Preparation method of biaxially oriented film of highly isotactic narrow molecular weight distribution polypropylene resin

Through the processes of multi-region temperature control, inert gas protection, multi-point electrical bolt regulation, multi-stage stretching and high-temperature wide rail spacing, the poor film formation problem of high-grade narrow molecular weight distribution polypropylene resin is solved, and the crystallinity of the film is improved and breakdown field strength, achieving film preparation with better performance than traditional processes.

CN118578701BActive Publication Date: 2024-12-03CHINA ELECTRIC POWER RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073917.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-03
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a stable film pulling of a high-gauged narrow molecular weight distribution polypropylene resin, resulting in poor film forming properties.

Method used

Extrusion process using multi-region temperature control and inert gas protection, casting process using multi-point electrical bolts to regulate casting thickness, longitudinal pulling process of high-speed multi-stage stretching and high-temperature setting, and cross-pull process of high-temperature wide rail spacing , combined with optimized process parameters to prepare a bidirectional tensile film of high-coagular narrow molecular weight distribution.

Benefits of technology

The crystallinity, breakdown field strength and mechanical properties of the film are improved, and the film formation difficulties in the resin film making process of narrow molecular weight distribution is solved, and film preparation with better performance than traditional processes is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118578701B_ABST
    Figure CN118578701B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of plastic molding. The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin. The method includes an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process: the extrusion process includes multi-region temperature control and inert gas protection; the sheet casting process includes using multi-point electrical bolts to adjust the thickness of the sheet; the longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping; the transverse stretching process includes using high-temperature wide guide rail spacing for transverse stretching shaping. The present invention achieves stable film drawing of a high isotactic narrow molecular weight distribution polypropylene resin less than 4.5 by adjusting the extrusion and biaxial stretching processes. The biaxially stretched polypropylene film (BOPP) has an ultra-thin thickness (<5μm) and excellent high-temperature insulation. The present invention broadens the application of high isotactic narrow molecular weight distribution polypropylene resin in the field of high-voltage direct current transmission and new energy film dielectric materials, and achieves effective substitution of traditional polypropylene films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plastic molding, and in particular relates to a method for preparing a biaxially stretched film of a highly isotactic narrow molecular weight distribution polypropylene resin. Background Art

[0002] High-performance film capacitors are widely used in new energy transportation, flexible DC transmission, medical treatment equipment, and electromagnetic pulse weapons. Biaxially oriented polypropylene resin film (BOPP) has become the preferred dielectric material for mid- and high-end film capacitors due to its excellent high-temperature (85°C) insulation and mechanical properties and stable processing film properties. As the manufacturing material of BOPP film, the physical and chemical properties of polypropylene resin (PP) determine the processing characteristics and application performance of BOPP film.

[0003] PP resins for film capacitors usually have extremely low ash content (<15ppm), high isotacticity (>99%), high weight-average molecular weight (Mw>350,000) and wide molecular weight distribution index (Mw / Mn=5-8). The isotacticity and molecular weight distribution of the resin have an important influence on the film-forming characteristics and physical and chemical properties of the film during processing. Generally, films prepared from resins with higher isotacticity and narrower molecular weight distribution have better mechanical and electrical properties. However, the preparation process of such films is very unstable. The high crystallinity of the resin makes it difficult to draw the film, and the film is easy to break during processing, which greatly reduces the yield rate. Therefore, in order to balance the contradiction between film performance and processing stability, the isotacticity and molecular weight of the resin are often finely controlled. By slightly reducing the isotacticity and increasing the molecular weight distribution, the proportion of high and low molecular weight molecules is controlled to obtain a film material with both processing stability and excellent electrical and mechanical properties. For example, patent CN101065411B believes that PP resins with Mw / Mn above 5, preferably above 6, Mz / Mn above 15, preferably above 20, and NMR isotactic 5-unit composition between 0.9-0.99 often have excellent film-forming and electrical properties. Patent CN101172392B shows that resins with Mw above 100,000 and below 500,000 and Mw / Mn above 5 and below 15 have excellent film-forming and electrical properties. Patent CN101848961B makes more detailed provisions for the molecular weight of electrical film-grade PP resins, that is, in the molecular weight distribution curve, the resin with a difference of more than 2% and less than 15% from the differential distribution value when the logarithmic molecular weight is 4.5 to the differential distribution value when the logarithmic molecular weight is 6 has the best comprehensive film-drawing performance. Similar patents include CN102356439B, CN106574092B, CN107406543A, CN107406644A, CN110139738B and CN117043241A.

[0004] The above results show that the existing technology cannot achieve stable film drawing of highly isotactic narrow molecular weight distribution polypropylene resin. Summary of the invention

[0005] The invention aims to solve the problem of poor film-forming property of the existing high isotactic narrow molecular weight distribution polypropylene resin under the biaxial stretching production process.

[0006] The purpose of the present invention is to adopt the following technical solutions to achieve:

[0007] A method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin comprises an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process:

[0008] The extrusion process includes multi-zone temperature control and inert gas protection;

[0009] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0010] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0011] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0012] Preferably, the molecular weight of the polypropylene resin satisfies the following characteristics:

[0013] Mw=350000—550000; Mn=80000—160000; 3.4≤Mw / Mn≤4.5.

[0014] Preferably, the polypropylene resin has an isotactic 5-unit component content of 97.5%-98.3% and an isotactic 3-unit component content of 99.2%-99.6% as measured by high-temperature liquid nuclear magnetic resonance.

[0015] Preferably, the inert gas includes one or a combination of nitrogen, argon and helium.

[0016] Preferably, the extrusion process comprises: adjusting the pipe pressure and die head pressure of the extruded resin melt by adjusting the rotation speed of the feeding metering pump.

[0017] Preferably, the extrusion process comprises: controlling the fluid width of the resin by adjusting a width-adjustable die.

[0018] Preferably, the sheet casting process comprises: the extruded resin melt is received by a quenching roller to form a sheet, and the thickness of the sheet is regulated by multi-point electrical bolts.

