Fibrous silicon-carbon composite material and preparation method thereof, and lithium-ion battery
By doping metal lithium in carbon fibers and using silane coupling agents and other technologies, efficient fibrous silicon-carbon composite materials are formed, which solves the conductivity and expansion problems of lithium-ion battery materials and achieves higher specific capacity and cycle performance. .
Patent Information
- Application Number
- CN202411032241.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing silicon-carbon composite materials of lithium-ion battery materials have poor electronic conductivity and low compressive strength due to their porous structure, resulting in large expansion at full power, and the existing technology has not been able to effectively develop low-expansion carbon materials from the perspective of carbon matrix. Improve conductivity and cycle performance.
Using the preparation method of fibrous silicon-carbon composite materials, doping metal lithium in carbon fibers, using silane coupling agents to form a three-dimensional network structure, adding organic acid pore-forming agents to increase the number of holes, depositing nano-silica through negative pressure and in positive Surface passivation is carried out under pressure to reduce the growth of silicon grains and improve the electronic conductivity and specific capacity of the material.
It effectively reduces the expansion of the material, increases the electronic or ion conductivity, and improves the rate and cycle performance of lithium-ion batteries.
Smart Images

Figure CN118563564B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a fibrous silicon-carbon composite material and a preparation method thereof, and a lithium ion battery. Background Art
[0002] Silicon-carbon materials prepared by silane cracking method have become the preferred materials for high energy density lithium-ion batteries due to their high specific capacity (about 1850mAh / g), high first efficiency (about 92%) and low expansion when fully charged. However, due to the porous structure, the electronic conductivity of silicon-carbon materials is poor and the compressive strength of porous carbon itself is low. In addition, the full-charge expansion of the material is still large in the case of high addition amount. Therefore, it is necessary to improve the compressive strength of silicon-carbon materials to reduce the full-charge expansion of the material. There are many measures to reduce expansion or improve fast charging, such as increasing the pore volume to reserve space for its expansion, or doping materials with high electronic or ionic conductivity to improve the fast charging performance of the material.
[0003] The prior art (patent application number: CN202310437660.5) discloses: a fluorine-nitrogen doped amorphous carbon-coated silicon-carbon composite material and a preparation method thereof, using a silane cracking method, introducing a silane mixture into the porous carbon to deposit nano-silicon in the porous carbon; then introducing a nitrogen trifluoride and carbon source mixture, and coating the outer layer of the porous carbon on which nano-silicon is deposited with fluorine-nitrogen doped amorphous carbon to obtain the fluorine-nitrogen doped amorphous carbon-coated silicon-carbon composite material, wherein the outer layer electronic conductivity is improved, and the porous carbon with a large pore volume of the material can reduce the expansion of the material, and the porous carbon itself has low strength, and the expansion of the material is not greatly improved.
[0004] In the prior art, there is no low-expansion carbon material developed from the perspective of the carbon matrix, which can reduce expansion and increase the electronic or ionic conductivity of the material, thereby achieving increased rate and improved cycle performance.
[0005] Therefore, the existing technology needs to be improved. Summary of the invention
[0006] There is no low-expansion carbon material developed from the perspective of carbon matrix in the prior art, which can reduce expansion and increase the electronic or ionic conductivity of the material, thereby increasing the rate and improving the cycle performance. Therefore, the present invention provides a fibrous silicon-carbon composite material and a preparation method thereof, and a lithium-ion battery for solving the above problems.
[0007] In a first aspect, the present invention provides a method for preparing a fibrous silicon-carbon composite material, which comprises the following specific steps:
[0008] S1, adding an organic lithium salt, a silane coupling agent and an organic acid pore-forming agent into an organic solvent to prepare a solution, and adding carbon fiber to disperse evenly to obtain a mixed solution;
[0009] S2, subjecting the mixed solution to a hydrothermal reaction at a temperature of 100-200° C. and a pressure of 5-10 MPa for 1-6 h, filtering and freeze-drying;
[0010] S3, transferring the dried material to a tubular furnace, introducing an activated gas after heating to form pores, and obtaining lithium-doped porous carbon fibers;
[0011] S4, transferring the lithium-doped porous carbon fiber to a fluidized bed, introducing monosilane gas to perform negative pressure deposition of nano-silicon;
[0012] S5. After the silicon deposition reaction is completed, the introduction of monosilane gas is stopped, and unsaturated hydrocarbons are introduced to perform positive pressure and low temperature surface passivation to obtain a fibrous silicon-carbon composite material.
