A hydrogel fiber material and preparation method

By adding glycerin and PDMS to gelatin materials and using printing technology to prepare double-helical structure hydrogel fiber materials, the problem of poor mechanical properties of traditional hydrogel materials is solved, high tensile strength and flexibility are achieved, and its performance is improved. Application prospects in new functional materials.

CN118563455BActive Publication Date: 2024-10-22WEST CHINA HOSPITAL SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411016747.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-22
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Traditional hydrogel materials have low fracture stress, low tensile strength, and poor mechanical properties, which limit their application in new functional materials.

Method used

By adding glycerol and PDMS to the gelatin material, printing and extrusion technology is used to prepare a double-helical hydrogel fiber material. The double-helical PDMS fiber is wrapped with the gelatin material, and combined with ultraviolet curing and drying treatments to form a double-helical hydrogel fiber material with high tensile strength. and flexible hydrogel fiber materials.

Benefits of technology

The hydrogel fiber material has a flexible texture, high tensile strength, improved mechanical properties, avoids the problems of irregular shape and uneven diameter, and significantly improves the application prospects of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563455B_ABST
    Figure CN118563455B_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogel fiber material and a preparation method, relates to the technical field of hydrogels, and solves the technical problems of low fracture stress, low tensile strength and poor mechanical properties of existing hydrogel materials; the outer layer of the hydrogel fiber material is a gelatin material layer, and the inside of the gelatin material layer is wrapped with double-helix PDMS fibers, and the double-helix PDMS fibers are cylindrical double-helix structures; the invention provides a hydrogel fiber material with a flexible texture and high tensile strength, and has better mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogels, and in particular to a hydrogel fiber material and a preparation method thereof. Background Art

[0002] Hydrogel is an elastomeric material composed of water molecules and a hydrophilic polymer network. It is a typical soft material. It has attracted people's attention since it was proposed. Because hydrogel has mechanical properties similar to solids and can bear certain external forces, and because its internal liquid allows polymer chains to move flexibly, the study of hydrogel provides a new design idea for the design of new soft materials. Hydrogel has also developed rapidly in the biomedical field because of the above characteristics.

[0003] Traditional hydrogel materials are prepared by mixing multiple materials into one, so the finished product has a single internal structure and poor mechanical properties. It is soft and easy to crush, has low fracture stress, cannot be adjusted in mechanical strength, has poor expandability, and has a single functionality. These shortcomings greatly limit the application scope and prospects of hydrogel materials as new functional materials. Summary of the invention

[0004] The present invention aims to solve the technical problems of low fracture stress, low tensile strength and poor mechanical properties of existing hydrogel materials, and aims to provide a hydrogel fiber material and a preparation method thereof, thereby obtaining a hydrogel fiber material with a flexible texture, high tensile strength and better mechanical properties.

[0005] The present invention is achieved through the following technical solutions.

[0006] The first object of the present invention is to provide a method for preparing a hydrogel fiber material, comprising the following steps:

[0007] S1. Add water, acrylic acid, acrylamide, gelatin, glycerol and LAP into a reaction device with stirring and heating functions according to the mass ratio, heat the reaction device to 60-80°C, stir the raw materials to obtain a light yellow viscous solution, then put it into an ultrasonic vibration defoamer, oscillate at 60-80°C for 20-40 minutes, and obtain a transparent and clear light yellow viscous solution, i.e., feed liquid A;

[0008] S2, putting PDMS into a reaction device with a stirring function and mixing it thoroughly, then adding silicon dioxide, and stirring until the mixture is in a state where it does not flow freely, to obtain liquid B;

[0009] S3, respectively transferring liquid A and liquid B to the dispensing syringe of the printing extrusion device, starting continuous extrusion, adjusting the rotation speed of the nozzle during extrusion, and obtaining a preformed gel material with spiral structures of different densities; wherein the dispensing syringe of liquid A is connected to a short dispensing needle, and the dispensing syringe of liquid B is connected to a long dispensing needle, so that liquid A flows out before liquid B and completely wraps the long dispensing needle;

[0010] S4, while the preformed gel material is extruded and falls, irradiating with ultraviolet light for 30-60 seconds to completely solidify the outer layer of gelatin material;

[0011] S5, placing the illuminated gel material in a drying oven at 70-90°C for 2-4 hours to solidify the inner PDMS layer;

[0012] S6. Soak the dried gel material in pure water for 5-10 minutes to obtain a soft and elastic hydrogel fiber material.