[0019] Preferably, the longitudinal drawing process comprises: sequentially using three process sections of longitudinal drawing preheating, longitudinal drawing stretching and longitudinal drawing shaping to draw the cast sheet to form a longitudinally drawn thick sheet, and each process section adopts multi-zone temperature control.

[0020] Preferably, the transverse stretching process includes: using three process stages of transverse stretching preheating, transverse stretching and transverse stretching shaping to transversely stretch the longitudinally drawn thick sheet to form a final film product; wherein the transverse stretching shaping adopts high temperature and wide guide rail spacing.

[0021] Preferably, the multi-zone temperature control of the extrusion process includes: the temperature control zones of the extruder from the feeding port to the extruder die head are zone one, zone two, zone three, zone four, zone five, zone six and zone seven in sequence; the temperature ranges are: zone one 210-250°C; zone two 240-265°C; zone three 240-265°C; zone four 240-265°C; zone five 240-265°C; zone six 240-265°C; zone seven 210-250°C.

[0022] Preferably, the overall extrusion line speed of the extrusion process is 180-260 m / min.

[0023] Preferably, the speed range of the feeding metering pump is 30-60 rpm.

[0024] Preferably, the pipeline pressure range is 20-40 bar.

[0025] Preferably, the die pressure ranges from 80 to 150 bar.

[0026] Preferably, the fluid width is 1.5m-1.8m, with a deviation of no more than ±0.1%.

[0027] Preferably, the temperature range of the chill roller is 70-100°C.

[0028] Preferably, the multi-point electrical bolts include: 50-100 electrical bolts distributed over the width of the casting, wherein the number of bolts in the edge area of ​​the casting is 20-40, and the bolt temperature is 230-250°C; the number of bolts in the central part of the casting is 30-60, and the bolt temperature is 210-240°C.

[0029] Preferably, the cast sheet enters the longitudinal drawing process under the action of a traction force, and the traction force ranges from 280 to 350N.

[0030] Preferably, the longitudinal drawing preheating is divided into 5-8 temperature control zones, and the zone temperature range is 120-133°C.

[0031] Preferably, the longitudinal stretching is divided into 3-6 temperature control zones, the zone temperature range is 130-142°C, and the longitudinal stretching ratio is 4-6.

[0032] Preferably, the longitudinal drawing and shaping is divided into 2-4 temperature control zones, and the zone temperature range is 130-145°C.

[0033] Preferably, the transverse drawing preheating is divided into 5-8 temperature control zones with a total length of 10-15m and a zone temperature range of 150-170°C.

[0034] Preferably, the transverse stretching is divided into 2-4 temperature control zones with a total length of 10-15 m and a zone temperature range of 160-170°C.

[0035] Preferably, the transverse stretching and shaping is divided into 5-8 temperature control zones with a total length of 10-17m, the zone temperature range is 160-175°C, and the total length of the heating zone of the entire transverse stretching section is 40-50m.

[0036] Preferably, the high-temperature wide guide rail spacing includes: the sheet entry width range is 560-775mm, the outlet width range is 5600-6200mm, and the stretching ratio is 1:8-1:10.

[0037] Preferably, the film has a thickness of 2.9-5 μm.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] The invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin. The method comprises an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process. The extrusion process comprises multi-region temperature control and inert gas protection; the sheet casting process comprises adopting multi-point electrical bolts to adjust the thickness of the sheet casting; the longitudinal stretching process comprises high-ratio multi-stage stretching and high-temperature shaping; and the transverse stretching process comprises adopting a high-temperature wide guide rail spacing for transverse stretching shaping.

[0040] The breakdown voltage of biaxially oriented polypropylene film (BOPP) usually depends on the degree of crystallinity; the greater the degree of crystallinity, the higher the breakdown voltage of the film; the crystallinity of the film mainly depends on the isotacticity and molecular weight distribution of the resin; the higher the isotacticity and the more uniform the molecular weight distribution (narrower the distribution), the higher the crystallinity of the film prepared in theory. However, too high isotacticity and narrow molecular weight distribution will make it difficult for the resin to form a film. Therefore, films are often prepared with moderate isotacticity and wide molecular weight distribution at the expense of a certain degree of resin crystallinity.

[0041] The present invention can achieve uniform heating and melting to improve melt uniformity by adopting multi-zone temperature control and inert gas protection in the extrusion process: the temperature of each zone can be accurately controlled by multi-zone temperature control to avoid overheating, reduce the possibility of thermal degradation, and prevent resin denaturation and degradation; the fluidity is improved by appropriate temperature distribution, so that the resin material can pass through the die head more easily, reduce the extrusion pressure, and also facilitate the subsequent stretching process; by adjusting the temperature of different sections, the recrystallization process can be controlled to avoid the degradation of the highly isotactic narrow molecular weight distribution polypropylene resin, and the crystallinity of the final film can be optimized, thereby affecting its breakdown field strength, rigidity and thermal stability performance.

[0042] The present invention adopts a width-adjustable die in the casting process and can accurately control the thickness of the film by adjusting the die gap; by controlling the die gap, the microstructure of the film, especially the crystallinity and molecular orientation, can be controlled, thereby improving the performance of the film, such as the breakdown field strength.

[0043] The longitudinal stretching process of the present invention includes high-ratio multi-stage stretching and high-temperature shaping. The high-ratio stretching can make the polymer chains highly oriented along the stretching direction, thereby significantly improving the longitudinal tensile strength and tear resistance of the film; it can reduce microstructural defects and bubbles in the film, and improve the film's breakdown field strength and other properties; the multi-stage stretching can fine-tune the film's thickness at multiple stages to ensure that the thickness of the entire film surface is uniform and consistent, avoiding local excessive thinness or excessive thickness; and the high-temperature shaping can optimize the resin crystallinity and further improve the film's mechanical and electrical properties.

