A high-toughness optoelectronic composite cable and preparation method thereof
By adopting multi-layer structure and specific polymerization reaction in the optical cable, the tensile strength and compressive performance of the photoelectric composite cable are enhanced, the problem of unstable transmission performance in harsh environments is solved, and high-strength and high-strength optical cables are realized design.
Patent Information
- Application Number
- CN202411052490.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The transmission performance of existing optical cables is unstable in harsh environments, and the tensile strength and compressive performance are insufficient, making it difficult to withstand external force damage, affecting the stable operation of the communication system.
Using structures such as outer protective layer, waterproof layer, flame retardant layer, metal shield layer and elastic filling resin, a dense coating layer is formed through the action of carboxymethyl chitosan and coupling agent, and 4-hydroxystyrene and cashew nuts are used. Phenol polymerization enhances the tensile strength and elongation of breaking of composite materials.
It significantly improves the high strength and toughness of the photoelectric composite cable, ensuring the stability of transmission performance and the reliability of the communication system in harsh environments.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic composite cables and relates to a high-toughness optoelectronic composite cable and a preparation method thereof. Background Art
[0002] Optical cable is an integrated transmission medium that organically combines metal wires and optical fibers to transmit electrical energy and optical information at the same time, on the same route, and in the same direction. It realizes the integrated fusion of power flow, business flow, and information flow. During use, optical cables may face challenges in harsh environments, such as high temperature, low temperature, and humidity changes. High-toughness optical cables can maintain stable transmission performance under these conditions to ensure communication quality. In addition, high-toughness optical cables need to have good tensile strength and compressive resistance, be able to resist external damage, and extend their service life. In practical applications, such as subways, tunnels, overhead and other scenarios, high-toughness optical cables can adapt to various complex environments and ensure the stable operation of communication systems. Summary of the invention
[0003] The purpose of the present invention is to provide a high-toughness optoelectronic composite cable and a preparation method thereof, wherein the prepared optoelectronic composite cable has the characteristics of high strength and high toughness.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A high-toughness optoelectronic composite cable comprises an outer protective layer, a waterproof layer and several groups of cables. The outer protective layer is arranged on the outer wall of the waterproof layer, the outer diameter of the waterproof layer matches the inner diameter of the outer protective layer, and several groups of cables are arranged inside the waterproof layer.
[0006] As a preferred technical solution of the present invention, a flame retardant layer and a metal shielding layer are sequentially provided on the inner wall of the waterproof layer, the flame retardant layer covers the metal shielding layer, the metal shielding layer covers several groups of the cables, and an elastic filling resin is provided between the cables and the metal shielding layer.
[0007] As a preferred technical solution of the present invention, the outer protective layer comprises the following components by weight: 95-100 parts of polypropylene, 16-20 parts of polyamide fiber, 15-18 parts of modified silicon carbide, 1.5-2 parts of antioxidant, 7-10 parts of compatibilizer, 4-6 parts of lubricant and 0-1 part of additive.
[0008] As a preferred technical solution of the present invention, the compatibilizer is one or both of maleic anhydride grafted PP and maleic anhydride grafted POE.
[0009] As a preferred technical solution of the present invention, the antioxidant is one or more of antioxidant 168, antioxidant 1010 and antioxidant 1098.
[0010] As a preferred technical solution of the present invention, the lubricant is one or more of PP wax, calcium stearate and paraffin.
[0011] As a preferred technical solution of the present invention, the auxiliary agent is prepared by mixing the light stabilizer UV-9 and the heat stabilizer DLTP in a mass ratio of (2-4): (3-5).
[0012] As a preferred technical solution of the present invention, the preparation method of the modified silicon carbide comprises the following steps:
[0013] 1) mixing silicon carbide powder, a dispersant and a carboxymethyl chitosan solution, grinding and drying to obtain a composite powder;
[0014] 2) After the ethanol solution and the coupling agent are stirred and mixed, the composite powder is added, heated and stirred, and then dried, placed in a tube furnace for sintering, and then ground after cooling to room temperature to obtain prefabricated silicon carbide;
[0015] 3) After ultrasonically mixing the prefabricated silicon carbide and anhydrous ethanol, 4-hydroxystyrene, cardanol and an initiator are added, heated and stirred, and then filtered, washed and dried to obtain modified silicon carbide.