[0013] In one implementation, in S1, raw materials are provided according to a mass ratio of organic lithium salt: silane coupling agent: organic acid pore-forming agent: organic solvent: carbon fiber = (1-5): (1-5): (1-5): (500-2000): 100.
[0014] In one implementation, in S1, the organic lithium salt includes any one or a combination of phenyl lithium, methyl lithium, n-butyl lithium and tert-butyl lithium diisopropylamide; the silane coupling agent includes any one or a combination of γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane; the organic acid pore-forming agent includes any one or a combination of oxalic acid, citric acid, diethylaminetetraacetic acid and lactic acid; the organic solvent includes any one or a combination of tetrahydrofuran, cyclohexane, tetrachloromethane and N,N-dimethylacetamide.
[0015] In one implementation, in S1, the length of the carbon fiber is 10-100 μm, the diameter of the carbon fiber is 1-10 μm, and the wall thickness of the carbon fiber is 50-500 nm.
[0016] In one implementation, in S2, the freeze drying is performed at -40°C for 24 hours; in S3, the activated gas is introduced when the temperature is raised to 500-800°C, the flow rate of the activated gas is 100-500 ml / min, and the pore making time is 60-600 min.
[0017] In one implementation, in S4, the temperature needs to be raised to 300-400°C before introducing monosilane gas, the flow rate of the monosilane gas is 100-500 ml / min, the pressure of the cavity during silicon deposition is 0.1-0.5 MPa, and the silicon deposition time is 30-300 min.
[0018] In one implementation, in S4, the activation gas is carbon dioxide or water vapor; in S5, the unsaturated hydrocarbon includes any one of acetylene, ethylene, propyne and butyne.
[0019] In one implementation, in S5, the time for low-temperature surface passivation is 30 to 300 minutes, and the pressure of the passivation reaction is 5 to 10 MPa.
[0020] In a second aspect, the present invention further provides a fibrous silicon-carbon composite material, which is prepared by the above-mentioned preparation method of the fibrous silicon-carbon composite material.
[0021] In a third aspect, the present invention further provides a lithium-ion battery, which comprises the fibrous silicon-carbon composite material provided by the present invention as a negative electrode material of the battery.
[0022] Beneficial effects: The preparation method of the fibrous silicon-carbon composite material provided by the present invention improves the electronic conductivity and the initial efficiency of the material by doping metallic lithium into the carbon fiber; forms a three-dimensional network structure of the carbon fiber through a silane coupling agent, which can improve the electronic conductivity between the materials and reduce the expansion; increases the pores of the lithium-doped carbon fiber composite material by adding an organic acid pore-forming agent, so that it can accommodate more lithium ions and improve the specific capacity of the silicon-carbon composite material; decomposes monosilane gas through negative pressure deposition, so that nano-silicon is easily deposited in the porous carbon and passivated under positive pressure; introduces monosilane gas for negative pressure deposition of nano-silicon, and under negative pressure Nano-silicon is deposited in porous carbon fibers by a silane cracking method, so that the nano-silicon is more easily deposited in the internal pores. Under positive pressure conditions, amorphous carbon is deposited on the surface to improve the quality of Si-CH deposition, so that the carbon material has the characteristics of high density and the like. Positive pressure and low-temperature surface passivation are performed by introducing unsaturated hydrocarbons, and the growth of silicon grains is avoided by low-temperature passivation, and expansion is reduced to obtain a fibrous silicon-carbon composite material. The fibrous silicon-carbon composite material and lithium-ion battery obtained by the preparation method provided by the present invention can reduce expansion and improve the electronic or ionic conductivity of the material, while increasing the rate and improving the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of the steps of the method for preparing the fibrous silicon-carbon composite material provided by the present invention;
[0024] Figure 2 It is a graph showing the cycle performance test results when the fibrous silicon-carbon composite material in Example 1 and Comparative Example 1 is used as the negative electrode material.
[0025] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the description of the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" described below means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms is not necessarily for the same embodiment or example. Moreover, the technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.