[0013] When preparing the hydrogel fiber material, the present invention adds glycerol to the gelatin material, so that the gel material is extruded more smoothly and more easily to form a cylindrical strip, thereby avoiding the generation of gel with irregular shape and uneven diameter; the dispensing syringe of liquid A is connected to a short dispensing needle, and the dispensing syringe of liquid B is connected to a long dispensing needle, so that liquid A can flow out before liquid B and merge in the nozzle, so that the liquid A that flows out first completely wraps the long dispensing needle (the outflowing liquid B), ensuring that liquid A fully wraps liquid B, thereby achieving the wrapping of the double-helix PDMS fiber inside the gelatin material layer; the gel material is initially formed by irradiating ultraviolet light while the preformed gel material is extruded and falling, thereby avoiding the problem of irregular gel shape and uneven cross-sectional area caused by the flow of the liquid.

[0014] As a further technical solution of the present invention, a dimensionless rotation rate n=Rw / v is defined, wherein R is the radius of the inner side of the nozzle, w is the angular velocity, and v is the linear velocity of the inner side of the nozzle; during continuous extrusion in step S3, the adjustment range of n is 0-15, and the rotation lasts for 30-60s.

[0015] Because the translation speed between the printing platform and the printing nozzle remains unchanged (at a speed of 3 mm / s), and the different rotation speeds of the nozzle will cause the extruded gel to rotate different numbers of times at the same distance and time, it is possible to obtain a gel with a double-helix structure PDMS material containing different numbers of spirals in the same length. By adjusting the dimensionless rotation rate n to 0, 5, 10, and 15, respectively, and continuing for 30-60 seconds, a certain length of preformed gel containing a spiral structure PDMS material with different densities can be obtained.

[0016] As a further technical solution of the present invention, in the liquid A, the mass ratio of water, acrylic acid, acrylamide, gelatin and glycerol is (4~4.5):2:2:4:2, and the mass of LAP accounts for 0.1~0.15% of the total mass of the liquid A; in the liquid B, silicon dioxide accounts for 5~8% of the mass of PDMS.

[0017] The second object of the present invention is to provide a hydrogel fiber material prepared by the aforementioned preparation method, wherein the outer layer of the hydrogel fiber material is a gelatin material layer, and the inside of the gelatin material layer wraps a double-helix PDMS fiber, and the double-helix PDMS fiber is a cylindrical double-helix structure.

[0018] The hydrogel fiber material provided by the present invention has double-helix PDMS fibers formed by rotation inside, and is fully wrapped in an outer layer with a gelatin material. The PDMS fibers with a double-helix structure can effectively enhance and toughen the hydrogel fiber material, and is a hydrogel fiber material with a flexible texture and high tensile strength. Compared with existing hydrogel materials, the hydrogel fiber material of the present invention has better mechanical properties; and glycerol is added to the hydrogel fiber material of the present invention, so that the gel material is extruded more smoothly and more easily to form cylindrical strips, thereby avoiding the generation of gels with irregular shapes and uneven diameters.

[0019] The third object of the present invention is to provide a printing and extrusion device for hydrogel fiber materials, comprising:

[0020] Fixed frame;

[0021] A motor connected to a fixed frame;

[0022] A connecting shaft connected to an output end of a motor;

[0023] The dispensing syringe is fixed on the connecting shaft and is used to contain the material liquid;

[0024] An air guide mechanism, fixed on the connecting shaft, is used to guide compressed air into the dispensing syringe;

[0025] The dispensing needle is connected to the dispensing syringe through a catheter, and includes a long dispensing needle and a short dispensing needle that are alternately arranged;

[0026] A nozzle connected to the outlet end of the dispensing needle;

[0027] The liquid flowing out of the short dispensing needle merges in the nozzle and completely wraps the long dispensing needle.