[0016] As a preferred technical solution of the present invention, in step 1), the grinding is performed at 300-400 r / min for 2-3 h; and the drying is performed at 70° C. for 10-12 h.
[0017] As a preferred technical solution of the present invention, in step 1), the mass ratio of the silicon carbide powder, the dispersant and the carboxymethyl chitosan solution is (25-26): (0.8-1.0): (40-45); the carboxymethyl chitosan solution is prepared by mixing carboxymethyl chitosan and deionized water in a mass ratio of (1.0-1.2): 35; and the dispersant is triethanolamine.
[0018] As a preferred technical solution of the present invention, in step 2), the stirring and mixing time is 30-45 minutes; the heating and stirring is at 50-60°C and stirring for 3-4 hours; and the sintering is at 460-500°C and heat preservation for 4-5 hours.
[0019] As a preferred technical solution of the present invention, in step 2), the usage ratio of the ethanol solution, the coupling agent and the composite powder is 300mL: (3.0-4.0)g: 50g; the coupling agent is aluminum zirconium coupling agent LD-139; and the mass fraction of the ethanol solution is 65%.
[0020] As a preferred technical solution of the present invention, in step 3), the ultrasonic mixing is performed at 150-200W for 8-10 minutes; the heating stirring is performed at 500-600r / min and 80°C for 5-6 hours; the washing is performed with anhydrous ethanol; and the drying is performed to constant weight.
[0021] As a preferred technical solution of the present invention, in step 3), the mass ratio of the prefabricated silicon carbide, anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator is 20: (3-4): (1.6-2.0): (0.1-0.12); the initiator is one or two of azobisisobutyronitrile and azobisisoheptanenitrile.
[0022] As a preferred technical solution of the present invention, the preparation method of the outer protective layer includes the following steps: weighing each raw material by weight and mixing them, kneading each raw material for 15-20 minutes at 160-170°C, then placing it in a twin-screw extruder, and melt-extruding it at a temperature of 180-200°C to obtain the outer protective layer.
[0023] A method for preparing a high-toughness optoelectronic composite cable comprises the following steps: bundling a plurality of optical cables to form a plurality of cable groups, arranging the plurality of cable groups and elastic filling resin, and then sequentially coating them with a metal shielding layer, a flame retardant layer, a waterproof layer and an outer protective layer to obtain the cable.
[0024] Beneficial effects of the present invention:
[0025] The present invention utilizes the effect of carboxymethyl chitosan and a coupling agent, so that the coupling agent is bonded to the surface of silicon carbide and sintered to form a dense coating layer, and utilizes the polymerization reaction of 4-hydroxystyrene and cardanol to introduce organic groups and carbon-carbon double bonds, thereby significantly enhancing the tensile strength and elongation at break of the composite material. The high-toughness optical-electrical composite cable prepared by the present invention has excellent high-strength and high-toughness characteristics. DETAILED DESCRIPTION
[0026] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments. Example 1
[0027] A high-toughness optoelectronic composite cable, comprising an outer protective layer, a waterproof layer and a plurality of groups of cables, wherein the outer protective layer is arranged on the outer wall of the waterproof layer, the outer diameter of the waterproof layer matches the inner diameter of the outer protective layer, and a plurality of groups of cables are arranged inside the waterproof layer; a flame retardant layer and a metal shielding layer are arranged on the inner wall of the waterproof layer in sequence, the flame retardant layer covers the metal shielding layer, the metal shielding layer covers a plurality of groups of cables, and an elastic filling resin is arranged between the cable and the metal shielding layer;
[0028] A preparation method of a high-toughness optoelectronic composite cable comprises the following steps: bundling a number of optical cables to form a number of cable groups, arranging the several cable groups and elastic filling resin, and then coating them with a metal shielding layer, a flame retardant layer, a waterproof layer and an outer protective layer in sequence to obtain the cable.