[0027] See also Figure 1 , Figure 1 The present invention provides a method for preparing a fibrous silicon-carbon composite material, which comprises the following specific steps:
[0028] S1, adding an organic lithium salt, a silane coupling agent and an organic acid pore-forming agent into an organic solvent to prepare a solution, and adding carbon fiber to disperse evenly to obtain a mixed solution;
[0029] S2, subjecting the mixed solution to a hydrothermal reaction at a temperature of 100-200° C. and a pressure of 5-10 MPa for 1-6 h, filtering and freeze-drying;
[0030] S3, transferring the dried material to a tubular furnace, introducing an activated gas to form pores after heating, and obtaining lithium-doped porous carbon fibers;
[0031] S4, transferring the lithium-doped porous carbon fiber to a fluidized bed, introducing monosilane gas to perform negative pressure deposition of nano-silicon;
[0032] S5. After the silicon deposition reaction is completed, the introduction of monosilane gas is stopped, and unsaturated hydrocarbons are introduced to perform positive pressure and low temperature surface passivation to obtain a fibrous silicon-carbon composite material.
[0033] Specifically, in S1, raw materials are provided according to the mass ratio of organic lithium salt: silane coupling agent: organic acid pore-forming agent: organic solvent: carbon fiber = (1~5): (1~5): (1~5): (500~2000): 100. Wherein, the organic lithium salt includes any one or a combination of phenyl lithium, methyl lithium, n-butyl lithium and tert-butyl lithium diisopropyl amide lithium. The silane coupling agent includes any one or a combination of γ-mercaptopropyl triethoxysilane, γ-aminopropyl triethoxysilane and γ-(2,3-epoxypropoxy)propyl trimethoxysilane. The organic acid pore-forming agent includes any one or a combination of oxalic acid, citric acid, diethylaminetetraacetic acid and lactic acid. The organic solvent includes any one or a combination of tetrahydrofuran, cyclohexane, tetrachloromethane and N,N-dimethylacetamide. The length of the carbon fiber is 10-100 μm, the diameter of the carbon fiber is 1-10 μm, and the wall thickness of the carbon fiber is 50-500 nm.
[0034] Doping carbon fiber with lithium salt reduces the defects of the material and improves its ion conductivity, improves the rate and its initial efficiency; at the same time, the carbon fiber is coupled by the silane coupling agent to form a three-dimensional structure to reduce expansion. Adding the organic acid pore-forming agent helps to increase the pores of the lithium-doped carbon fiber composite material, helps to accommodate more lithium ions, and improves the specific capacity of the silicon-carbon composite material.
[0035] Specifically, in S2, the freeze drying is performed at -40°C for 24 hours. The hydrothermal reaction causes the organic lithium salt, the silane coupling agent and the organic acid pore-forming agent to react at a certain temperature and pressure to form a pore structure. The solvent is evaporated by freeze drying in this step to obtain a porous material with a high pore volume.
[0036] Specifically, in S3, the activation gas is introduced when the temperature is raised to 500-800°C, the flow rate of the activation gas is 100-500 ml / min, and the pore-making time is 60-600 min.
[0037] In S4, the temperature needs to be raised to 300-400°C before the monosilane gas is introduced, the flow rate of the monosilane gas is 100-500ml / min, the pressure of the cavity during silicon deposition is 0.1-0.5Mpa, and the silicon deposition time is 30-300min. Among them, nano-silicon is deposited in porous carbon fibers by silane cracking method under negative pressure, so that the nano-silicon is more easily deposited in the internal pores, and amorphous carbon is deposited on its surface under positive pressure conditions, which has the characteristics of high density of carbon materials. Further, the activation gas is carbon dioxide or water vapor.
[0038] Specifically, in S5, the surface low-temperature passivation time is 30 to 300 minutes, and the passivation reaction pressure is 5 to 10 MPa. The unsaturated hydrocarbon includes any one of acetylene, ethylene, propyne and butyne. Wherein, under positive pressure and low temperature, the unsaturated hydrocarbon is used to form Si-CH- chemical bonds with the hydrocarbon, and the low-temperature passivation avoids the growth of silicon grains and reduces the expansion of the composite material.
[0039] In a second aspect, the present invention further provides a fibrous silicon-carbon composite material, which is prepared by the above-mentioned preparation method of the fibrous silicon-carbon composite material.
[0040] In a third aspect, the present invention further provides a lithium-ion battery, which comprises the fibrous silicon-carbon composite material provided by the present invention as a negative electrode material of the battery.
[0041] The technical solution of the present invention is further illustrated by the following examples.