[0028] When the printing extrusion device of the present invention is working, compressed air is transmitted into the air guide mechanism through the air pump, and then the compressed air is introduced into the glue dispensing syringe through the air guide mechanism. The material liquid in the glue dispensing syringe is squeezed out by the gas pressure, and the material liquid enters the nozzle through the glue dispensing needle. In the nozzle, the short glue dispensing needle first flows out the material liquid and merges in the nozzle, and completely wraps the long glue dispensing needle, thereby wrapping the material liquid flowing out of the long glue dispensing needle; at the same time, the motor drives the nozzle to rotate through the connecting shaft, thereby realizing the operation of spiralizing the extruded material.

[0029] As a further technical solution of the present invention, the air guide mechanism includes an air inlet cylinder and an air guide pipe. The air inlet cylinder is fixed on the connecting shaft. An air inlet is opened on the side of the air inlet cylinder. The upper end of the air guide pipe is connected to the air outlet of the air inlet cylinder, and the lower end is connected to the glue dispensing syringe.

[0030] As a further technical solution of the present invention, the lower end of the air guide tube is connected to the top of the glue dispensing syringe through a vent plug.

[0031] As a further technical solution of the present invention, the upper end of the dispensing syringe is connected to the connecting shaft through a syringe fixing plate.

[0032] As a further technical solution of the present invention, it also includes a needle connector, the upper end of which is fixed to the connecting shaft through a lower coupling, and the lower end of which is connected to the dispensing needle.

[0033] As a further technical solution of the present invention, a positioning groove is provided on the needle connector, and the dispensing needles are clamped in the positioning groove. The middle part of the needle connector is provided with needle channels with the same number as the dispensing needles, and the needle channels are connected to the nozzle below.

[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The hydrogel fiber material provided by the present invention has double-helix PDMS fibers formed by rotation inside, and is fully wrapped in the outer layer with gelatin material. The PDMS fibers with double-helix structure can effectively enhance and toughen, and are a hydrogel fiber material with a flexible texture and high tensile strength. Compared with the existing hydrogel materials, the hydrogel fiber material of the present invention has better mechanical properties; 2. The present invention adds glycerol to the gelatin material, which makes it smoother to extrude the gel material and easier to extrude into cylindrical strips, thus avoiding the formation of gels with irregular shapes and uneven diameters. By adding glycerol to the PDMS material Silicon can increase the viscosity of the PDMS liquid so that it will not flow freely and will only flow out when under pressure; 3. The present invention connects the dispensing syringe of liquid A to a short dispensing needle and connects the dispensing syringe of liquid B to a long dispensing needle, so that liquid A can flow out before liquid B and merge in the nozzle, so that the liquid A that flows out first can completely wrap the long dispensing needle (the outflowing liquid B), ensuring that liquid A fully wraps liquid B, thereby wrapping the double-helix PDMS fiber inside the gelatin material layer; 4. The present invention preliminarily forms the gel material by irradiating it with ultraviolet light while the preformed gel material is extruded and falling, thereby avoiding the problems of irregular gel shape and uneven cross-sectional area caused by the flow of the liquid. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0036] Figure 1 It is a schematic structural diagram of the hydrogel fiber material of the present invention;

[0037] Figure 2 It is a schematic diagram of the three-dimensional structure of the printing extrusion device of the present invention;

[0038] Figure 3 for Figure 2 A magnified view of the middle A area;

[0039] Figure 4 A bottom view of the printing extrusion device of the present invention;

[0040] Figure 5 is a schematic diagram of the three-dimensional structure of the needle connector;

[0041] Figure 6 is a top view of the needle connector;

[0042] Figure 7 for Figure 6 Middle BB section view;

[0043] Figure 8 It is the stress-strain diagram of the tensile test of the hydrogel fiber material prepared in Examples 1-4;

[0044] Fig. 9 It is the stress-strain diagram of the tensile test of the hydrogel fiber material prepared in Comparative Examples 1-3;

[0045] Fig.10 This is the stress-strain diagram of the tensile test of the hydrogel fiber material prepared in Comparative Example 4.