[0029] The outer protective layer comprises the following components by weight: 95 parts of polypropylene, 16 parts of polyamide fiber, 15 parts of modified silicon carbide, 1.5 parts of antioxidant, 7 parts of compatibilizer and 4 parts of lubricant;
[0030] The compatibilizer is a mixture of maleic anhydride grafted PP and maleic anhydride grafted POE in a mass ratio of 2:1; the antioxidant is antioxidant 1010; and the lubricant is paraffin;
[0031] The preparation method of the modified silicon carbide comprises the following steps:
[0032] 1) mixing silicon carbide powder, a dispersant and a carboxymethyl chitosan solution, grinding and drying to obtain a composite powder;
[0033] In step 1), the grinding is performed at 300 r / min for 2 hours; the drying is performed at 70° C. for 10 hours; the mass ratio of the silicon carbide powder, the dispersant and the carboxymethyl chitosan solution is 25:0.8:40; the carboxymethyl chitosan solution is prepared by mixing carboxymethyl chitosan and deionized water at a mass ratio of 1.0:35; the dispersant is triethanolamine;
[0034] 2) After the ethanol solution and the coupling agent are stirred and mixed, the composite powder is added, heated and stirred, and then dried, placed in a tube furnace for sintering, and then ground after cooling to room temperature to obtain prefabricated silicon carbide;
[0035] In step 2), the stirring and mixing time is 30 minutes; the heating and stirring is at 50°C and stirring for 3 hours; the sintering is at 460°C and heat preservation for 4 hours; the amount ratio of the ethanol solution, the coupling agent and the composite powder is 300mL:3.0g:50g; the coupling agent is aluminum zirconium coupling agent LD-139; the mass fraction of the ethanol solution is 65%, and the solvent is deionized water;
[0036] 3) After ultrasonically mixing the prefabricated silicon carbide and anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator are added, heated and stirred, filtered, washed and dried to obtain modified silicon carbide;
[0037] In step 3), the ultrasonic mixing is performed at 150 W for 8 minutes; the heating stirring is performed at 500 r / min and 80° C. for 5 hours; the washing is performed with anhydrous ethanol; the drying is performed to constant weight; the mass ratio of the prefabricated silicon carbide, anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator is 20:3:1.6:0.1; and the initiator is azobisisobutyronitrile.
[0038] The preparation method of the outer protective layer comprises the following steps: weighing each raw material by weight and mixing them, kneading each raw material at 160° C. for 15 minutes, then placing them in a twin-screw extruder and performing melt extrusion at 180° C. to obtain the outer protective layer. Example 2
[0039] A high-toughness optoelectronic composite cable, comprising an outer protective layer, a waterproof layer and a plurality of groups of cables, wherein the outer protective layer is arranged on the outer wall of the waterproof layer, the outer diameter of the waterproof layer matches the inner diameter of the outer protective layer, and a plurality of groups of cables are arranged inside the waterproof layer; a flame retardant layer and a metal shielding layer are arranged on the inner wall of the waterproof layer in sequence, the flame retardant layer covers the metal shielding layer, the metal shielding layer covers a plurality of groups of cables, and an elastic filling resin is arranged between the cable and the metal shielding layer;
[0040] A preparation method of a high-toughness optoelectronic composite cable comprises the following steps: bundling a number of optical cables to form a number of cable groups, arranging the several cable groups and elastic filling resin, and then coating them with a metal shielding layer, a flame retardant layer, a waterproof layer and an outer protective layer in sequence to obtain the cable.