[0042] Embodiment 1,
[0043] 3g of phenyl lithium, 3g of γ-mercaptopropyl triethoxysilane and 3g of oxalic acid were added to 1000g of tetrahydrofuran organic solvent to form a mixed solution, and then 100g of carbon fiber was added to disperse evenly and transferred to a high-pressure reactor. Among them, the length of the carbon fiber is 50μm, the diameter is 5μm, and the wall thickness is 200nm. The mixed solution was hydrothermally reacted for 3h at a temperature of 150°C and a pressure of 8Mpa, filtered, and the resulting filter residue was freeze-dried at -40°C for 24h. The dried material was transferred to a tubular furnace, heated to 700°C, and water vapor gas was introduced at a flow rate of 300ml / min. It was introduced for 300min to form pores to obtain lithium-doped porous carbon fibers.
[0044] The lithium-doped porous carbon fibers were transferred to a fluidized bed, heated to 350°C, and introduced with monosilane gas at a flow rate of 300 ml / min. The cavity pressure was maintained at 0.3 MPa for deposition for 150 min. Then, the introduction of monosilane gas was stopped and replaced with acetylene gas. The temperature was raised to 450°C and the pressure was 8 MPa for low-temperature surface passivation treatment for 150 min to obtain a fibrous silicon-carbon composite material.
[0045] Embodiment 2,
[0046] 1g of methyl lithium, 1g of γ-aminopropyltriethoxysilane and 1g of citric acid were added to 500g of cyclohexane organic solvent to form a mixed solution, and then 100g of carbon fiber was added and dispersed evenly, and transferred to a high-pressure reactor. The length of the carbon fiber is 10μmμm, the diameter of the carbon fiber is 1μm, and the wall thickness of the carbon fiber is 50nm. The mixed solution was hydrothermally reacted at a temperature of 100°C and a pressure of 5Mpa for 6h, filtered, and the resulting filter residue was freeze-dried at -40°C for 24h. The dried material was transferred to a tubular furnace, heated to 500°C, and carbon dioxide activation gas was introduced at a flow rate of 100ml / min. It was introduced for 600min to form pores to obtain lithium-doped porous carbon fibers.
[0047] The lithium-doped porous carbon fibers were transferred to a fluidized bed, heated to 300°C, and introduced with monosilane gas at a flow rate of 100 ml / min. The cavity pressure was maintained at 0.1 MPa for deposition for 300 min. Then, the introduction of monosilane gas was stopped and replaced with unsaturated ethylene gas. The temperature was raised to 400°C and the pressure was 10 MPa for low-temperature surface passivation treatment for 300 min to obtain a fibrous silicon-carbon composite material.
[0048] Embodiment 3,
[0049] 5g of n-butyl lithium, 5g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and 5g of diethylaminetetraacetic acid were added to 2000g of N, N-dimethylacetamide organic solvent to form a solution, and then 100g of carbon fiber was added to disperse evenly and transferred to a high-pressure reactor. Among them, the length of the carbon fiber is 100μm, the diameter of the carbon fiber is 10μm, and the wall thickness of the carbon fiber is 500nm. The mixed solution was hydrothermally reacted for 6h at a temperature of 200°C and a pressure of 10Mpa, filtered, and the resulting filter residue was freeze-dried at -40°C for 24h. The dried material was transferred to a tubular furnace, heated to 800°C, and carbon dioxide activated gas was introduced at a flow rate of 500ml / min. It was introduced for 60min to form pores to obtain lithium-doped porous carbon fibers.
[0050] The lithium-doped porous carbon fibers were transferred to a fluidized bed, heated to 400°C, and introduced with monosilane gas at a flow rate of 500 ml / min. The cavity pressure was maintained at 0.5 MPa for deposition for 30 min. Then, the introduction of monosilane gas was stopped and replaced with propyne gas. The temperature was raised to 500°C and the pressure was 5 MPa for low-temperature surface passivation treatment for 30 min to obtain a fibrous silicon-carbon composite material.
[0051] Comparative Example 1
[0052] The difference from Example 1 is that the carbon fiber in step S1 is changed to porous carbon, and the rest is the same as Example 1.
[0053] Comparative Example 2
[0054] The difference from Example 1 is that phenyl lithium and oxalic acid are not added in step S1, and the rest is the same as Example 1.
[0055] (1) Physical and chemical properties test
[0056] The specific surface area, particle size, and tap density of the fibrous silicon-carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-2 were tested in accordance with GB / T 38823-2020 "Silicon Carbon", and the powder resistivity was tested using a four-probe tester (model 4200A-SCS). The silicon grain size was tested and calculated by XRD, and the test results are shown in Table 1 below.
