A preparation method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingots

CN118563146BActive Publication Date: 2024-11-26XIAN WESTERN ENERGY MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410531672.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-11-26
Estimated Expiration
2044-04-29

AI Technical Summary

Technical Problem

During vacuum consumable smelting, the Cr elements in the zirconium alloy ingot are easily volatile, resulting in uneven chemical composition, especially the content of the element at the head of the ingot is relatively low, which affects the yield and performance.

Method used

By adjusting the batching method and smelting times of Cr raw materials in the electrode block, increasing the number of smelting times and adding Cr raw materials to the head of the ingot before the last smelting, combined with the shrinkage process, the smelting parameters such as vacuum degree, voltage rise rate, and smelting current are controlled. and voltage to ensure uniform distribution of Cr elements.

Benefits of technology

It effectively improves the uniformity of Cr elements in zirconium alloy ingots, reduces the amount of ingot head cut, improves the yield rate, simplifies production processes and reduces costs, and meets the nuclear industry's demand for high-quality materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563146B_ABST
    Figure CN118563146B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation of non-ferrous alloy materials, and relates to a preparation method for improving the uniformity of Cr elements in nuclear-grade zirconium alloy ingots. The preparation method comprises the following steps: 1. preparing alloy raw materials and performing intermediate alloy batching; 2. mixing the added raw materials with zirconium sponge and pressing them into the required electrode blocks; 3. welding the electrode blocks to obtain consumable electrodes for smelting; 4. performing multiple vacuum consumable smelting on the electrodes according to the designed smelting process parameters, and adding Cr raw materials before smelting the finished product; 5. performing flaw detection and machining on the ingot after the final smelting to obtain the finished ingot. The present invention firstly adjusts the batching target values ​​of different electrode blocks, and secondly adds Cr raw materials to the upper end surface of the ingot to compensate for the volatilization of Cr elements in the ingot head during the smelting process; at the same time, strictly controls the number of smelting times and parameters, reduces the volatilization loss of Cr elements, ensures the high uniformity of chemical composition, and thus greatly reduces the amount of ingot head resection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of nonferrous alloy materials, relates to zirconium alloys, and specifically relates to a preparation method for improving the uniformity of Cr elements in nuclear-grade zirconium alloy ingots. Background Art

[0002] Zirconium and zirconium alloys are widely used in the nuclear industry, chemical industry and other fields due to their good corrosion resistance and mechanical properties. Especially as key materials for nuclear power or nuclear power, their quality requirements are extremely high, and good ingots are the basis for subsequent processing of high-performance zirconium alloy materials. In particular, the chemical composition of the ingot has a great influence on the corrosion resistance, mechanical and other key properties of zirconium alloy materials. This requires the use of scientific and reasonable preparation processes in the process of preparing ingots, so as to prepare zirconium alloy ingots with high uniformity of chemical composition.

[0003] At present, the industry generally adopts the method of vacuum consumable melting to prepare zirconium or zirconium alloy ingots. The Cr element is beneficial to the improvement of the corrosion resistance and other properties of zirconium alloys. Therefore, many brands of zirconium alloys at home and abroad have added Cr, such as the classic brand Zr-4 alloy, Zr-2 alloy and the new brand X5A alloy. Due to the high saturated vapor pressure of elements such as Cr and Mn, they are very easy to volatilize during vacuum consumable melting, resulting in uneven chemical composition in the ingot, especially the head of the ingot, where the element content is significantly low, resulting in the need to increase the amount of resection of the ingot head to ensure the uniformity of the chemical composition of the entire ingot, which significantly reduces the yield of the ingot. In order to solve this problem, the industry generally adopts the process of preparing an alloy containing Cr or Mn through alloy weighing, alloy bag preparation, alloy bean pressing, alloy buckle smelting and other processes, and adding it in the form of an intermediate alloy. This not only increases the processing steps, reduces efficiency, and increases costs, but also has limited effect on improving the uniformity of the chemical composition and yield of the ingot, and the effect is not obvious. Therefore, how to solve the uniformity of volatile elements in zirconium alloy ingots efficiently and with high quality has become a key technical problem that needs to be solved urgently.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to overcome the disadvantages of the prior art and provide a preparation method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingots.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] On the one hand, the present invention provides a preparation method for improving the uniformity of Cr element in nuclear-grade zirconium alloy ingots, by adjusting the batching method, electrode block pressing method, smelting times and smelting process, so as to improve the uniformity of chemical composition and structure in nuclear-grade zirconium alloy ingots; wherein,

[0008] The consumable electrode for smelting the nuclear-grade zirconium alloy ingot is formed by welding a plurality of electrode blocks in sequence, and the addition amount Y of Cr raw material in the electrode block located at at least one end of the consumable electrode is 1.02 to 1.15 times the addition amount X of Cr raw material in the remaining electrode blocks, so as to compensate for the volatilization of Cr element at the head of the nuclear-grade zirconium alloy ingot during vacuum consumable smelting.

[0009] Specifically, the smelting times are 2 to 4 times.

