A composite fireproof sealing strip and its preparation process and application

By adding modified titanium dioxide and sericite powder composite structural particles to the fire-proof sealing strip, the problems of aging and sealing failure of the strip are solved, and better waterproof, aging and corrosion resistance are achieved, and high-performance sealing is met need.

CN118562419BActive Publication Date: 2024-11-12LINQU RUIXING PLASTIC PROD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411057147.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing fire-proof sealant strips are prone to aging, hardening and deforming under the influence of factors such as environmental temperature difference, ultraviolet irradiation, mechanical stress, etc., resulting in seal failure, water vapor and dust infiltration, increasing fire hazards, and water vapor invasion limits its application environment.

Method used

Using composite fire-resistant sealant strips, a mixture of modified titanium dioxide and sericite powder is added to form composite structural particles, improving waterproofness and aging resistance, and enhancing the penetration resistance and electrons inside the colloid by controlling the particle size and surface hydrophilicity. Current-carrying path to reduce corrosion and yellowing.

Benefits of technology

It achieves the improvement of waterproof, aging and corrosion resistance of rubber strips while maintaining excellent fire-resistant flame retardant performance, extending service life and enhancing market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of sealing rubber, and in particular to a composite fireproof sealing strip and its preparation process and application. The composite fireproof sealing strip, in parts by mass, comprises the following raw materials: 60 to 80 parts of base rubber, 30 to 45 parts of filling powder, 3 to 6 parts of cross-linking agent, 4 to 8 parts of dispersant, 0.5 to 3 parts of vulcanization accelerator, 3 to 5 parts of lubricant, 15 to 25 parts of oil agent, and 1 to 15 parts of auxiliary agent. The composite fireproof sealing strip prepared in the present application has excellent fireproof and flame retardant properties while ensuring that it has good waterproof, aging resistance, sealing and corrosion resistance, thereby meeting the performance requirements for fireproof sealing strips in existing specific environments, and has very excellent application and market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sealing rubber, and in particular to a composite fireproof sealing rubber strip and a preparation process and application thereof. Background Art

[0002] Sealing strips are a kind of strip or rod-shaped products made of rubber or similar elastic materials, which are widely used in automobiles, machinery, building doors and windows, and other fields that require sealing. Its main function is to form a barrier at various joints to prevent the penetration or loss of internal and external media such as gas, liquid, dust, etc., and it also has the effects of sound insulation, fireproofing, heat insulation, and shockproofing. Among them, fireproof sealing strips are usually installed in fire doors, firewalls, cable penetrations, pipe penetrations, and other gaps in buildings that require fireproofing and isolation, and maintain good softness and elasticity to ensure good sealing performance. When encountering high temperatures in fire, it can quickly expand to form a heat-insulating and smoke-isolating barrier, effectively preventing the spread of fire through the gaps, and reducing the spread of toxic smoke, protecting people's lives and reducing property losses.

[0003] In the prior art, the application of fireproof sealing strips often faces some challenges. For example, in the traditional fireproof sealing assembly of some structures, a single sealing structure is usually adopted, that is, only one fireproof sealing strip is arranged in the gap. Although this design is simple, as time goes by, because ordinary fireproof sealing strips tend to focus on fireproof effects, and their own sealing, waterproof and other properties are poor, under the influence of factors such as environmental temperature difference changes, ultraviolet radiation, and mechanical stress, fireproof sealing strips are prone to aging, hardening, deformation, and even failure, manifested as warping, shedding, blistering, yellowing and other phenomena. Once the seal fails, water vapor and dust can take advantage of the opportunity to enter and accumulate inside the gap. The accumulation of dust will increase the fire hazard, and the intrusion of water vapor greatly limits the application environment and scenarios of fireproof sealing strips. In some application environments, it is also prone to corrosion and sticking, oxidation and yellowing, which greatly reduces its quality of use and life.

[0004] Therefore, in order to solve the above problems, the present application provides a composite fireproof sealing strip and its preparation process and application. The composite fireproof sealing strip prepared in the present application has excellent fire retardant properties while ensuring that it has good waterproof, aging resistance, sealing and corrosion resistance, thereby meeting the performance requirements for fireproof sealing strips in the existing specific environment, and has very excellent application and market prospects. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present application provides a composite fireproof sealing strip, the raw materials of which include, by mass: 60 to 80 parts of base rubber, 30 to 45 parts of filling powder, 3 to 6 parts of cross-linking agent, 4 to 8 parts of dispersant, 0.5 to 3 parts of vulcanization accelerator, 3 to 5 parts of lubricant, 15 to 25 parts of oil agent, and 1 to 15 parts of auxiliary agent.

[0006] As a preferred solution, the mass ratio of the base rubber, filler powder and oil agent is (6.5~7.5):(3.2~4):(2~2.4).

[0007] As a preferred solution, the mass ratio of the base rubber, filler powder and oil agent is (7-7.5): (3.4-3.8): (2-2.2).

[0008] As a preferred solution, the base rubber is a composition of EPDM rubber, chloroprene rubber and fluorine-containing resin.

[0009] As a preferred solution, the mass ratio of the EPDM rubber, chloroprene rubber and fluororesin is (6-8): (2-3): (1-1.8).