[0057] Table 1. Physical and chemical properties test results of each group of materials
[0058]
[0059] Comparison between Example 1 and Comparative Example 1 shows that the resistivity of the powder is significantly reduced by using carbon fiber compared with porous carbon, and the lower temperature during the preparation process makes the silicon grains smaller. Comparison between Example 1 and Comparative Example 2 shows that lithium-doped porous carbon fibers obtained by adding phenyl lithium and oxalic acid for lithium doping reduce the resistivity of the powder.
[0060] (2) Button battery test
[0061] The fibrous silicon-carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-2 were used as negative electrode materials for lithium-ion batteries, and button batteries were prepared as follows: binder PVDF, conductive carbon black, and solvent NMP (the mass volume ratio of the silicon-carbon composite material to the binder, conductive agent, and solvent was 95g:1g:4g:220mL) were added to each silicon-carbon composite material, stirred to make a slurry, coated on a copper foil, dried, and rolled to obtain a negative electrode sheet, and each negative electrode sheet was respectively assembled with an electrolyte (1 mol / L LiPF6, a solvent mixed with EC and DEC in a volume ratio of 1:1), a counter electrode (metal lithium sheet), and a diaphragm (polypropylene film) in an argon-filled glove box to obtain a button battery. The button batteries were subjected to the following performance tests:
[0062] ① First discharge specific capacity and first efficiency: The first discharge specific capacity and first efficiency are tested using a battery tester, where the charge and discharge voltage range is 0.005-2V and the charge and discharge rate is 0.1C; at the same time, the second week of charging DCR (50% SOC) is tested.
[0063] ② Full charge expansion rate: Test the thickness D1 of the negative electrode sheet of the button battery after rolling, then fully charge the button battery to 100% SOC and dissect the full charge thickness D2 of the negative electrode sheet, and calculate the full charge expansion rate by the following formula:
[0064] Full charge expansion rate (%) = (D2-D1) / D1×100.
[0065] The test results are shown in Table 2 below.
[0066] Table 2. Button cell test results for each group of materials
[0067]
[0068] Comparison between Example 1 and Comparative Example 1 shows that the lithium-doped carbon fiber material reduces full charge expansion and charging DCR, reduces polarization, and improves the specific capacity of the material by relying on the high strength and low impedance of the carbon fiber itself. Compared with Comparative Example 2, Example 1 does not perform lithium doping, resulting in a larger powder resistivity, reducing the specific capacity of the material and reducing the initial efficiency.
[0069] (3) Soft pack performance test
[0070] The fibrous silicon-carbon composite material prepared in Example 1-3 and Comparative Example 1-2 was doped with 95 wt% of artificial graphite as the negative electrode plate, and the positive electrode ternary material LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, electrolyte (1.1 mol / L LiPF6, solvent is a mixture of EC and DEC with a volume ratio of 1:1) and diaphragm (celegard 2400) are assembled into a 5Ah soft pack battery, and the following performance tests are performed on the soft pack battery:
[0071] ① Liquid absorption capacity test: Use a 1mL burette to absorb 1mL of electrolyte, add one drop on the surface of the negative electrode, and time it until the electrolyte is completely absorbed, and record the time t;
[0072] ②Rate performance: Test the constant current ratio under 2C conditions (constant current ratio = 2C constant current capacity / (2C constant current capacity + 0.1C constant voltage capacity));
[0073] ③ Cycle performance: The test conditions are: charge and discharge voltage range is 2.5~4.2V, temperature is 25±3.0℃, charge and discharge rate is 1.0C / 1.0C, and the number of cycles is 500 times.
[0074] The test results are shown in Table 3 below.
[0075] Table 3. Soft pack performance test results of each group of materials
[0076]
[0077] in, Figure 2 3 is a graph showing the cycle performance test results when the fibrous silicon-carbon composite material in Example 1 and Comparative Example 1 is used as the negative electrode material. Figure 2 It can be seen that the comparison between Example 1 and Comparative Example 1 shows that the example material has low full-charge expansion and low powder resistivity, which can improve the cycle performance and fast charging performance. The comparison between Example 1 and Comparative Example 2 shows that magnesium doping in the material reduces impedance and improves fast charging performance, and the high specific surface area improves the material's liquid absorption and retention performance and improves the cycle performance.
