulated amounts of ethylene-vinyl acetate copolymer, anti-PID masterbatch, main cross-linking agent, auxiliary cross-linking agent and antioxidant, melt-extruding, and casting into a film to obtain an EVA photovoltaic encapsulation film.

[0027] Preferably, in step S1, the pretreatment comprises the following steps performed in sequence: ultrasonic dispersion, centrifugal treatment, solvent replacement with ethanol, drying the replaced precipitate, and grinding and dispersing the dried precipitate into a uniform powder; the granulation temperature is 90-130° C., and a twin-screw granulator is used for granulation;

[0028] In step S2, the temperature of the melt extrusion is 80-100°C.

[0029] The preparation method of the EVA photovoltaic encapsulation adhesive film of the present invention is simple and easy to implement, has low cost and can meet the requirements of batch production.

[0030] The invention also discloses an application of an EVA photovoltaic encapsulation film, and the EVA photovoltaic encapsulation film is applied to a photovoltaic module.

[0031] Compared with the prior art, the present invention has at least the following beneficial effects:

[0032] One-dimensional organic polymer nanomaterials and two-dimensional layered nanomaterials from specific biomass are introduced into ethylene-vinyl acetate copolymer, and an appropriate amount of silane coupling agent is added to achieve uniform compounding of the three materials; the diffusion barrier effect of specific two-dimensional layered nanomaterials (such as organic sodium montmorillonite with an ion exchange capacity of 120-145, an aspect ratio of 150:200-300:500, and a pH of 9.0-10.5) on the permeation path of oxygen and water vapor is utilized, and the environmentally friendly, degradable, high modulus characteristics of one-dimensional organic polymer nanomaterials from specific biomass sources and the hydroxyl groups on their molecular chains are utilized to It forms hydrogen bonds with the vinyl acetate bonds on the EVA molecular chains, reduces the polarity of the EVA molecular chains, effectively avoids the decomposition of EVA while improving the mechanical strength (such as tensile strength), improves the moisture resistance (without adding other moisture resistance additives, a lower water vapor permeability can be obtained), moisture and heat aging resistance, UV resistance and PID resistance of the EVA encapsulation film, and can also solve the problems of environmental post-treatment of film materials; therefore, the EVA encapsulation film of the present invention can improve its aging resistance and mechanical strength when used at the photovoltaic module end, reduce PID attenuation, extend the service life of the battery cell, and improve the photoelectric conversion efficiency. DETAILED DESCRIPTION

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.

[0034] Example 1

[0035] A method for preparing an EVA photovoltaic encapsulation film in this embodiment includes the following preparation steps:

[0036] S1. Preparation of anti-PID masterbatch:

[0037] S11. Pretreatment of one-dimensional organic polymer nanomaterials:

[0038] S111, taking an appropriate amount of one-dimensional organic polymer nanomaterial and dispersing it in water, and performing ultrasonic dispersion, the ultrasonic time is 50 minutes;

[0039] S112, subjecting the suspension after ultrasonic dispersion to high-speed centrifugation, replacing the solvent with ethanol three times, the centrifugal speed is 12000r / min, and the centrifugal time each time is 10min;

[0040] S113, pour out the supernatant after replacement, take the precipitate and dry it in an oven at 60°C for 12h;

[0041] S114, grinding the dried precipitate into powder using a ball mill, grinding the powder until the precipitate is dispersed into a uniform powder, and obtaining a pretreated one-dimensional organic polymer nanomaterial powder.

[0042] In step S11 of this embodiment, the one-dimensional organic polymer nanomaterial is cellulose nanofibrils (CNF), and the aspect ratio of CNF is 30:1.

[0043] S12. Pretreatment of two-dimensional layered nanomaterials:

[0044] S121, dispersing an appropriate amount of two-dimensional layered nanomaterials in water, and performing ultrasonic dispersion, the ultrasonic time being 48 min;

[0045] S122, subjecting the suspension after ultrasonic dispersion to high-speed centrifugation, and replacing the solvent with ethanol three times, with a centrifugal speed of 8000 r / min and a centrifugal time of 10 min each time;

[0046] S123, pour out the supernatant after replacement, take the precipitate and dry it in an oven at 60°C for 12h;

[0047] S124. Grind the dried precipitate into powder using a ball mill, and grind the powder until the precipitate is dispersed into a uniform powder to obtain a pretreated two-dimensional layered nanomaterial powder.

[0048] In step S12 of this embodiment, the two-dimensional layered nanomaterial is organic sodium montmorillonite (MMT), and the ion exchange capacity of the organic sodium montmorillonite is 120, the aspect ratio is 200:300, and the pH is 10.