[0010] As a preferred solution, the mass ratio of the EPDM rubber, chloroprene rubber and fluororesin is (7-8): (2-2.5): (1.5-1.8).

[0011] As a preferred solution, the mass ratio of the EPDM rubber, chloroprene rubber and fluorine-containing resin is 7.5:2.4:1.6.

[0012] As a preferred solution, the Mooney viscosity of the EPDM rubber is 65-80MU, ML 1+4 125℃.

[0013] As a preferred solution, the Mooney viscosity of the EPDM rubber is 70-75MU, ML 1+4 125℃.

[0014] As a preferred solution, the fluorine-containing resin is at least one of ethylene-tetrafluoroethylene copolymer resin, fluorinated ethylene propylene copolymer resin, polytetrafluoroethylene, and PFA.

[0015] As a preferred solution, the fluorine-containing resin is ethylene-tetrafluoroethylene copolymer resin.

[0016] As a preferred solution, the melt flow rate of the ethylene-tetrafluoroethylene copolymer resin is 5-12 g / 10 min, 300° C. / 1.2 kg.

[0017] As a preferred solution, the melt flow rate of the ethylene-tetrafluoroethylene copolymer resin is 6-8 g / 10 min, 300° C. / 1.2 kg.

[0018] As a preferred solution, the filler powder is a composition of sericite powder and modified titanium dioxide particles.

[0019] As a preferred solution, the mass ratio of the sericite powder to the modified titanium dioxide particles is (4-4.5): (1-1.5).

[0020] As a preferred solution, the average particle size of the sericite powder is 0.4-1 μm.

[0021] As a preferred scheme, the preparation method of the modified titanium dioxide particles comprises the following steps: S1: adding aluminum nitrate nonahydrate and acetic acid to deionized water and stirring evenly at room temperature, then adding to a closed reactor, and keeping warm for reaction at 50-65°C for 1-2 hours; S2: heating to 190-210°C, controlling the pressure of the reactor to 1.9-2.1 MPa, adding terephthalic acid and continuing stirring for reaction for 8-10 hours; S3: after the reaction is completed, taking the reaction solution to a common reaction container, adding succinic anhydride and 3-aminopropyltriethoxysilane, heating to 60-65°C and reacting for 2-3 hours; S4: after the reaction is completed, centrifugally filtering the product, washing it, adding it to deionized water, heating it to 55-60°C, and dropping a mixed solution containing ammonia water, ethyl orthosilicate and titanium dioxide, the dropping time is 20-40 minutes, and keeping warm for reaction for 2.2-2.8 hours after the dropping is completed. After completion, the product is centrifuged and washed, and vacuum dried to obtain.

[0022] As a preferred solution, the average particle size of the titanium dioxide is 15-30 nm.

[0023] As a preferred solution, the mass ratio of aluminum nitrate nonahydrate, acetic acid, terephthalic acid and titanium dioxide is (4-5): (15-20): (2-2.5): (3-4).

[0024] As a preferred solution, the mass ratio of succinic anhydride to 3-aminopropyltriethoxysilane is (3-5): (0.3-0.6).

[0025] As a preferred solution, the average particle size of the modified titanium dioxide is 480-600 nm.

[0026] In the present application, the modified titanium dioxide added above is mixed with the sericite powder to form composite structure particles, which greatly improves the waterproofness, aging resistance, corrosion resistance and UV resistance of the sealing strip. The added modified titanium dioxide can form a spherical structure in which the surface of the titanium dioxide particles wraps the framework particles. The existence of this structure can ensure the overall size of the composite particles by controlling the reaction time, thereby causing the surface of the framework particles to be exposed, and controlling the hydrophilicity of the particle surface, thereby ensuring that the modified particles can guide and attract water molecules inside the strip, and absorb and remove them through the pores of the framework particles, not only having excellent waterproofness, but also greatly improving the penetration resistance of active molecules and water-soluble groups to the internal system of the colloid, thereby greatly reducing the probability of corrosive chemical reactions; if the overall particle size of the modified particles is too small, it is easy to form an overly hydrophilic spherical surface, and the framework particles cannot be effectively exposed, and then during use, it can only play a water molecule attraction effect, but leads to a decrease in waterproofness. On the other hand, the coordination structure of titanium dioxide and framework particles can easily form a good electron current path, thereby reducing the bandgap distance of the modified particles as a whole, greatly improving the absorption of ultraviolet light energy by the modified particles, and avoiding yellowing and oxidation of the rubber strips under long-term light exposure.

[0027] As a preferred solution, the cross-linking agent is at least one of dibenzoyl peroxide, dicumyl peroxide, zinc oxide and magnesium oxide.

[0028] As a preferred solution, the cross-linking agent is dibenzoyl peroxide.

[0029] As a preferred solution, the dispersant is at least one of zinc stearate, sodium dodecyl sulfate, sodium lauryl sulfate, triethylhexyl phosphate, methyl amyl alcohol, sodium tripolyphosphate, sodium hexametaphosphate, and carboxymethyl cellulose.

[0030] As a preferred solution, the dispersant is a combination of zinc stearate and sodium lauryl sulfate.