[0044] The transverse stretching process of the present invention is a key step after longitudinal stretching, which involves the stretching and shaping of the film in the transverse direction. The present invention can promote the transverse orientation of the polymer molecular chain through high-temperature transverse stretching, thereby significantly improving the transverse tensile strength and toughness of the film; high temperature and wide guide rail spacing help the film to be stretched uniformly in the transverse direction, reduce the distortion of the microstructure, maintain and improve the isotacticity of the resin, maintain the molecular weight range of the raw resin, and improve the film drawing quality of the high isotactic narrow molecular weight distribution polypropylene resin; the wide guide rail spacing can ensure that the film has enough space to unfold evenly during transverse stretching, and with high-temperature shaping, it helps to eliminate internal stress, improve the dimensional stability of the film, and reduce shrinkage and deformation; transverse stretching at high temperature helps to optimize the microstructure of the film, such as crystallinity and orientation, which directly affects the breakdown field strength of the film; the wide guide rail spacing helps to maintain the tension balance of the film during the stretching process, avoid wrinkles and corrugations, and improve the flatness of the film; high-temperature transverse stretching helps to form a more compact molecular structure, thereby improving the isolation performance and anti-puncture ability of the film.

[0045] The innovation of the present invention is that we have achieved high-quality film drawing of high-isotactic and narrow molecular weight distribution resins, thereby achieving improved film crystallinity and improved breakdown field strength. The present invention solves the film-making process problems of high-isotactic and narrow molecular weight distribution resins, and achieves performance such as breakdown voltage that is superior to that of films prepared under traditional processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 Weibull distribution curve comparing the breakdown performance of the film prepared in Example 1 of the present invention and the traditional film;

[0047] Figure 2 Weibull distribution curve comparing the breakdown performance of the film prepared in Example 2 of the present invention and the traditional film;

[0048] Figure 3 Weibull distribution curve comparing the breakdown performance of the film prepared in Example 3 of the present invention and the traditional film;

[0049] Figure 4 Comparison of polarized morphology of the films prepared according to three typical embodiments of the present invention and traditional films. DETAILED DESCRIPTION

[0050] The technical solution is further described below in conjunction with the accompanying drawings and specific embodiments to help understand the content of the present invention.

[0051] Example 1

[0052] The present invention improves the extrusion and stretching process in the production process of BOPP film. The process of the present invention includes the following characteristic steps: using inert protective gas to achieve high-temperature extrusion of resin, by adjusting the speed of the metering pump, the extruded resin melt passes through the width-adjustable die under specific pipeline pressure and die head pressure, and is received by the quenching roller with a controllable fluid width to form a cast sheet. The thickness of the cast sheet is regulated by multi-point electrical bolts and then enters the stretching process section with a certain traction force. The longitudinal stretching process adopts high-ratio multi-stage stretching and high-temperature shaping, and the transverse stretching process adopts high-temperature wide guide rail spacing for transverse stretching shaping, and finally a BOPP film product with better performance than traditional resins is prepared.

[0053] The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process:

[0054] The extrusion process includes multi-zone temperature control and inert gas protection;

[0055] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0056] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0057] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0058] Preferably, the molecular weight of the polypropylene resin satisfies the following characteristics:

[0059] Mw=350000—550000; Mn=80000—160000; 3.4≤Mw / Mn≤4.5.

[0060] Preferably, the polypropylene resin has an isotactic 5-unit component content of 97.5%-98.3% and an isotactic 3-unit component content of 99.2%-99.6% as measured by high-temperature liquid nuclear magnetic resonance.

[0061] Preferably, the inert gas includes one or a combination of nitrogen, argon and helium.

[0062] Preferably, the extrusion process comprises: adjusting the pipe pressure and die head pressure of the extruded resin melt by adjusting the rotation speed of the feeding metering pump.

[0063] Preferably, the extrusion process comprises: controlling the fluid width of the resin by adjusting the width-adjustable die.

[0064] Preferably, the sheet casting process comprises: the extruded resin melt is received by a quenching roller to form a sheet, and the thickness of the sheet is regulated by multi-point electrical bolts.

[0065] Preferably, the longitudinal drawing process comprises: sequentially using three process sections of longitudinal drawing preheating, longitudinal drawing stretching and longitudinal drawing shaping to draw the cast sheet to form a longitudinally drawn thick sheet, and each process section adopts multi-zone temperature control.

[0066] Preferably, the transverse stretching process includes: using three process stages of transverse stretching preheating, transverse stretching and transverse stretching shaping to transversely stretch the longitudinally drawn thick sheet to form a final film product; wherein the transverse stretching shaping adopts high temperature and wide guide rail spacing.

[0067] Preferably, the multi-zone temperature control of the extrusion process includes: the temperature control zones of the extruder from the feeding port to the extruder die head are zone one, zone two, zone three, zone four, zone five, zone six and zone seven in sequence; the temperature ranges are: zone one 210-250°C; zone two 240-265°C; zone three 240-265°C; zone four 240-265°C; zone five 240-265°C; zone six 240-265°C; zone seven 210-250°C.

[0068] Preferably, the overall extrusion line speed of the extrusion process is 180-260 m / min.

[0069] Preferably, the speed range of the feeding metering pump is 30-60 rpm.

[0070] Preferably, the pipeline pressure range is 20-40 bar.

[0071] Preferably, the die pressure ranges from 80 to 150 bar.

[0072] Preferably, the fluid width is 1.5m-1.8m, with a deviation of no more than ±0.1%.

[0073] Preferably, the temperature range of the chill roller is 70-100°C.

[0074] Preferably, the multi-point electrical bolts include: 50-100 electrical bolts distributed over the width of the casting, wherein the number of bolts in the edge area of ​​the casting is 20-40, and the bolt temperature is 230-250°C; the number of bolts in the central part of the casting is 30-60, and the bolt temperature is 210-240°C.

[0075] Preferably, the cast sheet enters the longitudinal drawing process under the action of a traction force, and the traction force ranges from 280 to 350N.

[0076] Preferably, the longitudinal drawing preheating is divided into 5-8 temperature control zones, and the zone temperature range is 120-130°C.

[0077] Preferably, the longitudinal stretching is divided into 3-6 temperature control zones, the zone temperature range is 130-140°C, and the longitudinal stretching ratio is 4-6.

[0078] Preferably, the longitudinal drawing and shaping is divided into 2-4 temperature control zones, and the zone temperature range is 130-145°C.

[0079] Preferably, the transverse drawing preheating is divided into 5-8 temperature control zones with a total length of 10-15m and a zone temperature range of 150-170°C.