[0049] S13. 100 parts (weight parts, the same below) of ethylene-vinyl acetate copolymer (EVA), 10 parts of pretreated one-dimensional organic polymer nanomaterial powder, 5 parts of pretreated two-dimensional layered nanomaterial powder and 5 parts of silane coupling agent are granulated in a twin-screw granulator in a molten state at 110°C to obtain an anti-PID masterbatch.

[0050] Step S13 of this embodiment is specifically as follows: take 100 parts of EVA particles, 10 parts of pretreated CNF powder, 5 parts of pretreated MMT powder and 5 parts of γ-(methacryloyloxy)propyltrimethoxysilane, mix them evenly, and then granulate them in a twin-screw granulator at 110°C in a molten state to obtain the anti-PID masterbatch of this embodiment.

[0051] S2. Preparation of EVA photovoltaic encapsulation film: 100 parts of EVA particles, 6 parts of the anti-PID masterbatch of step S13, 0.8 parts of a main cross-linking agent, 0.6 parts of an auxiliary cross-linking agent and 0.5 parts of an antioxidant are blended, melt-extruded at 90° C., and cast into a film to obtain an EVA photovoltaic encapsulation film.

[0052] Step S2 of this embodiment is specifically as follows: take 100 parts of EVA particles, 6 parts of the anti-PID masterbatch of step S13, 0.8 parts of tert-butyl peroxide-2-ethylhexyl carbonate, 0.6 parts of triallyl isocyanurate, and 0.5 parts of bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, mix them evenly, melt them at 90°C, extrude them through a co-extrusion die, and after casting, cooling, and embossing, measure the thickness, trim the edges, roll them up, and package them for storage to obtain the EVA photovoltaic encapsulation film of this embodiment.

[0053] Example 2

[0054] The method for preparing an EVA photovoltaic encapsulation film of this embodiment has specific preparation steps as described in Example 1, and the difference between the method and Example 1 is that:

[0055] In step S11 of this embodiment, the one-dimensional organic polymer nanomaterial is cellulose nanocrystals (CNC), and the crystallinity of CNC is 80%.

[0056] The two-dimensional layered nanomaterial in step S12 of this embodiment is still organic sodium montmorillonite (MMT), and the aspect ratio of the organic sodium montmorillonite is 300:500. The other parameters are the same as those in Example 1.

[0057] In step S13 of this embodiment, in the process of preparing the anti-PID masterbatch, 10 parts of the pretreated CNF powder in Example 1 are replaced with 10 parts of the pretreated CNC powder in this embodiment. The remaining preparation steps and preparation parameters of this embodiment are all referred to Example 1, and the anti-PID masterbatch and EVA photovoltaic encapsulation film of this embodiment are obtained.

[0058] Example 3

[0059] The method for preparing an EVA photovoltaic encapsulation film of this embodiment has specific preparation steps as described in Example 1, and the difference between the method and Example 1 is that:

[0060] In step S11 of this embodiment, the one-dimensional organic polymer nanomaterial is bacterial cellulose (BC), and the crystallinity of BC is 83%.

[0061] The two-dimensional layered nanomaterial in step S12 of this embodiment is the same as that in the first embodiment.

[0062] In step S13 of this embodiment, in the process of preparing the anti-PID masterbatch, 10 parts of the pretreated CNF powder in Example 1 are replaced with 10 parts of the pretreated BC powder in this embodiment. The remaining preparation steps and preparation parameters of this embodiment are all referred to Example 1, and the anti-PID masterbatch and EVA photovoltaic encapsulation film of this embodiment are obtained.

[0063] Example 4

[0064] The method for preparing an EVA photovoltaic encapsulation film of this embodiment has specific preparation steps as described in Example 1, and the difference between the method and Example 1 is that:

[0065] In step S11 of this embodiment, the one-dimensional organic polymer nanomaterial is cellulose nanocrystals (CNC), and the crystallinity of CNC is 80%.

[0066] The two-dimensional layered nanomaterial in step S12 of this embodiment is the same as that in the first embodiment.

[0067] In step S13 of this embodiment, during the process of preparing the anti-PID masterbatch, 10 parts of the pretreated CNF powder in Example 1 are replaced with 10 parts of the pretreated CNC powder in this embodiment, and the remaining preparation steps and preparation parameters are referred to Example 1, so as to obtain the anti-PID masterbatch of this embodiment.

[0068] In step S2 of this embodiment, during the process of preparing the EVA photovoltaic encapsulation film, the 6 parts of anti-PID masterbatch in Example 1 are changed to 10 parts of the anti-PID masterbatch in this embodiment, and the remaining preparation steps and preparation parameters are all referred to Example 1, so as to obtain the EVA photovoltaic encapsulation film of this embodiment.