[0010] Furthermore, when the number of smelting times is greater than 2 times, before the last smelting, Cr raw materials are further added to the upper end surface of the ingot charged with the furnace to compensate for the volatilization of the Cr element during the last smelting, and the chemical uniformity of the head of the nuclear-grade zirconium alloy ingot is guaranteed in combination with the final shrinkage feeding process. Among them, the shrinkage is fed by step-by-step current reduction and a specific holding time to reduce the shrinkage cavity depth and improve the uniformity of the Cr element, thereby improving the yield rate.

[0011] Specifically, when the number of smelting times is greater than 2 times, before the last smelting, the specific method of further adding Cr raw material to the upper end surface of the ingot charged into the furnace is as follows:

[0012] On the upper end surface of the charged ingot, a first hole with a depth of h1 is drilled along the center of the upper end surface, and a circle is determined with the center of the upper end surface as the center and a radius of 0.4R~0.75R, and a plurality of second holes with a depth of h2 are drilled along the circumferential direction of the circle, and the first hole and the second hole are both used to add Cr raw material; wherein R is the radius of the charged ingot, and after the Cr raw material is added, the corresponding holes are welded and sealed with zirconium alloy material of the same grade.

[0013] Specifically, the depths of the first hole and the second hole are both 0.25R to 0.75R.

[0014] Specifically, a line connecting two adjacent second holes and the first hole forms an angle α, and the angle α is 60° to 180°.

[0015] Specifically, the Cr raw material added to the first hole and the second hole is in the form of particles or crumbs, and the total amount added is 0.43πR 3 X×10 -3 g~1.3πR 3 X×10 -3 g; wherein the amount of Cr raw material added in each hole is close, preferably, the amount of Cr raw material added in each hole is the same.

[0016] Specifically, the batching method is as follows:

[0017] The sponge zirconium in the nuclear-grade zirconium alloy ingot is nuclear-grade sponge zirconium, and the Cr raw material is chromide or chromium-containing alloy or pure chromium metal.

[0018] Specifically, the electrode block pressing method is as follows:

[0019] First, a layer of zirconium sponge is laid, and then the added raw materials are evenly arranged on the surface of the first layer of zirconium sponge. Finally, another layer of zirconium sponge is laid on the raw materials, and the two layers of zirconium sponge are used in the same amount; then, the required electrode blocks are pressed, and the number of the electrode blocks is determined according to the feed amount.

[0020] Specifically, the smelting process is as follows:

[0021] The crucible diameter for vacuum consumable melting is 450mm to 750mm, and the ingot is turned around after each melting for the next melting.

[0022] During smelting: the first smelting is controlled by current, the subsequent smelting is controlled by melting rate, and the last smelting is carried out at the head of the ingot to ensure the chemical uniformity of the head of the nuclear-grade zirconium alloy ingot;

[0023] During the smelting process: the ingot is flattened and surface cleaned after each smelting;

[0024] After the final smelting is completed: the ingot after the final smelting is subjected to flaw detection and machining to obtain a finished nuclear-grade zirconium alloy ingot that meets the requirements;

[0025] Among them, the smelting process parameters are: vacuum degree less than 1.5Pa, pressure rise rate less than 1.5Pa / min, smelting voltage of 28V~45V, smelting speed of 10kg / min~45kg / min, smelting current of 8kA~36kA, and cooling time after smelting is not less than 4h.

[0026] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0027] 1) The present invention reasonably designs the target values ​​of raw material ingredients in different electrode blocks, and increases the addition amount Y (target value) of Cr raw material in the end electrode block to a reasonable range to offset the volatilization of Cr element in the ingot head during the smelting process; in addition, when the number of smelting times is greater than 2 times, before the last smelting, Cr raw material is further added to the upper end surface of the ingot charged into the furnace to compensate for the volatilization of Cr element during the final smelting, and combined with the final shrinkage feeding process, the chemical composition uniformity of the head of the nuclear-grade zirconium alloy ingot is guaranteed, which solves the problem that the prior art cannot effectively improve the uniformity of the chemical composition of the ingot, especially the problem that the Cr element in the ingot head is seriously low and uneven, thereby reducing the amount of resection of the ingot head and greatly improving the ingot yield.

[0028] 2) The present invention further ensures the uniformity of chemical composition in the nuclear-grade zirconium alloy ingot obtained by smelting by limiting the number of smelting times, controlling the smelting turning and feeding processes, and strictly controlling the smelting process parameters including vacuum degree, pressure rise rate, smelting current, smelting voltage, cooling time, etc.

[0029] 3) The addition of Cr raw materials in the present invention no longer requires the preparation of intermediate alloys through processes such as alloy weighing, alloy bag preparation, alloy bean pressing, and alloy button smelting, and is not limited by the addition method. That is, the Cr raw materials in the raw materials are added directly in the form of chromide, chromium-containing alloy, or pure chromium metal, etc., which has great flexibility and adjustment space, simplifies the production process, reduces production costs, and improves preparation efficiency.

[0030] 4) The present invention can produce nuclear-grade zirconium alloy ingots with high uniformity of chemical composition, and its chemical composition is far better than the index requirements, which not only meets the high demands of the nuclear industry, but also significantly improves the utilization rate of raw materials and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0033] Figure 1 A flow chart of a preparation method for improving the uniformity of Cr element in a nuclear-grade zirconium alloy ingot provided by the present invention;

[0034] Figure 2 A schematic diagram of the installation for melting two primary ingots provided in Example 1 of the present invention;

[0035] Figure 3 Schematic diagram of the zirconium alloy ingot and its drilling provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention described in detail in the appended claims.