[0031] As a preferred solution, the mass ratio of zinc stearate to sodium lauryl sulfate is (2-4): (0.4-0.6).

[0032] As a preferred solution, the vulcanization accelerator is at least one of ZDC, DPTT, DZ, TMTD, TETD, and CBS.

[0033] As a preferred solution, the vulcanization accelerator is a combination of ZDC and DPTT.

[0034] As a preferred solution, the mass ratio of ZDC to DPTT is (1.5~2):(0.8~1).

[0035] As a preferred solution, the lubricant is at least one of polyethylene wax, fatty acid amides, silicone oil, and calcium-based ester.

[0036] As a preferred solution, the lubricant is polyethylene wax.

[0037] As a preferred solution, the oil agent is at least one of white mineral oil, epoxidized soybean oil and olive oil.

[0038] As a preferred solution, the oil agent is a composition of white mineral oil and epoxidized soybean oil.

[0039] As a preferred solution, the mass ratio of the white mineral oil to the epoxidized soybean oil is (3-4): (0.6-1).

[0040] As a preferred solution, the auxiliary agent at least includes a flame retardant.

[0041] As a preferred solution, the flame retardant is at least one of aluminum hydroxide, magnesium hydroxide, zinc borate, molybdenum oxide, chlorinated paraffin, triphenyl phosphate, and tricresyl phosphate.

[0042] As a preferred solution, the flame retardant is a combination of zinc borate and triphenyl phosphate.

[0043] As a preferred solution, the mass ratio of zinc borate to triphenyl phosphate is (1-1.5):(2-4).

[0044] The second aspect of the present application provides a preparation process for the above-mentioned composite fireproof sealing strip, and the preparation process comprises the following steps: D1: putting the base rubber into an internal mixer, adjusting the temperature to 60-80°C and mixing for 4-5 minutes; D2: adding the remaining raw materials, and mixing at 65-75°C for 2-3 minutes; D3: after the mixing is completed, taking out the obtained rubber material and stretching it into a strip-shaped colloid, and placing it into an extruder, and extruding it through a mold to obtain a molded rubber strip; D4: subjecting the molded rubber strip to a salt bath and vulcanization setting, and then cleaning it to obtain the obtained strip.

[0045] The third aspect of the present application provides the use of any of the above-mentioned composite fireproof sealing strips in the field of door and window sealing.

[0046] The beneficial effects of this application are:

[0047] 1. A composite fireproof sealing strip provided in the present application has excellent fireproof and flame retardant properties while ensuring that it has good waterproof, aging-resistant, sealing and corrosion-resistant properties, thereby meeting the performance requirements for fireproof sealing strips in existing specific environments and having very excellent application and market prospects.

[0048] 2. A composite fireproof sealing strip provided in the present application, in which modified titanium dioxide is added and mixed with sericite powder to form composite structure particles, which greatly improves the waterproofness, aging resistance and corrosion resistance of the sealing strip; the added modified titanium dioxide can form a spherical structure in which the surface of the titanium dioxide particles wraps the framework particles. The existence of this structure can ensure the overall size of the composite particles by controlling the reaction time, thereby causing the surface of the framework particles to be exposed and controlling the hydrophilicity of the particle surface, thereby ensuring that the modified particles can guide and attract water molecules inside the strip and absorb and remove them through the pores of the framework particles. It not only has excellent waterproofness, but also can greatly improve the penetration resistance of active molecules and water-soluble groups to the internal system of the colloid, thereby greatly reducing the probability of corrosive chemical reactions. If the overall particle size of the modified particles is too small, it is easy to form an overly hydrophilic spherical surface, and the framework particles cannot be effectively exposed, so that during use, it can only play a water molecule attraction effect, which leads to a decrease in waterproofness.

[0049] 3. The composite fireproof sealing strip provided in the present application has a modified titanium dioxide whose coordination structure can easily form a good electron current path, thereby reducing the bandgap distance of the modified particles as a whole, greatly improving the absorption effect of the modified particles on ultraviolet light energy, and avoiding the yellowing and oxidation of the strip under long-term light exposure. DETAILED DESCRIPTION

[0050] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.

[0051] The composite fireproof sealing strips described in the examples of the present application are mainly used in the field of door and window sealing. In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.

[0052] Example 1

[0053] Embodiment 1 The first aspect provides a composite fireproof sealing strip, and the raw materials include, by mass: 73.5 parts of base rubber, 35 parts of filling powder, 4.2 parts of cross-linking agent, 5.8 parts of dispersant, 2.1 parts of vulcanization accelerator, 3.8 parts of lubricant, 21 parts of oil agent, and 8.5 parts of auxiliary agent.

[0054] The base rubber is a composition of EPDM rubber, chloroprene rubber and fluorine-containing resin, and the mass ratio of the three is 7.5:2.4:1.6. The fluorine-containing resin is ethylene-tetrafluoroethylene copolymer resin.

[0055] The EPDM rubber was purchased from the 3112M model sold by Sinopec Mitsui, with a Mooney viscosity of 71MU, ML 1+ 4125℃.

[0056] The chloroprene rubber is CR244 chloroprene rubber; the ethylene-tetrafluoroethylene copolymer resin is purchased from Japan Daikin EP610 model product, and its melt flow rate is 6.6g / 10min, 300℃ / 1.2Kg.