[0046] Marks and corresponding parts names in the attached drawings:

[0047] 1-fixed frame, 2-motor, 3-upper coupling, 4-connecting shaft, 5-air inlet, 501-air inlet, 6-air guide tube, 7-syringe fixing plate, 8-vent plug, 9-dispensing syringe, 10-catheter, 11-dispensing needle, 111-long dispensing needle, 112-short dispensing needle, 12-needle connector, 121-positioning groove, 122-needle channel, 13-nozzle, 14-lower coupling, 15-double helix PDMS fiber, 16-gelatin material layer. DETAILED DESCRIPTION

[0048] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary implementation modes of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0049] Example 1

[0050] This embodiment provides a method for preparing a hydrogel fiber material, comprising the following steps:

[0051] S1: Weigh 2g of acrylic acid, 2g of acrylamide, 4g of gelatin, 2g of glycerol, 4g of water, and 0.02g of LAP and put them into a reaction device with stirring and heating functions, heat the reaction device to 70°C, stir the raw materials thoroughly to obtain a light yellow viscous solution, then put it into an ultrasonic vibration defoamer, oscillate at 70°C for 30min, and obtain a transparent and clear light yellow viscous solution, i.e., liquid A;

[0052] S2, 8 g of PDMS was put into a reaction device with a stirring function and stirred thoroughly to obtain a transparent liquid, and then 0.64 g of silicon dioxide (accounting for 8% of the mass of PDMS) was added, and stirred thoroughly until the mixture was in a state where it would not flow freely, to obtain liquid B;

[0053] S3, respectively transferring liquid A and liquid B to the dispensing syringe of the printing extrusion device, adjusting the extrusion air pressure to 0.2Mpa, starting continuous extrusion, with a dimensionless rotation rate n=15 during extrusion, and continuing for 30-60s to obtain a preformed gel material with a spiral structure of a certain density; wherein the dispensing syringe of liquid A is connected to a short dispensing needle, and the dispensing syringe of liquid B is connected to a long dispensing needle;

[0054] S4, while the preformed gel material is extruded and falls, irradiating with ultraviolet light for 30-60 seconds to completely solidify the outer layer of gelatin material;

[0055] S5, placing the illuminated gel material in a drying oven at 80° C. for 3 h to solidify the inner PDMS layer;

[0056] S6. Soak the dried gel material in pure water for 5-10 minutes to obtain a soft and elastic hydrogel fiber material.

[0057] The structure of the prepared hydrogel fiber material is as follows: Figure 1 As shown, the outer layer of the hydrogel fiber material is a gelatin material layer 16, and the inside of the gelatin material layer 16 wraps the double-helix PDMS fiber 15, and the double-helix PDMS fiber 15 is a cylindrical double-helix structure.

[0058] Example 2

[0059] The difference between this embodiment and embodiment 1 is that the dimensionless rotation rate n during extrusion is 10.

[0060] Example 3

[0061] The difference between this embodiment and embodiment 1 is that the dimensionless rotation rate n=5 during extrusion.

[0062] Example 4

[0063] The difference between this embodiment and embodiment 1 is that the dimensionless rotation rate n=0 during extrusion.

[0064] Example 5

[0065] The difference between this embodiment and embodiment 1 is that the amount of water added is increased to 4.5 g.

[0066] Example 6

[0067] The difference between this embodiment and embodiment 1 is that the amount of silicon dioxide added is adjusted to 5% of the mass of PDMS, that is, the added amount is 0.4 g.

[0068] Example 7

[0069] This embodiment provides a printing and extrusion device for preparing a hydrogel fiber material, such as Figure 2-7 As shown, including:

[0070] A fixing frame 1, used for fixing the device structure;

[0071] The motor 2 is connected to the fixing frame 1 through an L-shaped bracket;

[0072] The connecting shaft 4 is connected to the output end of the motor 2 through the upper coupling 3;

[0073] The dispensing syringe 9 is fixed on the connecting shaft 4 and is used to contain the material liquid;

[0074] An air guide mechanism, fixed on the connecting shaft 4, is used to guide compressed air into the glue dispensing syringe 9;

[0075] The glue dispensing needle 11 is connected to the glue dispensing syringe 9 through the catheter 10, and includes a long glue dispensing needle 111 and a short glue dispensing needle 112 that are alternately arranged;

[0076] The nozzle 13 is connected to the outlet end of the dispensing needle 11;

[0077] The liquid flowing out of the short dispensing needle 112 merges in the nozzle 13 and completely wraps the long dispensing needle 111 .