[0037] See also Figure 1As shown, the present invention provides a flow chart of a preparation method for improving the uniformity of Cr element in nuclear-grade zirconium alloy ingots, comprising the following steps: step one, preparing alloy raw materials and performing intermediate alloy batching; step two, mixing the added raw materials with zirconium sponge, and pressing them into required electrode blocks; step three, welding the electrode blocks to obtain consumable electrodes for smelting; step four, performing vacuum consumable smelting on the electrodes 2 to 4 times according to the designed smelting process parameters, and adding Cr raw materials before smelting the finished product; step five, performing flaw detection and machining on the ingot after the final smelting to obtain a finished ingot.

[0038] Here, for the convenience of the following description, the total amount of added materials is defined as the sum of the weight of the added raw materials and the weight of the zirconium sponge. The meaning of the total amount of added materials described below is the same as that defined here.

[0039] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0040] Example 1

[0041] This embodiment provides a preparation method for improving the uniformity of Cr element in a nuclear-grade zirconium alloy ingot. The nuclear-grade zirconium alloy ingot is a Zr-Sn-Fe-Cr alloy, and the smelting times are 4 times. The preparation method specifically comprises the following steps:

[0042] Step 1, batching: the raw materials added are pure metal tin particles / tin foil, iron filings, and chromium particles, wherein the batching target value of the Cr raw material is 0.13%, that is, the addition amount of the Cr raw material accounts for 0.13% (weight percentage) of the total added material amount, and each added raw material is weighed according to the batching calculation amount (calculated according to the weight ratio required by the Zr-Sn-Fe-Cr alloy grade), and is divided into several portions according to the number of electrode blocks;

[0043] Step 2, electrode block pressing: according to the result of the batching calculation, weigh the corresponding amount of nuclear-grade sponge zirconium; when pressing, first pour the first portion of sponge zirconium into the mold, then evenly arrange the mixed Sn, Fe, and Cr additive raw materials weighed in step 1 on the surface of the sponge zirconium, and then pour the second portion of sponge zirconium with the same mass as the first portion into the mold, and finally press it into a cylindrical electrode block with a diameter of Ф360mm; and press several electrode blocks in this way, wherein the batching target value Y of the Cr raw material of 2 electrode blocks is 0.1495%, and the batching target value X of the Cr raw material of the remaining electrode blocks is 0.13%, that is, Y=1.15X;

[0044] Step 3, welding consumable electrodes: using a vacuum plasma welding box to weld the electrode blocks pressed in step 2 to form two consumable electrodes with a diameter of 360×L0 (mm) for smelting; wherein, an electrode block with a high amount of Cr raw material added is welded to one end of one consumable electrode A1, and another electrode block with a high amount of Cr raw material added is welded to one end of another consumable electrode A2;

[0045] Step 4: Obtain 2 primary ingots through the first smelting:

[0046] The consumable electrode A1 obtained in step 3 is placed in a melting crucible with a diameter of 450 mm, wherein the end with a higher amount of Cr raw material added is placed at the upper part, and then evacuated. When the vacuum degree is 1.2 Pa, a leak test is performed, and the pressure rise rate is 1.0 Pa / min. After the leak test passes, the upper part of the consumable electrode A1 is welded to the auxiliary electrode. After the welding is completed, vacuum consumable melting is performed, and the melting voltage is 28 V and the melting current is 8 kA. After the melting is completed, the furnace is stopped and filled with argon and cooled for 4 hours before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, to obtain the first primary ingot of 450×L1 (mm);

[0047] The consumable electrode A2 obtained in step 3 is melted in the same manner, and the crucible specifications and the consumable electrode placement method are the same as those when the consumable electrode A1 is melted; when the vacuum degree is 1.3Pa, a leak test is performed, and the pressure rise rate is 1.1Pa / min. After the leak test passes, the upper part of the consumable electrode A2 is welded to the auxiliary electrode, and after the welding is completed, vacuum consumable melting is performed, the melting voltage is 28V, and the melting current is 8kA. After the melting is completed, the furnace is stopped and filled with argon and cooled for 4h before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, and finally a second primary ingot of Ф450×L1(mm) is obtained;

[0048] Step 5: Combine Figure 2 As shown, two primary ingots are melted for the second time to obtain secondary ingots:

[0049] The two primary ingots obtained in step 4 (referred to as 1# ingot and 2# ingot) are placed vertically in a smelting crucible with a diameter of 550 mm (the two primary ingots are placed up and down). The primary ingot needs to be turned when placed, that is, the head of the primary ingot is facing downward and placed in the lower part of the furnace chamber, and then evacuated. When the vacuum degree is 1.0 Pa, leak detection is performed, and the pressure rise rate is 1.0 Pa / min. After the leak detection passes, the primary ingot head welding (that is, the tail of the 2# ingot is welded with the auxiliary electrode) and the middle welding (that is, the tail of the 1# ingot is welded with the head of the 2# ingot), and after welding, vacuum consumable smelting is performed, the smelting voltage is 37 V, the smelting speed is 21 kg / min, and the smelting current is 17 kA. After the smelting is completed, the furnace is stopped and argon is filled and cooled for 5 hours before being taken out of the furnace, and a machine flattening process is performed without peeling process, and the surface is cleaned to remove impurities such as surface volatiles, to obtain a secondary ingot of 550×L2 (mm);