[0057] The filling powder is a composition of sericite powder and modified titanium dioxide particles, and the mass ratio of the two is 4.2:1.2.

[0058] The average particle size of the sericite powder is 0.5 μm.

[0059] The preparation method of modified titanium dioxide particles comprises the following steps, calculated by mass: S1: adding 4.65 parts of aluminum nitrate nonahydrate and 18.8 parts of acetic acid to 150 parts of deionized water and stirring at room temperature, then adding to a closed reactor and keeping the temperature at 60°C for 1.5 hours; S2: heating to 200°C, controlling the pressure of the reactor to 2.1MPa, adding 2.32 parts of terephthalic acid and stirring the reaction for 9.5 hours; S3: after the reaction is completed, taking the reaction solution to a common reaction container and adding Add 3.88 parts of succinic anhydride and 0.42 parts of 3-aminopropyltriethoxysilane, heat to 60°C and react for 3 hours; S4: After the reaction is completed, centrifuge and filter the product, wash it, add it to 120 parts of deionized water, heat it to 60°C, and drop a mixed aqueous solution containing 1.2 parts of ammonia water, 2.2 parts of ethyl orthosilicate and 3.6 parts of titanium dioxide (30 parts in total), add it for 40 minutes, keep it warm and react for 2.4 hours, and after completion, centrifuge and wash the product, and dry it in vacuum to obtain the product.

[0060] The average particle size of titanium dioxide is 20 nm; the average particle size of modified titanium dioxide is 542 nm.

[0061] The cross-linking agent is dibenzoyl peroxide; the dispersing agent is a composition of zinc stearate and sodium lauryl sulfate, and the mass ratio of the two is 2.8:0.5.

[0062] The vulcanization accelerator is a composition of ZDC and DPTT, and the mass ratio of the two is 1.8:0.9.

[0063] The lubricant is polyethylene wax purchased from Henan Tianchou Chemical Industry with an acid value of 15.

[0064] The oil agent is a composition of white mineral oil and epoxidized soybean oil, and the mass ratio of the two is 3.2:0.8; the white mineral oil is white mineral oil 5#; the epoxidized soybean oil is purchased from the industrial-grade epoxidized soybean oil product sold by Nalmei New Materials Co., Ltd.

[0065] The auxiliary agent is a flame retardant, which is a combination of zinc borate and triphenyl phosphate, and the mass ratio of the two is 1.3:3.2.

[0066] The second aspect of the present embodiment provides a preparation process of the above-mentioned composite fireproof sealing strip, and the preparation process includes the following steps: D1: putting the base rubber into an internal mixer, adjusting the temperature to 70°C and mixing for 4 minutes; D2: adding the remaining raw materials and mixing at 65°C for 2 minutes; D3: after the mixing is completed, taking out the obtained rubber material and stretching it into a strip-shaped colloid, and placing it in an extruder, and extruding it through a mold to obtain a molded rubber strip; D4: salt bathing and vulcanization of the molded rubber strip, and cleaning it to obtain it.

[0067] Example 2

[0068] The first aspect of Example 2 provides a composite fireproof sealing strip, in which the raw materials include, by mass: 66.8 parts of base rubber, 32 parts of filling powder, 4.8 parts of cross-linking agent, 5.2 parts of dispersant, 1.9 parts of vulcanization accelerator, 4.1 parts of lubricant, 24 parts of oil agent, and 8 parts of auxiliary agent.

[0069] The base rubber is a composition of EPDM rubber, chloroprene rubber and fluorine-containing resin, and the mass ratio of the three is 7:2.6:1.2. The fluorine-containing resin is ethylene-tetrafluoroethylene copolymer resin.

[0070] The EPDM rubber was purchased from the 3112M model sold by Sinopec Mitsui, with a Mooney viscosity of 71MU, ML 1+ 4125℃.

[0071] The chloroprene rubber is CR244 chloroprene rubber; the ethylene-tetrafluoroethylene copolymer resin is purchased from Japan Daikin EP610 model product, and its melt flow rate is 6.6g / 10min, 300℃ / 1.2Kg.

[0072] The filling powder is a composition of sericite powder and modified titanium dioxide particles, and the mass ratio of the two is 4.5:1.

[0073] The average particle size of the sericite powder is 0.6 μm.

[0074] The preparation method of modified titanium dioxide particles comprises the following steps, calculated by mass: S1: adding 4.65 parts of aluminum nitrate nonahydrate and 18.8 parts of acetic acid to 150 parts of deionized water and stirring at room temperature, then adding to a closed reactor and keeping the temperature at 60°C for 1.5 hours; S2: heating to 200°C, controlling the pressure of the reactor to 2.1MPa, adding 2.32 parts of terephthalic acid and stirring the reaction for 9.5 hours; S3: after the reaction is completed, taking the reaction solution to a common reaction container and adding Add 3.88 parts of succinic anhydride and 0.42 parts of 3-aminopropyltriethoxysilane, heat to 60°C and react for 3 hours; S4: After the reaction is completed, centrifuge and filter the product, wash it, add it to 120 parts of deionized water, heat it to 60°C, and drop a mixed aqueous solution containing 1.2 parts of ammonia water, 2.2 parts of ethyl orthosilicate and 3.6 parts of titanium dioxide (30 parts in total), add it for 40 minutes, keep it warm and react for 2.4 hours, and after completion, centrifuge and wash the product, and dry it in vacuum to obtain the product.