[0078] In summary, the preparation method of the fibrous silicon-carbon composite material provided by the present invention improves the electronic conductivity and the initial efficiency of the material by doping metallic lithium into the carbon fiber; forms a three-dimensional network structure of the carbon fiber through a silane coupling agent, thereby improving the electronic conductivity between the materials and reducing the expansion; increases the pores of the lithium-doped carbon fiber composite material by adding an organic acid pore-forming agent, so that it can accommodate more lithium ions and improve the specific capacity of the silicon-carbon composite material; decomposes monosilane gas through negative pressure deposition, so that nano-silicon is easily deposited in the porous carbon and passivated under positive pressure; introduces monosilane gas to negatively deposit nano-silicon under negative pressure, and Nano-silicon is deposited in porous carbon fibers by a silane cracking method, so that the nano-silicon is more easily deposited in the internal pores. Under positive pressure conditions, amorphous carbon is deposited on the surface of the porous carbon fibers to improve the quality of Si-CH deposition, so that the carbon materials have the characteristics of high density and the like. Positive pressure and low-temperature surface passivation are performed by introducing unsaturated hydrocarbons, and the growth of silicon grains is avoided by low-temperature passivation, and expansion is reduced to obtain a fibrous silicon-carbon composite material. The fibrous silicon-carbon composite material and lithium-ion battery obtained by the preparation method provided by the present invention can reduce expansion and improve the electronic or ionic conductivity of the material, while increasing the rate and improving the cycle performance.
[0079] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a fibrous silicon-carbon composite material, characterized in that: The specific steps include: S1, adding an organic lithium salt, a silane coupling agent and an organic acid pore-forming agent to an organic solvent to prepare a solution, and adding carbon fiber to disperse evenly to obtain a mixed solution; S2, subjecting the mixed solution to a hydrothermal reaction at a temperature of 100-200° C. and a pressure of 5-10 MPa for 1-6 h, filtering and freeze-drying; S3, transferring the dried material to a tubular furnace, introducing an activated gas to form pores after heating, and obtaining lithium-doped porous carbon fibers; S4, transferring the lithium-doped porous carbon fiber to a fluidized bed, introducing monosilane gas to perform negative pressure deposition of nano-silicon; S5. After the silicon deposition reaction is completed, the introduction of monosilane gas is stopped, and unsaturated hydrocarbons are introduced to perform positive pressure and low temperature surface passivation to obtain a fibrous silicon-carbon composite material.
2. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S1, raw materials are provided according to the mass ratio of organic lithium salt: silane coupling agent: organic acid pore-forming agent: organic solvent: carbon fiber = (1-5): (1-5): (1-5): (500-2000):
100.
3. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S1, the organic lithium salt includes any one of phenyl lithium, methyl lithium, n-butyl lithium and tert-butyl lithium diisopropylamide or a combination thereof; the silane coupling agent includes any one of γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane or a combination thereof; the organic acid pore-forming agent includes any one of oxalic acid, citric acid, diethylaminetetraacetic acid and lactic acid or a combination thereof; the organic solvent includes any one of tetrahydrofuran, cyclohexane, tetrachloromethane and N,N-dimethylacetamide or a combination thereof.
4. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S1, the length of the carbon fiber is 10-100 μm, the diameter of the carbon fiber is 1-10 μm, and the wall thickness of the carbon fiber is 50-500 nm.
5. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S2, the freeze drying is performed at -40°C for 24 hours; in S3, the activated gas is introduced when the temperature is raised to 500-800°C, the flow rate of the activated gas is 100-500 ml / min, and the pore making time is 60-600 min.
6. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S4, the temperature needs to be raised to 300-400°C before introducing monosilane gas, the flow rate of the monosilane gas is 100-500 ml / min, the pressure of the cavity during silicon deposition is 0.1-0.5 MPa, and the silicon deposition time is 30-300 min.
7. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S4, the activation gas is carbon dioxide or water vapor; in S5, the unsaturated hydrocarbon includes any one of acetylene, ethylene, propyne and butyne.
8. The method for preparing the fibrous silicon-carbon composite material according to claim 1, characterized in that: In S5, the surface low-temperature passivation time is 30~300min, and the passivation reaction pressure is 5~10Mpa.
9. A fibrous silicon-carbon composite material, characterized in that: The fibrous silicon-carbon composite material is prepared by the preparation method of any one of claims 1 to 8.