[0050] Step 6: Smelt the secondary ingot for the third time to obtain the tertiary ingot:

[0051] The secondary ingot obtained in step 5 is placed in a melting crucible with a diameter of 650 mm. The secondary ingot needs to be turned around when placed, that is, the head of the secondary ingot is facing downward and placed in the lower part of the furnace chamber, and then evacuated. When the vacuum degree is 0.8 Pa, leak detection is performed, and the pressure rise rate is 0.7 Pa / min. After the leak detection passes, the secondary ingot head is welded (that is, the tail of the secondary ingot is welded to the auxiliary electrode). After welding, vacuum consumable melting is performed, the melting voltage is 43 V, the melting speed is 36 kg / min, and the melting current is 30 kA. After the melting is completed, the furnace is stopped and argon is filled and cooled for 6 hours before being taken out of the furnace, and a machine flat head treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles to obtain a tertiary ingot of 650 × L3 (mm);

[0052] Step 7: Before the fourth smelting of the tertiary ingot, add Cr raw material to the upper end surface of the tertiary ingot:

[0053] Combination Figure 3 As shown, the tertiary ingot obtained in step 6 is turned around, that is, the lower end face of the tertiary ingot is placed on the upper side, and the lower end face is drilled, and holes are drilled at six positions (at an angle of 60° to each other) at the center of the lower end face of the tertiary ingot and at a radius of about 244 mm (i.e., 0.75R), respectively. The depth of the seven holes is about 244 mm (i.e., 0.75R), and fine Cr particles are placed therein. The amount of Cr added to each hole is 26 g, and then the same grade of zirconium alloy round bars are used for welding and plugging the holes;

[0054] Step 8: Smelt the tertiary ingot to obtain the quaternary ingot:

[0055] The drilled end of the tertiary ingot obtained in step 7 is facing upwards, and is placed in a melting crucible with a diameter of 750 mm, and then evacuated. When the vacuum degree is 1.3 Pa, a leak test is performed, and the pressure rise rate is 1.1 Pa / min. After the leak test passes, the tertiary ingot head is welded (that is, the drilled end of the tertiary ingot is welded to the auxiliary electrode). After welding, vacuum consumable melting is performed, and the melting voltage is 45 V, the melting speed is 45 kg / min, and the melting current is 36 kA. After the melting is completed, the furnace is stopped and filled with argon for cooling for 8 hours, and then taken out of the furnace to obtain a 750×L4 (mm) quaternary ingot;

[0056] Step 9: Perform flaw detection and machining on the four ingots to obtain finished ingots:

[0057] The cylindrical surface of the quaternary ingot obtained in step 8 is peeled to remove surface defects such as pores, oxides, inclusions, etc., and the head and tail are sawed off after flaw detection to make the surface of the ingot present the original color of the metal, thereby obtaining a finished ingot; samples are taken at 1 / 2R of the head end face of the ingot and at four positions at the upper, middle and lower sides of the cylindrical side. The samples are qualified after chemical composition inspection and meet the technical index requirements of the target product zirconium alloy ingot and the chemical components are evenly distributed. The Cr element detection results at each position are shown in Table 1.

[0058] Example 2

[0059] This embodiment provides a preparation method for improving the uniformity of Cr element in a nuclear-grade zirconium alloy ingot. The nuclear-grade zirconium alloy ingot is a Zr-Sn-Fe-Cr-Ni alloy, and the smelting times are 3 times. The preparation method specifically comprises the following steps:

[0060] Step 1, batching: the raw materials added are pure metal tin particles / tin foil, iron filings, chromium carbide particles, and nickel particles, wherein the batching target value of the Cr raw material is 0.15%, that is, the addition amount of the Cr raw material accounts for 0.15% (weight percentage) of the total added material amount, and each added raw material is weighed according to the batching calculation amount (calculated according to the weight ratio required by the Zr-Sn-Fe-Cr-Ni alloy grade), and is divided into several portions according to the number of electrode blocks;

[0061] Step 2, electrode block pressing: according to the result of the batching calculation, weigh the corresponding amount of nuclear-grade sponge zirconium. When pressing, first pour the first portion of sponge zirconium into the mold, then evenly arrange the mixed Sn, Fe, and Cr additive raw materials weighed in step 1 on the surface of the sponge zirconium, and then pour the second portion of sponge zirconium with the same mass as the first portion into the mold, and finally press it into a cylindrical electrode block of Ф360mm; and press several electrode blocks in this way, wherein the batching target value Y of the Cr raw materials of 2 electrode blocks is 0.153%, and the batching target value X of the Cr raw materials of the remaining electrode blocks is 0.15%, that is, Y=1.02X;