[0075] The average particle size of titanium dioxide is 20 nm; the average particle size of modified titanium dioxide is 542 nm.

[0076] The cross-linking agent is dibenzoyl peroxide; the dispersing agent is a composition of zinc stearate and sodium lauryl sulfate, and the mass ratio of the two is 2.8:0.5.

[0077] The vulcanization accelerator is a composition of ZDC and DPTT, and the mass ratio of the two is 1.8:0.9.

[0078] The lubricant is polyethylene wax purchased from Henan Tianchou Chemical Industry with an acid value of 15.

[0079] The oil agent is a composition of white mineral oil and epoxidized soybean oil, and the mass ratio of the two is 3.2:0.8; the white mineral oil is white mineral oil 5#; the epoxidized soybean oil is purchased from the industrial-grade epoxidized soybean oil product sold by Nalmei New Materials Co., Ltd.

[0080] The auxiliary agent is a flame retardant, which is a combination of zinc borate and triphenyl phosphate, and the mass ratio of the two is 1.3:3.2.

[0081] The second aspect of the present embodiment provides a preparation process of the above-mentioned composite fireproof sealing strip, and the preparation process includes the following steps: D1: putting the base rubber into an internal mixer, adjusting the temperature to 70°C and mixing for 4 minutes; D2: adding the remaining raw materials and mixing at 65°C for 2 minutes; D3: after the mixing is completed, taking out the obtained rubber material and stretching it into a strip-shaped colloid, and placing it in an extruder, and extruding it through a mold to obtain a molded rubber strip; D4: salt bathing and vulcanization of the molded rubber strip, and cleaning it to obtain it.

[0082] Example 3

[0083] The first aspect of Example 3 provides a composite fireproof sealing strip, in which the raw materials include, by mass: 65 parts of base rubber, 40 parts of filling powder, 4.2 parts of cross-linking agent, 5.8 parts of dispersant, 2.1 parts of vulcanization accelerator, 3.8 parts of lubricant, 24 parts of oil agent, and 8.5 parts of additives.

[0084] The base rubber is a composition of EPDM rubber, chloroprene rubber and fluorine-containing resin, and the mass ratio of the three is 8:2:1.5. The fluorine-containing resin is ethylene-tetrafluoroethylene copolymer resin.

[0085] The EPDM rubber was purchased from the 3112M model sold by Sinopec Mitsui, with a Mooney viscosity of 71MU, ML 1+ 4125℃.

[0086] The chloroprene rubber is CR244 chloroprene rubber; the ethylene-tetrafluoroethylene copolymer resin is purchased from Japan Daikin EP610 model product, and its melt flow rate is 6.6g / 10min, 300℃ / 1.2Kg.

[0087] The filling powder is a composition of sericite powder and modified titanium dioxide particles, and the mass ratio of the two is 4.5:1.

[0088] The average particle size of the sericite powder is 0.9 μm.

[0089] The preparation method of modified titanium dioxide particles comprises the following steps, calculated by mass: S1: adding 4.65 parts of aluminum nitrate nonahydrate and 18.8 parts of acetic acid to 150 parts of deionized water and stirring at room temperature, then adding to a closed reactor and keeping the temperature at 60°C for 1.5 hours; S2: heating to 200°C, controlling the pressure of the reactor to 2.1MPa, adding 2.32 parts of terephthalic acid and stirring the reaction for 9.5 hours; S3: after the reaction is completed, taking the reaction solution to a common reaction container and adding Add 3.88 parts of succinic anhydride and 0.42 parts of 3-aminopropyltriethoxysilane, heat to 60°C and react for 3 hours; S4: After the reaction is completed, centrifuge and filter the product, wash it, add it to 120 parts of deionized water, heat it to 60°C, and drop a mixed aqueous solution containing 1.2 parts of ammonia water, 2.2 parts of ethyl orthosilicate and 3.6 parts of titanium dioxide (30 parts in total), add it for 40 minutes, keep it warm and react for 2.4 hours, and after completion, centrifuge and wash the product, and dry it in vacuum to obtain the product.

[0090] The average particle size of titanium dioxide is 30 nm; the average particle size of modified titanium dioxide is 592 nm.

[0091] The cross-linking agent is dibenzoyl peroxide; the dispersing agent is a composition of zinc stearate and sodium lauryl sulfate, and the mass ratio of the two is 3.8:0.4.

[0092] The vulcanization accelerator is a composition of ZDC and DPTT, and the mass ratio of the two is 1.5:1.

[0093] The lubricant is polyethylene wax purchased from Henan Tianchou Chemical Industry with an acid value of 15.

[0094] The oil agent is a composition of white mineral oil and epoxidized soybean oil, and the mass ratio of the two is 4:0.6; the white mineral oil is white mineral oil 5#; the epoxidized soybean oil is purchased from the industrial-grade epoxidized soybean oil product sold by Narmei New Materials Co., Ltd.