[0080] Preferably, the transverse stretching is divided into 2-4 temperature control zones with a total length of 10-15 m and a zone temperature range of 160-170°C.

[0081] Preferably, the transverse stretching and shaping is divided into 5-8 temperature control zones with a total length of 10-17m, the zone temperature range is 160-175°C, and the total length of the heating zone of the entire transverse stretching section is 40-50m.

[0082] Preferably, the high-temperature wide guide rail spacing includes: the sheet entry width range is 560-775mm, the outlet width range is 5600-6200mm, and the stretching ratio is 1:8-1:10.

[0083] Preferably, the film has a thickness of 2.9-5 μm.

[0084] A specific implementation process is as follows: a polypropylene resin with an isotactic 5-unit component content of 97.5%, an isotactic 3-unit component content of 99.2%, Mw=350000; Mn=800000; Mw / Mn=4.4 is put into an extruder, the feed pump speed is 30rpm, and the extrusion line speed is 180m / min. The temperatures of each zone of the extruder are: zone 1 210℃; zone 2 240℃; zone 3 240℃; zone 4 240℃; zone 5 240℃; zone 6 240℃; zone 7 210℃, and nitrogen is used as a protective gas in the extruder. The pressure of the resin melt in the pipeline is 20bar. The pressure of the extrusion die is 80bar. After the extruded melt flows out of the die, it is received by a quenching roller at a temperature of 70℃, and the melt flow width (casting sheet width) is 1.5m. The thickness of the casting sheet is adjusted by 50 electrical bolts distributed in the width direction, of which 20 bolts are close to the edge of the casting sheet, and the bolt temperature is 230℃; the number of bolts in the central part of the casting sheet is 30, and the bolt temperature is 210℃. The casting sheet enters the longitudinal drawing process section under the action of 280N traction force. The longitudinal drawing preheating section is divided into 5 temperature control areas, and the regional temperatures are 120℃, 120℃, 120℃, 120℃, and 120℃ respectively; the longitudinal drawing stretching section is divided into 3 temperature control areas, and the regional temperatures are 130℃, 130℃, and 130℃ respectively, and the longitudinal drawing ratio is 4; the longitudinal drawing shaping section is divided into 2 temperature control areas, and the regional temperatures are 130℃ and 130℃ respectively. After longitudinal drawing, the thick sheet enters the transverse drawing process area. The transverse drawing preheating section is divided into 5 temperature control areas with a total length of 10m. The regional temperatures are 150℃, 150℃, 150℃, 150℃, 150℃; the transverse drawing stretching section is divided into 2 temperature control areas with a total length of 10m. The regional temperatures are 160℃ and 160℃; the transverse drawing shaping section is divided into 5 temperature control areas with a total length of 10m. The temperatures of each area are 160℃, 160℃, 160℃, 160℃, 160℃. The total length of the heating area of ​​the entire transverse drawing section is 40m. The width of the transverse drawing guide rail is 560mm, the outlet width is 5600mm, and the stretching ratio is 1:10. The final thickness of the rolled film is 2.9μm.

[0085] In the preparation process of biaxially oriented polypropylene film (BOPP), the present invention adopts multi-stage or regional temperature control, which plays an important role in extruding polypropylene resin. Multi-stage temperature control is one of the key technologies to ensure the ideal material state and excellent product quality in the production process of BOPP film. This control strategy can bring the following beneficial technical effects:

[0086] 1. Improve melt uniformity: Through temperature control in different sections, it can ensure that the polypropylene resin can be evenly heated and melted after entering the extruder, avoiding local overheating or incomplete melting, thereby obtaining a more uniform melt.

[0087] 2. Prevent degradation: Polypropylene is prone to thermal degradation at high temperatures, producing volatiles and low molecular weight substances, which affect the performance of the final product. Multi-stage temperature control can accurately control the temperature of each zone, avoid overheating, and reduce the possibility of thermal degradation.

[0088] 3. Improve fluidity: Appropriate temperature distribution can improve the fluidity of the melt, making it easier for the material to pass through the die, reducing extrusion pressure, and also facilitating the subsequent stretching process.

[0089] 4. Optimize crystallinity: The crystallinity of polypropylene has an important influence on its physical properties. By adjusting the temperature of different sections, the crystallization process can be controlled and the crystallinity of the final film can be optimized, thereby affecting its transparency, rigidity and heat sealing performance.

[0090] 5. Reduced energy consumption: Accurate temperature control can avoid unnecessary energy waste, because it is not necessary to maintain the highest temperature in all areas, but to adjust it according to the actual needs of the material.

[0091] 6. Reduce failure and maintenance costs: Good temperature control helps reduce equipment blockage or damage caused by uneven material or overheating, thereby reducing the cost of maintenance and production downtime.

[0092] 7. Improve product quality: All of the above factors work together to significantly improve the quality of BOPP film, including better optical properties, mechanical strength and processing performance, ultimately meeting various application requirements.

[0093] In the preparation process of biaxially oriented polypropylene film (BOPP), the width-adjustable die plays an important role in the production of BOPP film, which not only helps to improve the quality of the film, but also enhances the flexibility and efficiency of the production line. The casting process is a key step, in which the use of a width-adjustable die (die gap) has many beneficial technical effects, mainly including the following points:

[0094] 1. Control film thickness: The size of the die gap directly determines the flow rate of the melt through the die head, thus affecting the thickness of the final film. By adjusting the die gap, the thickness of the film can be precisely controlled, which is crucial to meet the needs of different applications.

[0095] 2. Ensure thickness uniformity: The uniformity and adjustability of the die gap help ensure the thickness consistency of the film in the width direction, avoid film thickness fluctuations caused by uneven die gap, and thus improve product quality.

[0096] 3. Adapt to different production needs: Different product specifications may require different film thicknesses. The adjustable die gap enables the production line to flexibly respond to these changes and quickly adjust to different production requirements.

[0097] 4. Optimize material usage: Fine control of die gap can reduce material waste, because excessive melt flow will lead to excessive film thickness, which not only increases costs but may also affect the final performance of the film.