[0041] The outer protective layer comprises the following components by weight: 98 parts of polypropylene, 18 parts of polyamide fiber, 16 parts of modified silicon carbide, 1.8 parts of antioxidant, 8 parts of compatibilizer, 5 parts of lubricant and 0.5 parts of auxiliary agent;
[0042] The compatibilizer is a mixture of maleic anhydride grafted PP and maleic anhydride grafted POE in a mass ratio of 2:1; the antioxidant is antioxidant 1010; and the lubricant is paraffin;
[0043] The auxiliary agent is a mixture of light stabilizer UV-9 and heat stabilizer DLTP in a mass ratio of 3:4;
[0044] The preparation method of the modified silicon carbide comprises the following steps:
[0045] 1) mixing silicon carbide powder, a dispersant and a carboxymethyl chitosan solution, grinding and drying to obtain a composite powder;
[0046] In step 1), the grinding is performed at 350 r / min for 2.5 h; the drying is performed at 70° C. for 11 h; the mass ratio of the silicon carbide powder, the dispersant and the carboxymethyl chitosan solution is 25.5:0.9:42; the carboxymethyl chitosan solution is prepared by mixing carboxymethyl chitosan and deionized water at a mass ratio of 1.1:35; the dispersant is triethanolamine;
[0047] 2) After the ethanol solution and the coupling agent are stirred and mixed, the composite powder is added, heated and stirred, and then dried, placed in a tube furnace for sintering, and then ground after cooling to room temperature to obtain prefabricated silicon carbide;
[0048] In step 2), the stirring and mixing time is 38 minutes; the heating and stirring is at 55°C and stirring for 3.5 hours; the sintering is at 480°C and heat preservation for 4.5 hours; the amount ratio of the ethanol solution, coupling agent and composite powder is 300mL:3.5g:50g; the coupling agent is aluminum zirconium coupling agent LD-139; the mass fraction of the ethanol solution is 65%, and the solvent is deionized water;
[0049] 3) After ultrasonically mixing the prefabricated silicon carbide and anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator are added, heated and stirred, filtered, washed and dried to obtain modified silicon carbide;
[0050] In step 3), the ultrasonic mixing is performed at 175 W for 9 minutes; the heating stirring is performed at 550 r / min and 80° C. for 5.5 hours; the washing is performed with anhydrous ethanol; the drying is performed to constant weight; the mass ratio of the prefabricated silicon carbide, anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator is 20:3.5:1.8:0.11; and the initiator is azobisisobutyronitrile.
[0051] The preparation method of the outer protective layer comprises the following steps: weighing each raw material by weight and mixing them, kneading each raw material at 165° C. for 18 minutes, then placing it in a twin-screw extruder and melt-extruding it at 190° C. to obtain the outer protective layer. Example 3
[0052] A high-toughness optoelectronic composite cable, comprising an outer protective layer, a waterproof layer and a plurality of groups of cables, wherein the outer protective layer is arranged on the outer wall of the waterproof layer, the outer diameter of the waterproof layer matches the inner diameter of the outer protective layer, and a plurality of groups of cables are arranged inside the waterproof layer; a flame retardant layer and a metal shielding layer are arranged on the inner wall of the waterproof layer in sequence, the flame retardant layer covers the metal shielding layer, the metal shielding layer covers a plurality of groups of cables, and an elastic filling resin is arranged between the cable and the metal shielding layer;
[0053] A preparation method of a high-toughness optoelectronic composite cable comprises the following steps: bundling a number of optical cables to form a number of cable groups, arranging the several cable groups and elastic filling resin, and then coating them with a metal shielding layer, a flame retardant layer, a waterproof layer and an outer protective layer in sequence to obtain the cable.
[0054] The outer protective layer comprises the following components by weight: 100 parts of polypropylene, 20 parts of polyamide fiber, 18 parts of modified silicon carbide, 2 parts of antioxidant, 10 parts of compatibilizer, 6 parts of lubricant and 1 part of auxiliary agent;
[0055] The compatibilizer is a mixture of maleic anhydride grafted PP and maleic anhydride grafted POE in a mass ratio of 2:1; the antioxidant is antioxidant 1010; and the lubricant is paraffin;
[0056] The auxiliary agent is a mixture of light stabilizer UV-9 and heat stabilizer DLTP in a mass ratio of 4:5;
[0057] The preparation method of the modified silicon carbide comprises the following steps:
[0058] 1) mixing silicon carbide powder, a dispersant and a carboxymethyl chitosan solution, grinding and drying to obtain a composite powder;
[0059] In step 1), the grinding is performed at 400 r / min for 3 hours; the drying is performed at 70° C. for 12 hours; the mass ratio of the silicon carbide powder, the dispersant and the carboxymethyl chitosan solution is 26:1.0:45; the carboxymethyl chitosan solution is prepared by mixing carboxymethyl chitosan and deionized water at a mass ratio of 1.2:35; the dispersant is triethanolamine;
[0060] 2) After the ethanol solution and the coupling agent are stirred and mixed, the composite powder is added, heated and stirred, and then dried, placed in a tube furnace for sintering, and then ground after cooling to room temperature to obtain prefabricated silicon carbide;
[0061] In step 2), the stirring and mixing time is 45 minutes; the heating and stirring is at 60°C and stirring for 4 hours; the sintering is at 500°C and heat preservation for 5 hours; the amount ratio of the ethanol solution, the coupling agent and the composite powder is 300mL:4.0g:50g; the coupling agent is aluminum zirconium coupling agent LD-139; the mass fraction of the ethanol solution is 65%, and the solvent is deionized water;
[0062] 3) After ultrasonically mixing the prefabricated silicon carbide and anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator are added, heated and stirred, filtered, washed and dried to obtain modified silicon carbide;
[0063] In step 3), the ultrasonic mixing is performed at 200 W for 10 minutes; the heating stirring is performed at 600 r / min and 80° C. for 6 hours; the washing is performed with anhydrous ethanol; the drying is performed to constant weight; the mass ratio of the prefabricated silicon carbide, anhydrous ethanol, 4-hydroxystyrene, cardanol and initiator is 20:4:2.0:0.12; and the initiator is azobisisobutyronitrile.