[0095] The auxiliary agent is a flame retardant, which is a combination of zinc borate and triphenyl phosphate, and the mass ratio of the two is 1:4.

[0096] The second aspect of the present embodiment provides a preparation process of the above-mentioned composite fireproof sealing strip, and the preparation process includes the following steps: D1: putting the base rubber into an internal mixer, adjusting the temperature to 70°C and mixing for 4 minutes; D2: adding the remaining raw materials and mixing at 65°C for 2 minutes; D3: after the mixing is completed, taking out the obtained rubber material and stretching it into a strip-shaped colloid, and placing it in an extruder, and extruding it through a mold to obtain a molded rubber strip; D4: salt bathing and vulcanization of the molded rubber strip, and cleaning it to obtain it.

[0097] Example 4

[0098] Example 4 The first aspect provides a composite fireproof sealing strip, in which the raw materials include, by mass: 75 parts of base rubber, 32 parts of filling powder, 4.2 parts of cross-linking agent, 5.8 parts of dispersant, 2.1 parts of vulcanization accelerator, 3.8 parts of lubricant, 20 parts of oil agent, and 8.5 parts of additives.

[0099] The base rubber is a composition of EPDM rubber, chloroprene rubber and fluorine-containing resin, and the mass ratio of the three is 6:3:1.8. The fluorine-containing resin is ethylene-tetrafluoroethylene copolymer resin.

[0100] The EPDM rubber was purchased from the 3112M model sold by Sinopec Mitsui, with a Mooney viscosity of 71MU, ML 1+ 4125℃.

[0101] The chloroprene rubber is CR244 chloroprene rubber; the ethylene-tetrafluoroethylene copolymer resin is purchased from Japan Daikin EP610 model product, and its melt flow rate is 6.6g / 10min, 300℃ / 1.2Kg.

[0102] The filling powder is a composition of sericite powder and modified titanium dioxide particles, and the mass ratio of the two is 4:1.5.

[0103] The average particle size of the sericite powder is 0.5 μm.

[0104] The preparation method of modified titanium dioxide particles comprises the following steps, calculated by mass: S1: adding 4.65 parts of aluminum nitrate nonahydrate and 18.8 parts of acetic acid to 150 parts of deionized water and stirring at room temperature, then adding to a closed reactor and keeping the temperature at 60°C for 1.5 hours; S2: heating to 200°C, controlling the pressure of the reactor to 2.1MPa, adding 2.32 parts of terephthalic acid and stirring the reaction for 9.5 hours; S3: after the reaction is completed, taking the reaction solution to a common reaction container and adding Add 3.88 parts of succinic anhydride and 0.42 parts of 3-aminopropyltriethoxysilane, heat to 60°C and react for 3 hours; S4: After the reaction is completed, centrifuge and filter the product, wash it, add it to 120 parts of deionized water, heat it to 60°C, and drop a mixed aqueous solution containing 1.2 parts of ammonia water, 2.2 parts of ethyl orthosilicate and 3.6 parts of titanium dioxide (30 parts in total), add it for 40 minutes, keep it warm and react for 2.4 hours, and after completion, centrifuge and wash the product, and dry it in vacuum to obtain the product.

[0105] The average particle size of titanium dioxide is 15 nm; the average particle size of modified titanium dioxide is 517 nm.

[0106] The cross-linking agent is dibenzoyl peroxide; the dispersing agent is a composition of zinc stearate and sodium lauryl sulfate, and the mass ratio of the two is 2:0.6.

[0107] The vulcanization accelerator is a composition of ZDC and DPTT, and the mass ratio of the two is 2:0.8.

[0108] The lubricant is polyethylene wax purchased from Henan Tianchou Chemical Industry with an acid value of 15.

[0109] The oil agent is a composition of white mineral oil and epoxidized soybean oil, and the mass ratio of the two is 3:1; the white mineral oil is white mineral oil 5#; the epoxidized soybean oil is purchased from the industrial-grade epoxidized soybean oil product sold by Narmei New Materials Co., Ltd.

[0110] The auxiliary agent is a flame retardant, which is a combination of zinc borate and triphenyl phosphate, and the mass ratio of the two is 1.5:2.

[0111] The second aspect of the present embodiment provides a preparation process of the above-mentioned composite fireproof sealing strip, and the preparation process includes the following steps: D1: putting the base rubber into an internal mixer, adjusting the temperature to 70°C and mixing for 4 minutes; D2: adding the remaining raw materials and mixing at 65°C for 2 minutes; D3: after the mixing is completed, taking out the obtained rubber material and stretching it into a strip-shaped colloid, and placing it in an extruder, and extruding it through a mold to obtain a molded rubber strip; D4: salt bathing and vulcanization of the molded rubber strip, and cleaning it to obtain it.

[0112] Comparative Example 1

[0113] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of EPDM rubber, chloroprene rubber and fluorine-containing resin is 9.5:1:0.4.

[0114] Comparative Example 2

[0115] The specific implementation of this comparative example is basically the same as that of Example 1, except that the Mooney viscosity of the EPDM rubber is 52MU, ML 1+4 125℃, purchased from Sinopec Mitsui with corresponding viscosity.