[0098] 5. Improve production efficiency: Appropriate die gap setting can ensure smooth flow of the melt and reduce fluctuations during extrusion, thereby improving the stability and efficiency of the production line.

[0099] 6. Improve film properties: By controlling the die gap, the microstructure of the film, such as crystallinity and molecular orientation, can be affected, which has a direct impact on improving the optical properties, mechanical strength and heat sealing properties of the film.

[0100] 7. Easy to maintain and clean: The die design with adjustable width is usually easier to disassemble and clean, which is beneficial for preventing the accumulation of scale and impurities, maintaining the cleanliness of the die, and extending the service life of the equipment.

[0101] 8. Adapt to raw material changes: When using different batches or types of polypropylene resin, the flow properties of the raw materials may be different. The adjustable die gap can better adapt to these changes and ensure the consistency of the production process.

[0102] In the preparation process of biaxially oriented polypropylene film (BOPP), the longitudinal stretching process (MD stretching) includes high-ratio multi-stage stretching and high-temperature shaping. This series of operations has a crucial impact on the performance of the final film. The high-ratio multi-stage stretching and high-temperature shaping in the longitudinal stretching process are key steps to ensure that the BOPP film has excellent performance. They directly affect the final use performance of the film. The specific beneficial technical effects include:

[0103] 1. Improve mechanical strength: High-ratio stretching can make the polymer chains highly oriented along the stretching direction, thereby significantly improving the longitudinal tensile strength and tear resistance of the film.

[0104] 2. Improve optical properties: Proper stretching can reduce defects and bubbles in the film and improve transparency and gloss, which is especially important for packaging, labeling and printing applications.

[0105] 3. Control thickness uniformity: Multi-stage stretching can fine-tune the thickness of the film at multiple stages to ensure uniform thickness across the entire film surface and avoid partial thinness or thickness.

[0106] 4. Optimize crystallinity: High temperature setting is carried out after the film reaches a certain degree of orientation, which helps to optimize the crystallinity and further improve the mechanical properties and thermal stability of the film.

[0107] 5. Dimensional stability: The film that has been treated with high temperature shaping has better dimensional stability during subsequent use or processing and is not easily deformed by temperature changes.

[0108] 6. Improve heat sealing performance: By controlling the stretching and shaping conditions, the heat sealing performance of the film can be adjusted to make it more suitable for high-speed heat sealing operations of automatic packaging machines.

[0109] 7. Reduce internal stress: Multi-stage stretching and high-temperature shaping help release residual stress inside the film, reduce curling and warping, and improve the flatness of the film.

[0110] 8. Improve chemical resistance: Appropriate stretching and shaping conditions can improve the molecular structure of the film and enhance its resistance to chemical corrosion.

[0111] 9. Enhanced barrier properties: The oriented molecular structure helps to form a tighter film structure, thereby improving the barrier properties to gases, water vapor and odors.

[0112] 10. Energy saving and production efficiency: Although high-ratio stretching and high-temperature shaping require more energy, higher production efficiency can be achieved by optimizing process parameters, which may have better economic benefits in the long run.

[0113] In the preparation process of biaxially oriented polypropylene film (BOPP) of the present invention, the transverse stretching process (TD stretching) is a key step after longitudinal stretching, which involves the stretching and shaping of the film in the transverse direction. The use of high temperature and wide rail spacing for transverse stretching and shaping can significantly improve the physical and mechanical properties of the BOPP film, optimize its microstructure, and enhance its functionality and market competitiveness. The use of high temperature and wide rail spacing for transverse stretching and shaping has the following beneficial technical effects:

[0114] 1. Improve the transverse mechanical strength of the film: High-temperature transverse stretching can promote the transverse orientation of polymer molecular chains, thereby significantly improving the transverse tensile strength and toughness of the film.

[0115] 2. Improve the optical properties of the film: High temperature and wide guide rail spacing help the film to stretch evenly in the transverse direction, reduce optical distortion, and improve transparency and gloss.

[0116] 3. Enhanced dimensional stability: The wide rail spacing can ensure that the film has enough space to unfold evenly when stretched horizontally. Combined with high temperature shaping, it helps to eliminate internal stress, improve the dimensional stability of the film, and reduce shrinkage and deformation.

[0117] 4. Optimize film structure: Horizontal stretching at high temperature helps to optimize the film's microstructure, such as crystallinity and orientation, which directly affects the film's barrier properties, heat sealing properties and printability.

[0118] 5. Improve film flatness: Wide guide rail spacing helps to maintain the tension balance of the film during stretching, avoid wrinkles and ripples, and improve the flatness of the film.

[0119] 6. Improve thermal stability: High-temperature horizontal drawing and shaping can enhance the thermal stability of the film, making it less susceptible to thermal deformation during subsequent processing or use.

[0120] 7. Improve the heat sealing performance of the film: By controlling the horizontal drawing temperature and shaping conditions, the heat sealing layer characteristics of the film can be adjusted to make it more suitable for the heat sealing needs of the packaging industry.

[0121] 8. Enhance the chemical resistance of the film: High temperature horizontal drawing helps to form a more compact molecular structure, thereby improving the film's resistance to chemicals.

[0122] 9. Improve the barrier properties of the film: Optimized molecular structure and high orientation can enhance the barrier effect of the film against gas, water vapor and other small molecules.

[0123] 10. Improve production efficiency and product quality: Appropriate horizontal drawing process parameters can reduce the scrap rate in the production process and increase the yield rate, thereby improving the overall production efficiency and product quality of the film.

[0124] The method for preparing a biaxially stretched film of a high-isotactic narrow molecular weight distribution polypropylene resin provided by the present invention comprises an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process, which support and act together with each other, and a single process cannot achieve high-quality film drawing of a high-isotactic narrow molecular weight distribution resin; at the same time, the process parameters contained in each process and the process parameters of other processes are also interrelated and support each other and act together, and cannot solve the technical problem alone, and changing some of the parameters will also produce more crystallinity distortion or other microstructure problems, and cannot achieve high-quality film drawing of a high-isotactic narrow molecular weight distribution resin: all the processes and technical parameters of the present invention are an organic whole, not a mechanical accumulation, and at the same time, the final technical effect exceeds the simple accumulation of the existing technical effects of each process, and achieves an unexpectedly significant technical effect.