[0064] The preparation method of the outer protective layer comprises the following steps: weighing each raw material by weight and mixing them, kneading each raw material for 20 minutes at 170° C., then placing them in a twin-screw extruder and performing melt extrusion at 200° C. to obtain the outer protective layer.
[0065] Comparative Example 1
[0066] Compared with Example 2, the difference in Comparative Example 1 is that deionized water replaces the carboxymethyl chitosan solution, and the other components, preparation steps and parameters are the same.
[0067] Comparative Example 2
[0068] Compared with Example 2, Comparative Example 2 is different in that no coupling agent is used, and the remaining components, preparation steps and parameters are the same.
[0069] Comparative Example 3
[0070] Compared with Example 2, the difference in Comparative Example 3 is that 3-vinylphenol replaces cardanol, and the other components, preparation steps and parameters are the same.
[0071] Comparative Example 4
[0072] Compared with Example 2, Comparative Example 4 is different in that styrene replaces 4-hydroxystyrene, and the other components, preparation steps and parameters are the same.
[0073] Comparative Example 5
[0074] Compared with Example 2, the difference in Comparative Example 5 is that cardanol is not used, and the other components, preparation steps and parameters are the same.
[0075] The outer protective layers prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to the following tests, respectively, and the test results are shown in Table 1.
[0076] Tensile strength and elongation at break test: according to GB / T 2951.11-2008;
[0077] Table 1
[0078] Tensile strength (MPa) Elongation at break (%) Example 1 11.2 232 Example 2 11.7 239 Example 3 11.5 236 Comparative Example 1 10.0 188 Comparative Example 2 9.3 167 Comparative Example 3 8.2 149 Comparative Example 4 9.7 182 Comparative Example 5 7.8 134
[0079] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-5, the tensile strength and elongation at break of the outer protective layer prepared by the scheme of the present invention in Examples 1-3 are significantly better than those in Comparative Examples 1-5. This is because the present invention utilizes the hydrogen bond and electrostatic adsorption between carboxymethyl chitosan and the coupling agent to enhance the bonding force between silicon carbide and the coupling agent, which is beneficial to cover a dense metal oxide coating layer on the edge of the silicon carbide surface in the later stage, and obtain more metal oxides, and then bond to the surface of silicon carbide through the coupling agent, and after sintering, the aluminum oxide / zirconium oxide compound is evenly dispersed on the surface of silicon carbide. Since aluminum oxide / zirconium oxide is formed by in-situ reaction on the surface of silicon carbide, each phase interface is pure, and the phases are tightly combined, which significantly improves the stability, tensile strength and elongation at break of the composite material; then, 4-hydroxystyrene and cardanol contain thiol and hydroxyl groups, and the coverage rate of prefabricated silicon carbide is improved through hydrogen bonding and adsorption, more organic groups and carbon-carbon double bonds are introduced, and the compatibility and dispersibility of prefabricated silicon carbide in the system are increased. Combined with the long carbon chain on cardanol, the fluidity of the reaction monomer is improved, and the tensile strength and elongation at break of the composite material are further enhanced. In summary, the high-toughness optoelectronic composite cable prepared by the present invention has the characteristics of excellent high strength and high toughness.