[0116] Comparative Example 3

[0117] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of sericite powder to modified titanium dioxide particles is 9:1.

[0118] Comparative Example 4

[0119] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of modified titanium dioxide particles comprises the following steps, calculated by mass: S1: adding 2.25 parts of aluminum nitrate nonahydrate and 20 parts of acetic acid to 150 parts of deionized water and stirring at room temperature, then adding to a sealed reactor, and keeping the temperature at 60°C for 1.5 hours; S2: heating to 200°C, controlling the pressure of the reactor to 2.1MPa, adding 1.2 parts of terephthalic acid and continuing stirring for 9.5 hours; S3: taking out after the reaction is completed Add 3.88 parts of succinic anhydride and 0.42 parts of 3-aminopropyltriethoxysilane to the reaction solution in a common reaction container, heat to 60°C and react for 3 hours; S4: After the reaction is completed, centrifuge and filter the product, wash it, add it to 120 parts of deionized water, heat it to 60°C, and drop a mixed aqueous solution containing 1.2 parts of ammonia water, 2.8 parts of ethyl orthosilicate and 5.8 parts of titanium dioxide (40 parts in total) for 40 minutes. After the addition is completed, keep the temperature for reaction for 2.4 hours. After completion, centrifuge and wash the product, and vacuum dry it to obtain the product.

[0120] The average particle size of the modified titanium dioxide is 345 nm.

[0121] Comparative Example 5

[0122] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of modified titanium dioxide particles comprises the following steps, calculated by mass: S1: adding 8.85 parts of aluminum nitrate nonahydrate and 28 parts of acetic acid to 150 parts of deionized water and stirring at room temperature, then adding to a sealed reactor and keeping the temperature at 60°C for 1.5 hours; S2: heating to 200°C, controlling the pressure of the reactor to 2.1MPa, adding 3.65 parts of terephthalic acid and continuing stirring for 9.5 hours; S3: after the reaction is completed The reaction solution is taken into a common reaction container, 6.8 parts of succinic anhydride and 0.11 parts of 3-aminopropyltriethoxysilane are added, and the temperature is raised to 60°C for reaction for 3 hours; S4: after the reaction is completed, the product is centrifuged and filtered, washed and added to 120 parts of deionized water, the temperature is raised to 60°C, and a mixed aqueous solution containing 0.8 parts of ammonia water, 1.65 parts of ethyl orthosilicate and 1.4 parts of titanium dioxide (30 parts in total) is added dropwise, the addition time is 40 minutes, and the reaction is kept warm for 2.4 hours after the addition is completed. After completion, the product is centrifuged and washed, and vacuum dried to obtain the product.

[0123] The average particle size of the modified titanium dioxide is 672 nm.

[0124] Comparative Example 6

[0125] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average particle size of titanium dioxide is 50 nm; the average particle size of modified titanium dioxide is 691 nm.

[0126] Comparative Example 7

[0127] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average particle size of titanium dioxide is 5 nm; the average particle size of modified titanium dioxide is 424 nm.

[0128] Comparative Example 8

[0129] The specific implementation of this comparative example is basically the same as that of Example 1, except that the filling powder is sericite powder, the average particle size of the sericite powder is 0.5 μm, and no modified titanium dioxide particles are added.

[0130] Comparative Example 9

[0131] The specific implementation of this comparative example is basically the same as that of Example 1, except that the filling powder is modified titanium dioxide particles, and no sericite powder is added.

[0132] Comparative Example 10

[0133] The specific implementation of this comparative example is basically the same as that of Example 1, except that in the preparation method of modified titanium dioxide particles, the insulation reaction time after the mixed aqueous solution of ethyl orthosilicate and titanium dioxide is added dropwise is 4 hours, and after completion, the product is centrifuged and washed, and vacuum dried to obtain the product.

[0134] The average particle size of titanium dioxide is 20 nm; the average particle size of modified titanium dioxide is 764 nm.

[0135] Comparative Example 11

[0136] The specific implementation of this comparative example is basically the same as that of Example 1, except that in the preparation method of modified titanium dioxide particles, the insulation reaction time after the mixed aqueous solution of ethyl orthosilicate and titanium dioxide is added dropwise is 1.5 hours, and after completion, the product is centrifuged and washed, and vacuum dried to obtain the product.

[0137] The average particle size of titanium dioxide is 20 nm; the average particle size of modified titanium dioxide is 325 nm.

[0138] Performance Evaluation

[0139] Flame retardancy: The flame retardancy of the sealing strip was tested with reference to standard GB 8624-2012, and the results are recorded in Table 1.

[0140] Waterproofness: The water vapor permeability of the sealing strip was tested with reference to the standard ISO 15106-2:2019. The test value was the average of 10 tests and recorded in Table 1.

[0141] Aging resistance: The sealing strips prepared in the examples and comparative examples were placed in a constant temperature and humidity chamber at 60°C and 85% relative humidity for 21 weeks. After 21 weeks, the sealing strips were observed to see if they had obvious yellowing, warping, and adhesion. If so, they were considered unqualified, otherwise, they were qualified. 50 samples were tested in each group, and the qualified rate was recorded in Table 1.