[0062] Step 3, welding consumable electrodes: using argon arc welding outside the furnace to weld the electrode blocks pressed in step 2 to form two consumable electrodes with a diameter of 360×L0 (mm) for melting; wherein an electrode block with a high amount of Cr raw material added is welded to one end of one consumable electrode B1, and another electrode block with a high amount of Cr raw material added is welded to one end of another consumable electrode B2;

[0063] Step 4: Obtain 2 primary ingots through the first smelting:

[0064] The consumable electrode B1 obtained in step 3 is placed in a melting crucible with a diameter of 450 mm, wherein the higher end of the Cr raw material is placed at the upper part, and then evacuated. When the vacuum degree is 1.4 Pa, a leak test is performed, and the pressure rise rate is 1.3 Pa / min. After the leak test passes, the upper part of the consumable electrode B1 is welded to the auxiliary electrode. After the welding is completed, vacuum consumable melting is performed, and the melting voltage is 32 V and the melting current is 14 kA. After the melting is completed, the furnace is stopped and filled with argon and cooled for 5 hours before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, so as to obtain the first primary ingot of 450×L1 (mm);

[0065] The consumable electrode B2 obtained in step 3 is melted in the same manner, and the crucible specifications and electrode placement method are the same as those of the first melting. When the vacuum degree is 1.1Pa, a leak test is performed, and the pressure rise rate is 1.0Pa / min. After the leak test passes, the upper part of the consumable electrode B2 is welded to the auxiliary electrode. After the welding is completed, vacuum consumable melting is performed, and the melting voltage is 32V and the melting current is 14kA. After the melting is completed, the furnace is stopped and filled with argon and cooled for 5h before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, to obtain a second primary ingot of Ф450×L2(mm);

[0066] Step 5: Smelt the two primary ingots for the second time to obtain secondary ingots. The installation principle of the two primary ingots is the same as Figure 2 The same, no further description is given here, the specific smelting process is:

[0067] The two primary ingots obtained in step 4 are placed vertically in a smelting crucible with a diameter of Ф550mm (two primary ingots are placed up and down). When the primary ingot is placed, it is necessary to turn around, that is, the head of the primary ingot is facing down and placed in the lower part of the furnace chamber, and then evacuate. When the vacuum degree is 0.8Pa, leak detection is performed, and the pressure rise rate is 0.9Pa / min. After the leak detection passes, the head welding of the primary ingot (i.e., the tail of the previous ingot is welded with the auxiliary electrode) and the middle welding (i.e., the tail of the next ingot is welded with the head of the previous ingot), and after welding, vacuum consumable melting is performed, the melting voltage is 38V, the melting speed is 24kg / min, and the melting current is 20kA. After the melting is completed, the furnace is stopped and argon is filled and cooled for 6h before being taken out of the furnace, and a machine flat head treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, to obtain a secondary ingot of Ф550×L2(mm);

[0068] Step 6: Before the third smelting of the secondary ingot, add Cr raw material to the upper end surface of the secondary ingot:

[0069] The secondary ingot obtained in step 5 is turned around, that is, the lower end face of the secondary ingot is placed on the upper side, and the lower end face is drilled, and holes are drilled at four positions (at 90° to each other) at the center of the ingot end face and at a radius of about 137 mm (i.e. 0.5R), respectively, and the depth of the five holes is 69 mm (i.e. 0.25R), and fine Cr chips are placed therein, and the amount of Cr added to each hole is 8.4 g, and then the same grade of zirconium alloy chips are used to weld and seal the holes;

[0070] Step 7: Smelt the secondary ingot for the third time to obtain the tertiary ingot:

[0071] The drilled end of the secondary ingot obtained in step 6 is facing upwards, and is placed in a melting crucible with a diameter of 650 mm, and then evacuated. When the vacuum degree is 0.6 Pa, a leak test is performed, and the pressure rise rate is 0.6 Pa / min. After the leak test passes, the secondary ingot head is welded (that is, the drilled end of the secondary ingot is welded to the auxiliary electrode). After welding, vacuum consumable melting is performed, and the melting voltage is 42 V, the melting speed is 30 kg / min, and the melting current is 29 kA. After the melting is completed, the furnace is stopped and filled with argon for cooling for 7 hours, and then taken out of the furnace to obtain a tertiary ingot of 650×L3 (mm);

[0072] Step 8: Perform flaw detection and machining on the three ingots to obtain finished ingots:

[0073] The cylindrical surface of the tertiary ingot obtained in step 7 is peeled to remove surface defects such as pores, oxides, inclusions, etc., and the head and tail are sawed off after flaw detection to make the surface of the ingot present the original color of the metal to obtain a finished ingot. Samples are taken at 1 / 2R of the head end face of the ingot and at four positions on the upper, middle and lower sides of the cylindrical side. The chemical composition test is qualified and all meet the technical index requirements of the target product zirconium alloy ingot and the chemical components are evenly distributed. The Cr element detection results at each position are shown in Table 1.