[0078] When the printing extrusion device of the present invention is working, compressed air is transmitted to the air guide mechanism through the air pump, and then the compressed air is introduced into the glue dispensing syringe 9 through the air guide mechanism. The liquid in the glue dispensing syringe 9 is squeezed out by the gas pressure, and the liquid enters the nozzle 13 through the glue dispensing needle 11. In the nozzle 13, the short glue dispensing needle 112 first flows out the liquid and merges in the nozzle 13, and completely wraps the long glue dispensing needle 111, thereby wrapping the liquid flowing out of the long glue dispensing needle 111; at the same time, the motor 2 drives the nozzle 13 to rotate through the connecting shaft 4, so as to realize the operation of spiralizing the extruded material.

[0079] The air guide mechanism includes an air inlet cylinder 5 and an air guide pipe 6. The air inlet cylinder 5 is fixed on the connecting shaft 4. An air inlet 501 is provided on the side of the air inlet cylinder 5. The upper end of the air guide pipe 6 is connected to the air outlet of the air inlet cylinder 5, and the lower end is connected to the glue dispensing syringe 9. The air inlet 501 on the side of the air inlet cylinder 5 is used to introduce compressed air, and then the compressed air enters the air guide pipe 6 from the air outlet, and then the compressed air is introduced into the glue dispensing syringe 9 through the air guide pipe 6, so as to realize the extrusion of the material liquid.

[0080] Specifically, the lower end of the air guide tube 6 is connected to the top of the glue dispensing syringe 9 through the vent plug 8. The vent plug 8 is provided to facilitate the connection between the air guide tube 6 and the glue dispensing syringe 9.

[0081] Specifically, the upper end of the dispensing syringe 9 is connected to the connecting shaft 4 through a syringe fixing plate 7. The syringe fixing plate 7 is disc-shaped and is provided with a through hole matching the dispensing syringe 9. The upper end of the dispensing syringe 9 is fixed in the through hole. The dispensing syringe 9 is fixed by the setting of the syringe fixing plate 7 to improve its stability.

[0082] Example 8

[0083] This embodiment further illustrates the printing extrusion device based on the embodiment 7.

[0084] The printing extrusion device of this embodiment further includes a needle connector 12 , the upper end of the needle connector 12 is fixed to the connecting shaft 4 via a lower coupling 14 , and the lower end of the needle connector 12 is connected to the dispensing needle 11 .

[0085] The needle connector 12 is provided with a positioning groove 121. Figure 2-7 As shown, taking two long dispensing needles 111 and two short dispensing needles 112 as an example, the two long dispensing needles 111 are arranged opposite to each other, and the two short dispensing needles 112 are arranged opposite to each other, and each dispensing needle 11 corresponds to a positioning groove 121, and the dispensing needle 11 is clamped in the positioning groove 121 to play a positioning role, and the middle part of the needle connector 12 is provided with needle channels 122 with the same number as the dispensing needles 11, and the needle channels 122 are connected to the nozzle 13 below; specifically, the nozzle 13 has a channel, and the dispensing needle 11 is L-shaped, and its lower end passes through the needle channel 122 and extends into the internal channel of the nozzle 13. In the internal channel of the nozzle 13, the length of the short dispensing needle 112 is smaller than that of the long dispensing needle 111, so that the liquid flowing out of the short dispensing needle 112 can wrap the long dispensing needle 111.

[0086] Comparative example 1.