[0142]

[0143] It can be seen from the examples and comparative examples of the present application and the data results in Table 1 that, compared with comparative examples 1 to 11, examples 1 and 2 of the present application can maintain better waterproofness, aging resistance and corrosion resistance while ensuring excellent flame retardancy, which is mainly due to the addition of modified fillers and the selection of specific rubber compositions in the present application; and comparative examples 1 to 11 have obvious gaps in the above-mentioned performances because they do not adopt the correct limiting technical scheme, which further proves the necessity of the limiting technical scheme in the present application for the technical effect.

Claims

1. A composite fireproof sealing strip, Features: Composite fireproof sealing strip, calculated by weight, the raw materials include: 60-80 parts of base rubber, 30-45 parts of filling powder, 3-6 parts of cross-linking agent, 4-8 parts of dispersant, 0.5-3 parts of vulcanization accelerator, 3-5 parts of lubricant, 15-25 parts of oil agent, 1-15 parts of auxiliary agent; The base rubber is a composition of EPDM, chloroprene rubber and fluorine-containing resin; The mass ratio of the EPDM rubber, chloroprene rubber and fluorine-containing resin is (6-8): (2-3): (1-1.8); The Mooney viscosity of the EPDM rubber is 65~80MU, ML 1+4 125℃; The filler powder is a composition of sericite powder and modified titanium dioxide particles; the mass ratio of the sericite powder to the modified titanium dioxide particles is (4-4.5): (1-1.5); The average particle size of the sericite powder is 0.4-1 μm; The preparation method of the modified titanium dioxide particles comprises the following steps: S1: Add aluminum nitrate nonahydrate and acetic acid to deionized water and stir evenly at room temperature, then add to a closed reactor, and keep warm at 50-65°C for 1-2 hours; S2: Heat to 190-210°C, control the pressure of the reactor to 1.9-2.1MPa, add terephthalic acid and continue stirring for 8-10 hours; S3: After the reaction is completed, take the reaction solution to a common reaction container, add succinic anhydride and 3-aminopropyltriethoxysilane, heat to 60-65°C for 2-3 hours; S4: After the reaction is completed, centrifuge and filter the product, wash it, add it to deionized water, heat to 55-60°C, and drop a mixed solution containing ammonia water, tetraethyl orthosilicate and titanium dioxide, wherein the average particle size of the titanium dioxide is 15-30nm, and the dropping time is 20-40min. After the dropping is completed, keep warm for 2.2-2.8 hours, and after completion, centrifuge and wash the product, and vacuum dry it to obtain the product; The mass ratio of aluminum nitrate nonahydrate, acetic acid, terephthalic acid and titanium dioxide is (4-5): (15-20): (2-2.5): (3-4); the average particle size of the modified titanium dioxide is 480-600 nm; The fluorine-containing resin is an ethylene-tetrafluoroethylene copolymer resin, and the melt flow rate of the ethylene-tetrafluoroethylene copolymer resin is 5-12 g / 10 min, 300° C. / 1.2 kg.

2. The composite fireproof sealing strip according to claim 1, Features: The mass ratio of the base rubber, the filling powder and the oil agent is (6.5-7.5): (3.2-4): (2-2.4).

3. The composite fireproof sealing strip according to claim 2, Features: The cross-linking agent is at least one of dibenzoyl peroxide, dicumyl peroxide, zinc oxide and magnesium oxide.

4. The composite fireproof sealing strip according to claim 3, Features: The dispersant is at least one of zinc stearate, sodium dodecyl sulfate, sodium lauryl sulfate, triethylhexyl phosphate, methyl amyl alcohol, sodium tripolyphosphate, sodium hexametaphosphate, and carboxymethyl cellulose.

5. The composite fireproof sealing strip according to claim 4, Features: The dispersant is a composition of zinc stearate and sodium lauryl sulfate; the mass ratio of the zinc stearate to sodium lauryl sulfate is (2-4): (0.4-0.6).

6. A process for preparing the composite fireproof sealing strip according to any one of claims 1 to 5, Features: The preparation process comprises the following steps: D1: Put the base rubber into the internal mixer, adjust the temperature to 60~80℃ and mix for 4~5min; D2: Add the remaining raw materials and mix at 65-75℃ for 2-3min; D3: After the mixing is completed, the obtained rubber material is taken out and stretched into a strip-shaped colloid, and the strip-shaped colloid is placed in an extruder and extruded through a mold to obtain a molded rubber strip; D4: Put the molded rubber strip into a salt bath and vulcanize it, then clean it.

7. Application of the composite fireproof sealing strip as claimed in any one of claims 1 to 5 in the field of door and window sealing.

Citation Information

Patent Citations

  • High-performance ethylene propylene rubber sealing gasket and preparation method and application thereof

    CN111548570A

  • Modified PET base material for solar cell backboard and preparation method of modified PET base material

    CN112745645A

  • Cabin door movable window sealing structure and application thereof

    CN113733878A

  • High-temperature heat-resistant flexible flame-retardant modified power cable based on fluoropolymer shell coating and preparation method thereof

    CN118155923A

  • Rubber composite, processing method, sealing element applying composite, and manufacturing method

    WO2018130186A1