[0069] Example 5

[0070] The method for preparing an EVA photovoltaic encapsulation film of this embodiment has specific preparation steps as described in Example 1, and the difference between the method and Example 1 is that:

[0071] In step S11 of this embodiment, the one-dimensional organic polymer nanomaterial is bacterial cellulose (BC), and the crystallinity of BC is 83%.

[0072] The two-dimensional layered nanomaterial in step S12 of this embodiment is still organic sodium montmorillonite (MMT), the ion exchange capacity of the organic sodium montmorillonite is 145, and the other parameters are the same as those in Example 1.

[0073] In step S13 of this embodiment, in the process of preparing the anti-PID masterbatch, 10 parts of the pretreated CNF powder in Example 1 are replaced with 10 parts of the pretreated BC powder in this embodiment. The remaining preparation steps and preparation parameters of this embodiment are all referred to Example 1, and the anti-PID masterbatch and EVA photovoltaic encapsulation film of this embodiment are obtained.

[0074] Comparative Example 1

[0075] The preparation method of an EVA photovoltaic encapsulation film in this comparative example comprises the following steps:

[0076] Take 100 parts of EVA particles, 0.8 parts of tert-butyl peroxide-2-ethylhexyl carbonate, 0.6 parts of triallyl isocyanurate, 5 parts of γ-(methacryloyloxy)propyltrimethoxysilane, and 0.5 parts of bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, mix them evenly, melt them at 90°C, extrude them through a co-extrusion die, and after casting, cooling, and embossing, measure the thickness, trim, roll up, and package them for storage to obtain the EVA photovoltaic encapsulation film of this comparative example (that is, the EVA photovoltaic encapsulation film of this comparative example does not include 6 parts of anti-PID masterbatch).

[0077] Comparative Example 2

[0078] The preparation method of an EVA photovoltaic encapsulation film in this comparative example has specific preparation steps referring to Example 1, and the difference between the comparative example and Example 1 is that:

[0079] Step S12 of Example 1 was omitted (ie, the pretreatment step of the two-dimensional layered nanomaterial MMT was omitted).

[0080] Moreover, the preparation process of the anti-PID masterbatch of this comparative example is: take 100 parts of EVA particles, 10 parts of pretreated CNF powder and 5 parts of γ-(methacryloyloxy)propyltrimethoxysilane, mix them evenly, and then granulate them through a twin-screw granulator in a molten state at 110°C to obtain the anti-PID masterbatch of this comparative example (that is, in the preparation process of the anti-PID masterbatch of this comparative example, 5 parts of pretreated MMT powder were not added).

[0081] In the process of preparing the EVA photovoltaic encapsulation film in step S2 of this comparative example, 6 parts of the anti-PID masterbatch in Example 1 are replaced with 6 parts of the anti-PID masterbatch in this comparative example, and the remaining preparation steps and preparation parameters are referred to Example 1, so as to obtain the EVA photovoltaic encapsulation film of this comparative example.

[0082] Comparative Example 3

[0083] The preparation method of an EVA photovoltaic encapsulation film in this comparative example has specific preparation steps referring to Example 1, and the difference between the comparative example and Example 1 is that:

[0084] Step S11 of Example 1 was omitted (ie, the pretreatment step of the one-dimensional organic polymer nanomaterial CNF was omitted).

[0085] Moreover, the preparation process of the anti-PID masterbatch of this comparative example is: take 100 parts of EVA particles, 5 parts of pretreated MMT powder and 5 parts of γ-(methacryloyloxy)propyltrimethoxysilane, mix them evenly, and then granulate them through a twin-screw granulator in a molten state at 110°C to obtain the anti-PID masterbatch of this comparative example (that is, in the preparation process of the anti-PID masterbatch of this comparative example, 10 parts of pretreated CNF powder were not added).

[0086] In the process of preparing the EVA photovoltaic encapsulation film in step S2 of this comparative example, 6 parts of the anti-PID masterbatch in Example 1 are replaced with 6 parts of the anti-PID masterbatch in this comparative example, and the remaining preparation steps and preparation parameters are referred to Example 1, so as to obtain the EVA photovoltaic encapsulation film of this comparative example.