[0074] Example 3

[0075] This embodiment provides a preparation method for improving the uniformity of Cr element in a nuclear-grade zirconium alloy ingot. The nuclear-grade zirconium alloy ingot is a Zr-Sn-Fe-Cr alloy, and the smelting times are 2 times. The preparation method specifically comprises the following steps:

[0076] Step 1, batching: the added raw materials are Zr-Sn-Fe-Cr master alloy particles prepared by smelting in advance, wherein the batching target value of the Cr raw material is 0.13%, that is, the addition amount of the Cr raw material accounts for 0.13% (weight percentage) of the total added feed amount, and each added raw material is weighed according to the batching calculation amount (calculated according to the weight ratio required by the Zr-Sn-Fe-Cr alloy grade), and is divided into several portions according to the number of electrode blocks;

[0077] Step 2, electrode block pressing: according to the result of the batching calculation, weigh the corresponding amount of nuclear-grade sponge zirconium; when pressing, first pour a portion of sponge zirconium into the mold, then evenly arrange the mixed Zr-Sn-Fe-Cr master alloy additive raw material weighed in step 1 on the surface of the sponge zirconium, and then pour a second portion of sponge zirconium with the same mass as the first portion into the mold, and finally press it into a semicircular electrode block of Ф450mm, and press several electrode blocks in this way; among them, the batching target value Y of the Cr raw material of 4 electrode blocks is 0.143%, and the batching target value X of the Cr raw material of the remaining electrode blocks is 0.13%, that is, Y=1.1X;

[0078] Step 3: Welding the consumable electrode: Use a vacuum plasma welding box to weld the electrode block pressed in step 2.

[0079] First, four semicircular electrode blocks with high Cr raw material addition were welded in pairs to form full-circle electrode blocks, and then the remaining electrode blocks were welded in pairs to form full-circle electrode blocks. Finally, two full-circle electrode blocks with high Cr raw material addition were placed at both ends, and the remaining circular electrode blocks were placed randomly, and welded in sequence to obtain a 450×L0 (mm) consumable electrode for smelting.

[0080] Step 4: Obtain one primary ingot through the first smelting:

[0081] The consumable electrode obtained in step 3 is placed in a melting crucible with a diameter of 550 mm, wherein any end of the Cr raw material with a higher height is placed on the upper part, and then evacuated. When the vacuum degree is 1.3 Pa, a leak test is performed, and the pressure rise rate is 1.2 Pa / min. After the leak test passes, the consumable electrode head is welded (that is, any end of the Cr raw material with a higher height is welded to the auxiliary electrode). After the welding is completed, vacuum consumable melting is performed, and the melting voltage is 35 V, and the melting current is 19 kA. After the melting is completed, the furnace is stopped and argon is filled and cooled for 5 hours before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, and finally a primary ingot of 550×L1 (mm) is obtained;

[0082] Step 5: Smelt the primary ingot for the second time to obtain the secondary ingot:

[0083] The primary ingot obtained in step 4 is placed in a melting crucible with a diameter of 650 mm. The primary ingot needs to be turned around when placed, that is, the tail of the primary ingot is facing upwards, and placed in the upper part of the furnace chamber, and then evacuated. When the vacuum degree is 0.7 Pa, a leak test is performed, and the pressure rise rate is 0.6 Pa / min. After the leak test passes, the head of the primary ingot (i.e., the tail facing upwards) is welded. After the welding is completed, vacuum consumable melting is performed, the melting voltage is 40 V, the melting speed is 30 kg / min, and the melting current is 27 kA. After the melting is completed, the furnace is stopped and argon is filled and cooled for 6 hours before being taken out of the furnace to obtain a secondary ingot of 650×L2 (mm);

[0084] Step 6: Perform flaw detection and machining on the secondary ingot to obtain the finished ingot:

[0085] The cylindrical surface of the secondary ingot obtained in step 5 is peeled to remove surface defects such as pores, oxides, inclusions, etc., and the head and tail are sawed off after flaw detection to make the surface of the ingot present the original color of the metal to obtain a finished ingot. Samples are taken at 1 / 2R of the head end face of the ingot and at four positions on the upper, middle and lower sides of the cylindrical side. The chemical composition test is qualified and all meet the technical index requirements of the target product zirconium alloy ingot and the chemical components are evenly distributed. The Cr element detection results at each position are shown in Table 1.

[0086] Example 4

[0087] This embodiment provides a preparation method for improving the uniformity of Cr element in a nuclear-grade zirconium alloy ingot. The nuclear-grade zirconium alloy ingot is a Zr-Sn-Nb-Fe-Cr alloy, and the smelting times are 3 times. The preparation method specifically includes the following steps:

[0088] Step 1, batching: the raw materials added are pure metal tin particles / tin foil, iron filings, chromium particles, and Zr-40Nb filings, wherein the batching target value of the Cr raw material is 0.25%, that is, the addition amount of the Cr raw material accounts for 0.25% (weight percentage) of the total added material amount, and each added raw material is weighed according to the batching calculation amount (calculated according to the weight ratio required by the Zr-Sn-Fe-Cr alloy grade), and is divided into several portions according to the number of electrode blocks;