[0125] The innovation of the present invention is that we have achieved high-quality film drawing of high-isotactic and narrow molecular weight distribution resins, thereby achieving improved film crystallinity and improved breakdown field strength. The present invention solves the film-making process problems of high-isotactic and narrow molecular weight distribution resins, and achieves performance such as breakdown voltage that is superior to that of films prepared under traditional processes.

[0126] Example 2

[0127] The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process:

[0128] The extrusion process includes multi-zone temperature control and inert gas protection;

[0129] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0130] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0131] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0132] The specific implementation process of this embodiment is as follows: a polypropylene resin with an isotactic 5-unit component content of 98.3%, an isotactic 3-unit component content of 99.6%, Mw=550000; Mn=160000; Mw / Mn=3.4 is put into an extruder, the feed pump speed is 60rpm, and the extrusion line speed is 260m / min. The temperatures of each zone of the extruder are: zone 1 250℃; zone 2 265℃; zone 3 265℃; zone 4 265℃; zone 5 265℃; zone 6 265℃; zone 7 250℃, and helium is used as a protective gas in the extruder. The pressure range of the resin melt in the pipeline is 40bar. The pressure range of the extrusion die is 150bar. After the extruded melt flows out of the die, it is received by a quenching roller with a temperature of 100℃, and the melt flow width (casting sheet width) is 1.8m. The thickness of the casting sheet is adjusted by 100 electrical bolts distributed in the width direction, of which 40 bolts are near the edge of the casting sheet, and the bolt temperature is 250℃; the number of bolts in the central part of the casting sheet is 60, and the bolt temperature is 240℃. The casting sheet enters the longitudinal drawing process section under the action of 350N traction force. The longitudinal drawing preheating section is divided into 8 temperature control areas, and the temperatures of each area are 130℃, 130℃, 130℃, 130℃, 130℃, 130℃, 130℃, 130℃, 130℃; the longitudinal drawing stretching section is divided into 6 temperature control areas, and the temperatures of each area are 140℃, 140℃, 140℃, 140℃, 140℃, 140℃, and the longitudinal drawing ratio is 6; the longitudinal drawing shaping section is divided into 4 temperature control areas, and the temperatures of each area are 145℃, 145℃, 145℃, 145℃, and 145℃. After longitudinal drawing, the thick sheet enters the transverse drawing process area. The transverse drawing preheating section is divided into 8 temperature control areas with a total length of 15m. The temperatures of each area are 170℃, 170℃, 170℃, 170℃, 170℃, 170℃, 170℃, 170℃, 170℃; the transverse drawing stretching section is divided into 4 temperature control areas with a total length of 15m. The temperatures of each area are 170℃, 170℃, 170℃, 170℃, 170℃; the transverse drawing shaping section is divided into 8 temperature control areas with a total length of 17m. The temperatures of each area are 175℃, 175℃, 175℃, 175℃, 175℃, 175℃, 175℃, 175℃; the total length of the heating area of ​​the entire transverse drawing section is 50m. The width of the transverse drawing guide rail entry is 775mm, the exit width is 6200mm, and the stretching ratio is 1:8. The final winding film thickness is 5μm.

[0133] The necessary technical contents not described in this example are the same as those in Example 1 or are prior art, so they will not be repeated here.

[0134] Example 3

[0135] The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process:

[0136] The extrusion process includes multi-zone temperature control and inert gas protection;

[0137] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0138] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0139] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0140] The specific implementation process of this embodiment is as follows: a polypropylene resin with an isotactic 5-unit component content of 97.8%, an isotactic 3-unit component content of 99.4%, Mw=380000; Mn=85000; Mw / Mn=4.5 is put into an extruder, the feed pump speed is 38rpm, and the extrusion line speed is 242m / min. The temperatures of each zone of the extruder are: zone 1 245℃; zone 2 250℃; zone 3 255℃; zone 4 255℃; zone 5 255℃; zone 6 250℃; zone 7 248℃, and argon is used as a protective gas in the extruder. The pressure range of the resin melt in the pipeline is 25bar. The pressure range of the extrusion die is 143bar. After the extruded melt flows out of the die, it is received by a quenching roller at a temperature of 90℃, and the melt flow width (casting sheet width) is 1.7m. The thickness of the casting sheet is adjusted by 80 electrical bolts distributed in the width direction, of which 25 bolts are near the edge of the casting sheet, and the bolt temperature is 240℃; the number of bolts in the central part of the casting sheet is 55, and the bolt temperature is 220℃. The casting sheet enters the longitudinal drawing process section under the action of 320N traction force. The longitudinal drawing preheating section is divided into 6 temperature control areas, and the temperatures of each area are 126℃, 127℃, 128℃, 128℃, 132℃, and 133℃ respectively; the longitudinal drawing stretching section is divided into 5 temperature control areas, and the temperatures of each area are 138℃, 139℃, 142℃, 140℃, and 140℃ respectively, and the longitudinal drawing ratio is 5; the longitudinal drawing shaping section is divided into 3 temperature control areas, and the temperatures of each area are 140℃, 140℃, and 141℃ respectively. After longitudinal drawing, the thick sheet enters the transverse drawing process area. The transverse drawing preheating section is divided into 6 temperature control areas with a total length of 12m. The temperatures of each area are 167℃, 167℃, 167℃, 166℃, 166℃, and 166℃ respectively; the transverse drawing stretching section is divided into 3 temperature control areas with a total length of 12m. The temperatures of each area are 161℃, 161℃, and 162℃ respectively; the transverse drawing shaping section is divided into 7 temperature control areas with a total length of 15m. The temperatures of each area are 162℃, 165℃, 169℃, 169℃, 169℃, 169℃, 161℃; the total length of the heating area of ​​the entire transverse drawing section is 42m. The width of the transverse drawing guide rail for sheet entry is 600mm, the outlet width is 5800mm, and the stretching ratio is 1:9.7. The final thickness of the rolled film is 3.8μm.