[0080] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A high-toughness optoelectronic composite cable, It is characterized in that The high-toughness optoelectronic composite cable comprises an outer protective layer, a waterproof layer and several groups of cables, wherein the outer protective layer is arranged on the outer wall of the waterproof layer, the outer diameter of the waterproof layer matches the inner diameter of the outer protective layer, and several groups of cables are arranged inside the waterproof layer, and the outer protective layer comprises the following components by weight: 95-100 parts of polypropylene, 16-20 parts of polyamide fiber, 15-18 parts of modified silicon carbide, 1.5-2 parts of antioxidant, 7-10 parts of compatibilizer, 4-6 parts of lubricant and 0-1 part of auxiliary agent; wherein the preparation method of the modified silicon carbide comprises the following steps: 1) Silicon carbide powder, a dispersant and a carboxymethyl chitosan solution are mixed, ground and dried to obtain a composite powder; the mass ratio of the silicon carbide powder, the dispersant and the carboxymethyl chitosan solution is (25-26): (0.8-1.0): (40-45); the dispersant is triethanolamine; 2) After the ethanol solution and the coupling agent are stirred and mixed, the composite powder is added, heated and stirred, and then dried, placed in a tube furnace for sintering, and ground after cooling to room temperature to obtain prefabricated silicon carbide; the amount ratio of the ethanol solution, the coupling agent and the composite powder is 300mL: (3.0-4.0)g: 50g; the coupling agent is aluminum zirconium coupling agent LD-139; 3) After ultrasonically mixing the prefabricated silicon carbide and anhydrous ethanol, 4-hydroxystyrene, cardanol and an initiator are added, heated and stirred, and then filtered, washed and dried to obtain modified silicon carbide.
2. A high-toughness optoelectronic composite cable according to claim 1, Features: A flame retardant layer and a metal shielding layer are arranged in sequence on the inner wall of the waterproof layer, the flame retardant layer covers the metal shielding layer, the metal shielding layer covers a plurality of groups of the cables, and an elastic filling resin is arranged between the cables and the metal shielding layer.
3. A high-toughness optoelectronic composite cable according to claim 1, Features: The compatibilizer is one or two of maleic anhydride grafted PP and maleic anhydride grafted POE; the antioxidant is one or more of antioxidant 168, antioxidant 1010 and antioxidant 1098; the lubricant is one or more of PP wax, calcium stearate and paraffin; the auxiliary agent is a mixture of light stabilizer UV-9 and heat stabilizer DLTP in a mass ratio of (2-4): (3-5).
4. A high-toughness optoelectronic composite cable according to claim 1, Features: In step 1), the grinding is performed at 300-400 r / min for 2-3 h; and the drying is performed at 70° C. for 10-12 h.
5. The high-toughness optoelectronic composite cable according to claim 1, Features: In step 1), the carboxymethyl chitosan solution is prepared by mixing carboxymethyl chitosan and deionized water in a mass ratio of (1.0-1.2):
35.
6. A high-toughness optoelectronic composite cable according to claim 1, Features: In step 2), the stirring and mixing time is 30-45 minutes; the heating and stirring is at 50-60° C. and stirring for 3-4 hours; and the sintering is at 460-500° C. and heat preservation for 4-5 hours.
7. The high-toughness optoelectronic composite cable according to claim 1, Features: In step 2), the mass fraction of the ethanol solution is 65%.
8. The high-toughness optoelectronic composite cable according to claim 1, Features: In step 3), the ultrasonic mixing is performed at 150-200W for 8-10 minutes; the heating stirring is performed at 500-600r / min and 80°C for 5-6 hours; the washing is performed with anhydrous ethanol; the drying is performed to constant weight; and the initiator is one or both of azobisisobutyronitrile and azobisisoheptanenitrile.
9. The high-toughness optoelectronic composite cable according to claim 1, It is characterized in that The preparation method of the outer protective layer comprises the following steps: weighing each raw material by weight, mixing each raw material for 15-20 minutes at 160-170° C., then placing it in a twin-screw extruder, and melt-extruding it at a temperature of 180-200° C. to obtain the outer protective layer.
10. A method for preparing a high-toughness optoelectronic composite cable according to any one of claims 1 to 9, It is characterized in that The preparation method comprises the following steps: bundling a plurality of optical cables to form a plurality of cable groups, arranging the plurality of cable groups and elastic filling resin, and then coating them with a metal shielding layer, a flame retardant layer, a waterproof layer and an outer protective layer in sequence to obtain the optical cable.