[0087] In this comparative example, the mass ratio of gelatin to glycerol is adjusted from 4:2 to 5:1, and a method for preparing a hydrogel fiber material is provided, comprising the following steps:

[0088] S1: Weigh 2g of acrylic acid, 2g of acrylamide, 5g of gelatin, 1g of glycerol, 4g of water, and 0.021g of LAP and put them into a reaction device with stirring and heating functions. Heat the reaction device to 70°C, fully stir the raw materials to obtain a light yellow viscous solution, then put it into an ultrasonic vibration defoamer, and oscillate at 70°C for 30 minutes to obtain a transparent and clear light yellow viscous solution, i.e., liquid A;

[0089] S2, put 8 g of PDMS into a reaction device with a stirring function and stir it thoroughly to obtain a transparent liquid, then add 0.64 g of silicon dioxide, and stir it thoroughly until the mixture is in a state where it does not flow freely, to obtain liquid B;

[0090] S3, respectively transferring liquid A and liquid B to the dispensing syringe of the printing extrusion device, adjusting the extrusion air pressure to 0.2Mpa, starting continuous extrusion, with a dimensionless rotation rate n=15 during extrusion, and continuing for 30-60s to obtain a preformed gel material with a spiral structure of a certain density; wherein the dispensing syringe of liquid A is connected to a short dispensing needle, and the dispensing syringe of liquid B is connected to a long dispensing needle;

[0091] S4, while the preformed gel material is extruded and falls, ultraviolet light is irradiated for 30-60 seconds to completely solidify the outer layer gelatin material;

[0092] S5, placing the illuminated gel material in a drying oven at 80° C. for 3 h to solidify the inner PDMS layer;

[0093] S6. Soak the dried gel material in pure water for 5-10 minutes to obtain a soft and elastic hydrogel fiber material.

[0094] Comparative example 2.

[0095] The difference between this comparative example and comparative example 1 is that the dimensionless rotation rate n=5 during extrusion.

[0096] Comparative example 3.

[0097] The difference between this comparative example and comparative example 1 is that the dimensionless rotation rate n=0 during extrusion.

[0098] Comparative example 4.

[0099] The difference between this comparative example and Example 1 is that only liquid A is used without liquid B, and a gel material of pure gelatin is obtained.

[0100] Performance testing.

[0101] The hydrogel fiber materials prepared in Examples 1-4 and Comparative Examples 1-4 were printed and their performance tested.

[0102] 1. The printing test method is: circular printing shape (diameter is 8mm).

[0103] Examples 1-4 can all be printed successfully, but Example 1 cannot print out a complete and regular cylindrical strip sample when the rotation speed is 15 or above. This is because the viscosity of the material in Example 1 is too high due to the increased gelatin content. When the rotation speed increases to a certain level, a complete and regular cylindrical strip sample cannot be printed out.

[0104] 2. Tensile mechanical properties test: Print 60×10 mm cylindrical tensile specimens and test at a tensile rate of 100 mm / min. The results are as follows Figure 8-9 shown.

[0105] from Figure 8 and Fig. 9 By comparison, it can be seen that the mechanical properties (elastic modulus, fracture energy) of the gel materials prepared in Examples 1-4 increase with the increase of the rotation speed, and the mechanical properties are good. This is because the PDMS fibers with a double helix structure can effectively enhance the toughness, thereby obtaining a hydrogel fiber material with a flexible texture and high tensile strength. The mechanical properties of the gel materials prepared in Comparative Examples 1-3 are significantly lower than those of the gel materials prepared in Examples 1-4, and a complete and regular cylindrical strip sample cannot be printed when the rotation speed is 15 or above.

[0106] from Figure 8 and Fig.10 By comparison, it can be seen that the strength of the gel material introduced with PDMS fibers in the present invention is significantly higher than that of the gel material with only pure gelatin.