[0087] Performance Testing

[0088] The EVA photovoltaic encapsulation films and corresponding photovoltaic modules prepared in Examples 1-5 and Comparative Examples 1-3 were tested for light transmittance, water vapor permeability, tensile strength, volume resistivity and anti-PID, and the test results are shown in Table 1. The photovoltaic module includes a photovoltaic front panel, a first encapsulation film, a photovoltaic cell sheet, a second encapsulation film and a photovoltaic back panel stacked in sequence from top to bottom; the first encapsulation film and the second encapsulation film are respectively made of the EVA photovoltaic encapsulation films prepared in Examples 1-5 and Comparative Examples 1-3, so that the photovoltaic modules corresponding to Examples 1-5 and Comparative Examples 1-3 are obtained respectively.

[0089] Among them, the transmittance is tested according to the national standard GB / T 29848-2013 "Ethylene-vinyl acetate copolymer (EVA) film for photovoltaic module encapsulation", the water vapor permeability is tested according to the national standard GB / T 26253-2010, the tensile strength is tested according to the national standard GB / T 1040.1-2018, the volume resistivity is tested according to the national standard GB / T 31838.2-2019, and the anti-PID test is carried out according to the industry standard IEC-61215 for the anti-PID test of photovoltaic modules.

[0090] Table 1

[0091]

[0092] From Table 1 we can see that:

[0093] (1) According to the test data of Examples 1-5 (especially Example 1) and Comparative Example 1, it can be seen that the introduction of the anti-PID masterbatch in the present invention is beneficial to improving the tensile strength, volume resistivity and anti-PID performance of the EVA photovoltaic encapsulation film.

[0094] According to the test data of Example 1 and Comparative Example 2, it can be seen that the addition of pretreated two-dimensional layered nanomaterial (MMT) powder to the anti-PID masterbatch in the present invention is beneficial to improving the volume resistivity and anti-PID performance of the EVA photovoltaic encapsulation film.

[0095] According to the test data of Example 1 and Comparative Examples 2-3, it can be known that: the anti-PID masterbatch of Comparative Example 2 contains only pretreated one-dimensional organic polymer nanomaterial (CNF) powder, but does not contain pretreated two-dimensional layered nanomaterial (MMT) powder, and the tensile strength and volume resistivity of the EVA photovoltaic encapsulation film of Comparative Example 2 are not as good as those of Example 1, and the PID attenuation of the EVA photovoltaic encapsulation film of Comparative Example 2 is relatively serious; the anti-PID masterbatch of Comparative Example 3 contains only pretreated two-dimensional layered nanomaterial (MMT) powder, but does not contain pretreated one-dimensional organic polymer nanomaterial (CNF) powder. Although the volume resistivity of the EVA photovoltaic encapsulation film of Comparative Example 3 is improved compared with that of Comparative Example 2, the tensile strength of the EVA photovoltaic encapsulation film of Comparative Example 3 is reduced compared with that of Comparative Example 2, and the tensile strength and volume resistivity of the EVA photovoltaic encapsulation film of Comparative Example 3 are also not as good as those of Example 1, and the PID attenuation of the EVA photovoltaic encapsulation film of Comparative Example 3 is still relatively serious.

[0096] (2) According to the test data of Examples 1-3, it can be seen that: as the crystallinity of the pretreated one-dimensional organic polymer nanomaterial powder added to the anti-PID masterbatch increases, the tensile strength and volume resistivity of the EVA photovoltaic encapsulation film obtained by the present invention increase accordingly, but the transmittance of the EVA photovoltaic encapsulation film at 380-1100nm decreases.

[0097] (3) According to the test data of Example 3 (the ion exchange capacity of MMT in its anti-PID masterbatch is 120) and Example 5 (the ion exchange capacity of MMT in its anti-PID masterbatch is 145), Example 2 (the aspect ratio of MMT in its anti-PID masterbatch is 300:500) and Example 4 (the aspect ratio of MMT in its anti-PID masterbatch is 200:300), it can be known that: if the ion exchange capacity of the treated MMT powder contained in the anti-PID masterbatch is higher, the bulk resistivity of the EVA photovoltaic encapsulation film obtained by the present invention is higher, and the corresponding anti-PID performance is better, but the tensile strength of the EVA photovoltaic encapsulation film is reduced; if the aspect ratio of the treated MMT powder contained in the anti-PID masterbatch is smaller, the tensile strength and anti-PID performance of the corresponding EVA photovoltaic encapsulation film of the present invention are better.

[0098] In summary, as shown in the test results of Examples 1-5 of the present invention, the anti-PID masterbatch obtained by compounding one-dimensional organic polymer nanomaterials with higher crystallinity and two-dimensional layered nanomaterials with smaller aspect ratio and higher ion exchange capacity has an excellent synergistic effect on improving the overall performance of EVA photovoltaic encapsulation film. Therefore, the EVA photovoltaic encapsulation film prepared by the present invention has the advantages of good light transmittance, low water vapor permeability, high tensile strength and low PID attenuation, which expands the application of EVA photovoltaic encapsulation film in the field of photovoltaic module packaging.