[0089] Step 2, electrode block pressing: according to the result of the batching calculation, weigh the corresponding amount of nuclear-grade sponge zirconium; when pressing, first pour a portion of sponge zirconium into the mold, then evenly arrange the weighed and mixed Sn, Fe, Cr, and Nb additive raw materials in step 1 on the surface of the sponge zirconium, and then pour a second portion of sponge zirconium with the same mass as the first portion into the mold, and finally press it into a semicircular electrode block of Φ360mm. In this way, several electrode blocks are pressed, among which the batching target value Y of the Cr raw material of 4 electrode blocks is 0.27%, and the batching target value X of the Cr raw material of the remaining electrode blocks is 0.25%, that is, Y=1.08X;

[0090] Step 3, welding the consumable electrodes, using a vacuum plasma welding box to weld the electrode blocks pressed in step 2, specifically: first, four semicircular electrode blocks with high Cr raw material addition are welded in pairs to form full-circle electrode blocks, and then the remaining electrode blocks are welded in pairs to form full-circle electrode blocks, and finally, a full-circle electrode block with high Cr raw material addition is welded to one end of a consumable electrode C1, and another electrode block with high Cr raw material addition is welded to one end of another consumable electrode C2, and the remaining electrode blocks are randomly placed and welded in sequence to form two consumable electrodes with a diameter of 360×L0 (mm) for smelting;

[0091] Step 4: Obtain 2 primary ingots through the first smelting:

[0092] The consumable electrode C1 obtained in step 3 is placed in a melting crucible with a diameter of 450 mm, wherein the higher end of the Cr raw material is placed on the upper part, and then evacuated. When the vacuum degree is 1.5 Pa, a leak test is performed, and the pressure rise rate is 1.4 Pa / min. After the leak test passes, the upper part of the consumable electrode C1 is welded to the auxiliary electrode. After the welding is completed, vacuum consumable melting is performed, the melting voltage is 30 V, and the melting current is 12 kA. After the melting is completed, the furnace is stopped and filled with argon and cooled for 4 hours before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, so as to obtain the first primary ingot of 450×L1 (mm);

[0093] The consumable electrode C2 obtained in step 3 is melted in the same manner, and the crucible specifications and electrode placement method are the same as those of the first melting. When the vacuum degree is 1.5Pa, a leak test is performed, and the pressure rise rate is 1.4Pa / min. After the leak test passes, the upper part of the consumable electrode C2 is welded to the auxiliary electrode. After the welding is completed, vacuum consumable melting is performed, the melting voltage is 30V, and the melting current is 12kA. After the melting is completed, the furnace is stopped and argon is filled and cooled for 4h before being taken out of the furnace, and a machine flattening treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, to obtain a second primary ingot of Ф450×L1(mm);

[0094] Step 5: Smelt the two primary ingots for the second time to obtain secondary ingots. The installation principle of the two primary ingots is the same as Figure 2 The same, no further description is given here, the specific smelting process is:

[0095] The two primary ingots obtained in step 4 are placed vertically in a smelting crucible with a diameter of 550 mm (two primary ingots are placed up and down). When the primary ingot is placed, it is necessary to turn around, that is, the head of the primary ingot is facing down and placed in the lower part of the furnace chamber, and then evacuate. When the vacuum degree is 0.9 Pa, leak detection is performed, and the pressure rise rate is 0.8 Pa / min. After the leak detection passes, the head of the primary ingot (i.e., the tail of the previous ingot is welded with the auxiliary electrode) and the middle welding (i.e., the tail of the next ingot is welded with the head of the previous ingot), and after welding, vacuum consumable melting is performed, the melting voltage is 35 V, the melting speed is 22 kg / min, and the melting current is 20 kA. After the melting is completed, the furnace is stopped and argon is filled and cooled for 5 hours before being taken out of the furnace, and a machine flat head treatment is performed without peeling treatment, and the surface is cleaned to remove impurities such as surface volatiles, to obtain a secondary ingot of 550 × L2 (mm);

[0096] Step 6: Before the third smelting of the secondary ingot, add Cr raw material to the upper end surface of the secondary ingot:

[0097] The secondary ingot obtained in step 5 is turned around, that is, the lower end face of the secondary ingot is placed on the top, and the lower end face is drilled, and holes are drilled at two positions (at an angle of 180°) at the center of the ingot end face and at a radius of about 110 mm (i.e. 0.4R), respectively. The depth of the three holes is 137 mm (i.e. 0.5R), and fine Cr chips are placed therein. The amount of Cr added to each hole is 43.3 g, and then the same grade of zirconium alloy rods are used for welding and plugging the holes;

[0098] Step 7: Smelt the secondary ingot for the third time to obtain the tertiary ingot:

[0099] The drilled end of the secondary ingot obtained in step 6 is facing upwards, and is placed in a melting crucible with a diameter of 650 mm, and then evacuated. When the vacuum degree is 0.5 Pa, a leak test is performed, and the pressure rise rate is 0.4 Pa / min. After the leak test passes, the secondary ingot head is welded (that is, the drilled end of the secondary ingot is welded to the auxiliary electrode). After welding, vacuum consumable melting is performed, and the melting voltage is 40 V, the melting speed is 28 kg / min, and the melting current is 26 kA. After the melting is completed, the furnace is stopped and filled with argon for cooling for 6 hours, and then taken out of the furnace to obtain a tertiary ingot of 650×L3 (mm);

[0100] Step 8: Perform flaw detection and machining on the three ingots to obtain finished ingots:

[0101] The cylindrical surface of the tertiary ingot obtained in step 7 is peeled to remove surface defects such as pores, oxides, inclusions, etc., and the head and tail are sawed off after flaw detection to make the surface of the ingot present the original color of the metal to obtain a finished ingot. Samples are taken at 1 / 2R of the head end face of the ingot and at four positions on the upper, middle and lower sides of the cylindrical side. The chemical composition test is qualified and all meet the technical index requirements of the target product zirconium alloy ingot and the chemical components are evenly distributed. The Cr element detection results at each position are shown in Table 1.