[0107] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a hydrogel fiber material, characterized in that: The following steps are involved: S1. Add water, acrylic acid, acrylamide, gelatin, glycerol and LAP into a reaction device with stirring and heating functions according to the mass ratio, heat the reaction device to 60-80°C, stir the raw materials to obtain a light yellow viscous solution, then put it into an ultrasonic vibration defoamer, oscillate at 60-80°C for 20-40 minutes, and obtain a transparent and clear light yellow viscous solution, i.e., feed liquid A; S2, putting PDMS into a reaction device with a stirring function and mixing it thoroughly, then adding silicon dioxide, and stirring until the mixture is in a state where it does not flow freely, to obtain liquid B; S3, respectively transferring liquid A and liquid B to the dispensing syringe of the printing extrusion device, starting continuous extrusion, adjusting the rotation speed of the nozzle during extrusion, and obtaining a preformed gel material with spiral structures of different densities; wherein the dispensing syringe of liquid A is connected to a short dispensing needle, and the dispensing syringe of liquid B is connected to a long dispensing needle, so that liquid A flows out before liquid B and completely wraps the long dispensing needle; S4, while the preformed gel material is extruded and falls, irradiating with ultraviolet light for 30-60 seconds to completely solidify the outer layer of gelatin material; S5, placing the illuminated gel material in a drying oven at 70-90°C for 2-4 hours to solidify the inner PDMS layer; S6. Soak the dried gel material in pure water for 5-10 minutes to obtain a soft and elastic hydrogel fiber material.

2. The method for preparing a hydrogel fiber material according to claim 1, characterized in that: A dimensionless rotation rate n=Rw / v is defined, where R is the radius of the inner side of the nozzle, w is the angular velocity, and v is the linear velocity of the inner side of the nozzle; during continuous extrusion in step S3, the adjustment range of n is 0-15, and the rotation lasts for 30-60s.

3. The method for preparing a hydrogel fiber material according to claim 1, characterized in that: In the liquid A, the mass ratio of water, acrylic acid, acrylamide, gelatin and glycerol is (4-4.5):2:2:4:2, and the mass of LAP accounts for 0.1-0.15% of the total mass of the liquid A; in the liquid B, silicon dioxide accounts for 5-8% of the mass of PDMS.

4. The method for preparing a hydrogel fiber material according to claim 1, characterized in that: The printed extrusion The device includes: Fixed frame (1); A motor (2) connected to the fixing frame (1); A connecting shaft (4) connected to an output end of the motor (2); A dispensing syringe (9) is fixed on the connecting shaft (4) and is used to contain the material liquid; An air guide mechanism, fixed on the connecting shaft (4), used for guiding compressed air into the glue dispensing syringe (9); A glue dispensing needle (11), connected to the glue dispensing syringe (9) via a conduit (10), comprising a long glue dispensing needle (111) and a short glue dispensing needle (112) arranged alternately; A nozzle (13) connected to the outlet end of the dispensing needle (11); The liquid flowing out of the short dispensing needle (112) merges in the nozzle (13) and completely wraps the long dispensing needle (111).

5. The method for preparing a hydrogel fiber material according to claim 4, characterized in that: The air guide mechanism comprises an air inlet cylinder (5) and an air guide pipe (6); the air inlet cylinder (5) is fixed on the connecting shaft (4); an air inlet (501) is provided on the side of the air inlet cylinder (5); the upper end of the air guide pipe (6) is connected to the air outlet of the air inlet cylinder (5), and the lower end is connected to the glue dispensing syringe (9).

6. The method for preparing a hydrogel fiber material according to claim 5, characterized in that: The lower end of the air guide tube (6) is connected to the top of the glue dispensing syringe (9) through a vent plug (8).

7. The method for preparing a hydrogel fiber material according to claim 4, characterized in that: The upper end of the glue dispensing syringe (9) is connected to the connecting shaft (4) via a syringe fixing plate (7).

8. The method for preparing a hydrogel fiber material according to claim 4, characterized in that: It also includes a needle connector (12), the upper end of the needle connector (12) is fixed to the connecting shaft (4) via a lower coupling (14), and the lower end of the needle connector (12) is connected to the dispensing needle (11).

9. The method for preparing a hydrogel fiber material according to claim 8, characterized in that: The needle connector (12) is provided with a positioning groove (121), and the dispensing needle (11) is clamped in the positioning groove (121). The middle part of the needle connector (12) is provided with needle channels (122) the same number as the dispensing needle (11), and the needle channels (122) are connected to the nozzle (13) below.

10. A hydrogel fiber material, characterized in that: The method is prepared according to any one of claims 1 to 9.