[0099] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0100] The technical solution provided by the present invention is introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. An EVA photovoltaic encapsulation film, characterized in that: It includes the following raw materials in parts by weight: 85-100 parts of ethylene-vinyl acetate copolymer, 1-15 parts of anti-PID masterbatch, 0.5-1 parts of main cross-linking agent, 0.1-0.8 parts of auxiliary cross-linking agent and 0.1-1 parts of antioxidant; Wherein, the anti-PID masterbatch comprises the following raw materials in parts by weight: 60-100 parts of ethylene-vinyl acetate copolymer, 1-20 parts of one-dimensional organic polymer nanomaterial, 1-10 parts of two-dimensional layered nanomaterial and 2-10 parts of silane coupling agent; The one-dimensional organic polymer nanomaterial is at least one of cellulose nanofibrils, cellulose nanocrystals, and bacterial cellulose with multiple hydroxyl groups; The two-dimensional layered nanomaterial is organic sodium montmorillonite; the organic sodium montmorillonite has an ion exchange capacity of 120-145, an aspect ratio of 300:500-150:200, and a pH of 9.0-10.5; The aspect ratio of the cellulose nanofibrils is 20:1-40:1; the crystallinity of the cellulose nanocrystals is 75-85%; and the crystallinity of the bacterial cellulose is 80-85%.

2. An EVA photovoltaic encapsulation film according to claim 1, characterized in that: The one-dimensional organic polymer nanomaterial is bacterial cellulose with a crystallinity of 80-85%.

3. The EVA photovoltaic encapsulation film according to claim 1, characterized in that: The organic sodium-based montmorillonite has an ion exchange capacity of 145 and an aspect ratio of 300:500-200:

300.

4. The EVA photovoltaic encapsulation film according to claim 1, characterized in that: In the EVA photovoltaic encapsulation film, the weight ratio of ethylene-vinyl acetate copolymer: anti-PID masterbatch: main cross-linking agent: auxiliary cross-linking agent: antioxidant is 100:6-10:0.8:0.6:0.5; In the anti-PID masterbatch, the weight ratio of ethylene-vinyl acetate copolymer: one-dimensional organic polymer nanomaterial: two-dimensional layered nanomaterial: silane coupling agent is 100:8-12:4-6:

5.

5. The EVA photovoltaic encapsulation film according to claim 1, characterized in that: The main cross-linking agent is one or more of tert-butyl peroxide-2-ethylhexyl carbonate, dibenzoyl peroxide, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, and 1,1-di-tert-butylperoxide-3,3,5-trimethylcyclohexane; The auxiliary cross-linking agent is one or more of triallyl isocyanurate, diethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, triallyl cyanurate, and ethoxylated trimethylolpropane triacrylate; The antioxidant is one or more of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris(2,4-di-tert-butylphenyl) phosphite, and bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate; The silane coupling agent is one or more of γ-glycidyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane or γ-(methacryloyloxy)propyltrimethoxysilane.

6. A method for preparing an EVA photovoltaic encapsulation film according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: S1. Pre-treating the one-dimensional organic polymer nanomaterial and the two-dimensional layered nanomaterial respectively to obtain the one-dimensional organic polymer nanomaterial powder and the two-dimensional layered nanomaterial powder respectively; blending the formulated amount of ethylene-vinyl acetate copolymer, the pre-treated one-dimensional organic polymer nanomaterial powder, the pre-treated two-dimensional layered nanomaterial powder and the silane coupling agent, and granulating them in a molten state to obtain an anti-PID masterbatch; S2. Blending the formulated amounts of ethylene-vinyl acetate copolymer, anti-PID masterbatch, main cross-linking agent, auxiliary cross-linking agent and antioxidant, melt-extruding, and casting into a film to obtain an EVA photovoltaic encapsulation film.

7. The method for preparing an EVA photovoltaic encapsulation film according to claim 6, characterized in that: In step S1, the pretreatment includes the following steps in sequence: ultrasonic dispersion, centrifugal treatment, solvent replacement with ethanol, drying the replaced precipitate, and grinding and dispersing the dried precipitate into a uniform powder; the granulation temperature is 90-130° C., and a twin-screw granulator is used for granulation; In step S2, the temperature of the melt extrusion is 80-100°C.

8. The use of an EVA photovoltaic encapsulation film according to any one of claims 1 to 5, characterized in that: The EVA photovoltaic encapsulation film is applied to photovoltaic modules.