[0102] Table 1 Cr content in each nuclear grade zirconium alloy ingot in Examples 1 to 4 (mass fraction, %)

[0103]

[0104]

[0105] As can be seen from Table 1, the preparation method provided by the present invention adjusts the target value of the ingredients of different electrode blocks and adds Cr raw materials to the upper end surface of the ingot to compensate for the volatilization of Cr elements in the ingot head during the smelting process; at the same time, the smelting times and parameters are strictly controlled to reduce the volatilization loss of Cr elements, thereby ensuring the high uniformity of chemical composition and greatly reducing the amount of ingot head removal. And by adopting the preparation method provided by the present invention, the process can be simplified, the ingot yield rate can be improved, the cost can be reduced, and a zirconium alloy ingot with high uniformity of chemical composition can be obtained to meet the high requirements of the nuclear industry.

[0106] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0107] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A preparation method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingots, characterized in that: By adjusting the batching method, electrode block pressing method, smelting times and smelting process, the uniformity of chemical composition and structure in nuclear-grade zirconium alloy ingots can be improved; The consumable electrode for smelting the nuclear-grade zirconium alloy ingot is formed by welding a plurality of electrode blocks in sequence, and the addition amount Y of the Cr raw material in the electrode block located at at least one end of the consumable electrode is 1.02 to 1.15 times the addition amount X of the Cr raw material in the remaining electrode blocks, so as to compensate for the volatilization of the Cr element at the head of the nuclear-grade zirconium alloy ingot during the vacuum consumable smelting process; The smelting times are 2 to 4 times; when the smelting times are greater than 2 times, before the last smelting, Cr raw material is further added to the upper end surface of the ingot charged into the furnace to compensate for the volatilization of the Cr element during the last smelting, and the chemical uniformity of the head of the nuclear-grade zirconium alloy ingot is ensured in combination with the final shrinkage feeding process; When the number of smelting times is greater than 2 times, before the last smelting, the specific method of further adding Cr raw material to the upper end face of the charged ingot is as follows: on the upper end face of the charged ingot, a first hole with a depth of h1 is drilled along the center of the upper end face, and a circle is determined with the center of the upper end face as the center and a radius of 0.4R~0.75R, and a plurality of second holes with a depth of h2 are drilled along the circumferential direction of the circle, and the first hole and the second hole are both used to add Cr raw material; wherein R is the radius of the charged ingot, and after the Cr raw material is added, the corresponding holes are welded and sealed with the same grade of zirconium alloy material.

2. The method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingot according to claim 1, characterized in that: The depths of the first hole and the second hole are both 0.25R to 0.75R.

3. The method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingot according to claim 1, characterized in that: A line connecting two adjacent second holes and the first hole forms an angle α, and the angle α is 60° to 180°.

4. The method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingot according to claim 2, characterized in that: The Cr raw material added to the first hole and the second hole is in the form of particles or crumbs, and the total amount added is 0.43πR 3 X×10 -3 g~1.3πR 3 X×10 -3 g.

5. The method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingot according to claim 1, characterized in that: The specific method of batching is: The sponge zirconium in the nuclear-grade zirconium alloy ingot is nuclear-grade sponge zirconium, and the Cr raw material is chromide or chromium-containing alloy or pure chromium metal.

6. The method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingot according to claim 1, characterized in that: The electrode block pressing method is specifically as follows: First, a layer of zirconium sponge is laid, and then the added raw materials are evenly arranged on the surface of the first layer of zirconium sponge. Finally, another layer of zirconium sponge is laid on the raw materials, and the two layers of zirconium sponge are used in the same amount; then, the required electrode blocks are pressed, and the number of the electrode blocks is determined according to the feed amount.

7. The method for improving the uniformity of Cr element in nuclear grade zirconium alloy ingot according to claim 1, characterized in that: The smelting process is specifically as follows: after each smelting, the obtained ingot is turned around and smelted again for the next time; During smelting: the first smelting is controlled by current, the subsequent smelting is controlled by melting rate, and the last smelting is carried out at the head of the ingot to ensure the chemical uniformity of the head of the nuclear-grade zirconium alloy ingot; During the smelting process: the ingot is flattened and surface cleaned after each smelting; After the final smelting is completed: the ingot after the final smelting is subjected to flaw detection and machining to obtain a finished nuclear-grade zirconium alloy ingot that meets the requirements; Among them, the smelting process parameters are: vacuum degree less than 1.5Pa, pressure rise rate less than 1.5Pa / min, smelting voltage of 28V~45V, smelting speed of 10kg / min~45kg / min, smelting current of 8kA~36kA, and cooling time after smelting is not less than 4h.