[0141] The necessary technical contents not described in this example are the same as those in Example 1 or are prior art, so they will not be repeated here.

[0142] Example 4

[0143] The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process:

[0144] The extrusion process includes multi-zone temperature control and inert gas protection;

[0145] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0146] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0147] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0148] The specific implementation process of this embodiment is as follows: a polypropylene resin with an isotactic 5-unit component content of 98.0%, an isotactic 3-unit component content of 99.3%, Mw=350000; Mn=90000; Mw / Mn=3.9 is put into an extruder, the feed pump speed is 42rpm, and the extrusion line speed is 220m / min. The temperatures of each zone of the extruder are: zone 1 245℃; zone 2 250℃; zone 3 260℃; zone 4 260℃; zone 5 260℃; zone 6 250℃; zone 7 248℃, and a mixed gas of nitrogen and argon is used as a protective gas in the extruder. The pressure range of the resin melt in the pipeline is 32bar. The pressure of the extrusion die is 138bar. After the extruded melt flows out of the die, it is received by a quenching roller with a temperature of 91.5℃, and the melt flow width (casting sheet width) is 1.75m. The thickness of the casting sheet is adjusted by 80 electrical bolts distributed in the width direction, of which 25 bolts are near the edge of the casting sheet, and the bolt temperature is 240℃; the number of bolts in the central part of the casting sheet is 55, and the bolt temperature is 220℃. The casting sheet enters the longitudinal drawing process section under the action of 320N traction force. The longitudinal drawing preheating section is divided into 5 temperature control areas, and the temperatures of each area are 127℃, 127℃, 129℃, 131℃, and 133℃ respectively; the longitudinal drawing stretching section is divided into 5 temperature control areas, and the temperatures of each area are 138℃, 139℃, 141℃, 139℃, and 139℃ respectively, and the longitudinal drawing ratio is 5; the longitudinal drawing shaping section is divided into 2 temperature control areas, and the temperatures of each area are 141℃ and 141℃ respectively. After longitudinal drawing, the thick sheet enters the transverse drawing process area. The transverse drawing preheating section is divided into 5 temperature control areas with a total length of 10m. The temperatures of each area are 168℃, 168℃, 168℃, 166℃, and 166℃ respectively; the transverse drawing stretching section is divided into 3 temperature control areas with a total length of 12m. The temperatures of each area are 162℃, 162℃, and 163℃ respectively; the transverse drawing shaping section is divided into 7 temperature control areas with a total length of 15m. The temperatures of each area are 163℃, 166℃, 169℃, 169℃, 169℃, 169℃, and 161℃; the total length of the heating area of ​​the entire transverse drawing section is 42m. The width of the transverse drawing guide rail entry is 750mm, the maximum stretching width is 6000mm, the outlet width is 5600mm, and the stretching ratio is 1:9.2. The final winding film thickness is 4.0μm.

[0149] The necessary technical contents not described in this example are the same as those in Example 1 or are prior art, so they will not be repeated here.

[0150] Example 5

[0151] The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process:

[0152] The extrusion process includes multi-zone temperature control and inert gas protection;

[0153] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0154] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0155] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0156] The specific implementation process of this embodiment is as follows: a polypropylene resin with an isotactic 5-unit component content of 97.8%, an isotactic 3-unit component content of 99.2%, Mw=350000; Mn=90000; Mw / Mn=3.9 is put into an extruder, the feed pump speed is 40rpm, and the extrusion line speed is 230m / min. The temperatures of each zone of the extruder are: zone 1 247℃; zone 2 250℃; zone 3 263℃; zone 4 263℃; zone 5 263℃; zone 6 251℃; zone 7 249℃, and nitrogen is used as a protective gas in the extruder. The pressure range of the resin melt in the pipeline is 36bar. The pressure of the extrusion die is 134bar. After the extruded melt flows out of the die, it is received by a quenching roller with a temperature of 90.5℃, and the melt flow width (casting sheet width) is 1.7m. The thickness of the casting sheet is adjusted by 80 electrical bolts distributed in the width direction, of which 25 bolts are near the edge of the casting sheet, and the bolt temperature is 233℃; the number of bolts in the central part of the casting sheet is 55, and the bolt temperature is 220℃. The casting sheet enters the longitudinal drawing process section under the action of 300N traction force. The longitudinal drawing preheating section is divided into 5 temperature control areas, and the temperatures of each area are 127.5℃, 128.5℃, 129℃, 131℃, and 133℃ respectively; the longitudinal drawing stretching section is divided into 5 temperature control areas, and the temperatures of each area are 138.5℃, 139℃, 142℃, 141℃, and 141℃ respectively, and the longitudinal drawing ratio is 5; the longitudinal drawing shaping section is divided into 2 temperature control areas, and the temperatures of each area are 141℃ and 141℃ respectively. After longitudinal drawing, the thick sheet enters the transverse drawing process area. The transverse drawing preheating section is divided into 5 temperature control areas with a total length of 10m. The temperatures of each area are 168℃, 168℃, 168℃, 166℃, and 166℃ respectively; the transverse drawing stretching section is divided into 3 temperature control areas with a total length of 12m. The temperatures of each area are 162℃, 162℃, and 163℃ respectively; the transverse drawing shaping section is divided into 7 temperature control areas with a total length of 15m. The temperatures of each area are 163℃, 166℃, 169℃, 169℃, 170℃, 170℃, and 161℃; the total length of the heating area of ​​the entire transverse drawing section is 42m. The width of the transverse drawing guide rail entry is 750mm, the maximum stretching width is 6000mm, the outlet width is 5600mm, and the stretching ratio is 1:8.5. The final winding film thickness is 5.8μm.

[0157] Table 1 Comparison of properties of films prepared in three typical embodiments of the present invention and conventional films

[0158]

[0159] As shown in Table 1, Figure 1-3 As shown, the films prepared in Examples 1-3 of the present invention are compared with the films of the same thickness prepared by the conventional process. The breakdown field strength of the films prepared in the present invention is significantly better than that of the films prepared by the conventional technology. Figure 4 As shown, there is no significant difference between the surface of the film prepared by the present invention and the surface of the film prepared by the conventional technology. The breakdown voltage of BOPP film usually depends on the degree of crystallinity. The greater the crystallinity, the higher the breakdown voltage of the film. The crystallinity of the film mainly depends on the isotacticity and molecular weight distribution of the resin. The higher the isotacticity and the more uniform the molecular weight distribution (narrower distribution) of the resin, the higher the crystallinity of the prepared film in theory. However, too high isotacticity and narrow molecular weight distribution will make it difficult for the resin to form a film. Therefore, the existing traditional process often adopts moderate isotacticity and wide molecular weight distribution to prepare films at the expense of a certain degree of resin crystallinity. The innovation of the present invention is that we have achieved high-quality film drawing of resins with high isotacticity and narrow molecular weight distribution, thereby achieving both an increase in film crystallinity and an increase in breakdown field strength.

[0160] The necessary technical contents not described in this example are the same as those in Example 1 or are prior art, so they will not be repeated here.

[0161] Example 6

[0162] The present invention provides a method for preparing a biaxially stretched film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising a resin reinforcement step, an extrusion step, a sheet casting step, a longitudinal stretching step and a transverse stretching step:

[0163] The resin reinforcement process includes adding nano-mica powder to the isotactic narrow molecular weight distribution polypropylene resin;

[0164] The extrusion process includes multi-zone temperature control and inert gas protection;

[0165] The casting process includes using multi-point electrical bolts to control the thickness of the casting;

[0166] The longitudinal stretching process includes high-ratio multi-stage stretching and high-temperature shaping;

[0167] The transverse drawing process includes adopting high temperature and wide guide rail spacing to perform transverse drawing and shaping.

[0168] The specific implementation process of this embodiment is as follows:

[0169] Firstly, 0.16-0.31 parts of nano-mica powder by mass ratio and 1 part of the highly isotactic narrow molecular weight distribution polypropylene resin are uniformly mixed at a temperature of 200° C. to 230° C. to obtain a reinforced resin raw material; the reinforced resin raw material is sequentially subjected to the extrusion process, the sheet casting process, the longitudinal drawing process and the transverse drawing process to make a film.

[0170] The nano mica powder is a micro-flaky structure, with a maximum particle size of 250nm-480nm and a lamella thickness of 70nm-120nm; the nano mica powder is prepared by crushing and grinding natural mica powder of 1500-2000 mesh in a liquid nitrogen grinder, and the grinding balls are zirconium oxide ZrO2. The nano mica powder is prevented from contacting with air during the preparation and addition of the high isotactic narrow molecular weight distribution polypropylene resin, or inert gas protection is used during the preparation and storage to maintain surface activity and ensure the bonding strength with the resin. The content of zirconium oxide ZrO2 in the prepared nano mica powder is not higher than 7%.

[0171] In this embodiment, the nano mica powder added in the resin reinforcement process is evenly distributed in the highly isotactic narrow molecular weight distribution polypropylene resin. After biaxial stretching, the micro-platelet structure of the nano mica is parallel to the film plane and most of the area is 1-2 layers distributed in the resin film to form mutually separated insulation reinforcement points. The breakdown field strength of the enhanced polypropylene resin film produced in this embodiment can reach 760-820 (25°C, kV / mm).

[0172] The multi-zone temperature control in the processes of extrusion, longitudinal stretching preheating, longitudinal stretching shaping, transverse stretching preheating, transverse stretching, transverse stretching shaping and the like is crucial to the recovery of the bonding strength between the micro-flaky structure of the nano-mica powder and the film resin after stretching. During the stretching process, the bonding strength between the micro-flaky structure of the nano-mica powder and the film resin decreases and even partial separation in the microstructure occurs. The multi-zone temperature control in each process can repair the microstructural defects caused by stretching, realize the reconstruction process of the bonding strength between the micro-flaky structure of the nano-mica powder and the film resin, and ensure the stability and further improvement of the physical and electrical properties of the enhanced high-isotactic narrow molecular weight distribution polypropylene resin film after molding.

[0173] Necessary technical contents not described in this example are the same as those in the aforementioned embodiments or are prior art, and thus will not be described in detail.

[0174] The above are merely embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are included in the scope of the claims of the present invention.

Claims

1. A method for preparing a biaxially oriented film of a high isotactic narrow molecular weight distribution polypropylene resin, the method comprising an extrusion process, a sheet casting process, a longitudinal stretching process and a transverse stretching process, characterized in that: The extrusion process includes multi-zone temperature control and inert gas protection; The casting process includes using multi-point electrical bolts to control the thickness of the casting; The longitudinal drawing process includes high-ratio multi-stage stretching and high-temperature shaping, and the casting sheet is stretched to form a longitudinally drawn thick sheet by sequentially adopting three process stages of longitudinal drawing preheating, longitudinal drawing stretching and longitudinal drawing shaping, and each process stage adopts multi-zone temperature control; The transverse stretching process includes using high temperature and wide guide rail spacing for transverse stretching and shaping, and using three process stages of transverse stretching preheating, transverse stretching and transverse stretching shaping to transversely stretch the longitudinally drawn thick sheet to form the final film product; wherein the transverse stretching shaping adopts high temperature and wide guide rail spacing; The multi-zone temperature control of the extrusion process includes: the temperature control zones of the extruder from the feed port to the extruder die head are zone one, zone two, zone three, zone four, zone five, zone six and zone seven in sequence; the temperature ranges are: zone one 210-250°C; zone two 240-265°C; zone three 240-265°C; zone four 240-265°C; zone five 240-265°C; zone six 240-265°C; zone seven 210-250°C.

2. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 1, characterized in that: The molecular weight of the polypropylene resin meets the following characteristics: Mw=350000-550000; Mn=80000-160000; 3.4≤Mw / Mn≤4.

5.

3. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 2, characterized in that: The polypropylene resin has an isotactic 5-unit component content of 97.5%-98.3% and an isotactic 3-unit component content of 99.2%-99.6% as measured by high-temperature liquid nuclear magnetic resonance.

4. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 1, characterized in that: The inert gas includes one or a combination of nitrogen, argon and helium.

5. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 1, characterized in that: The extrusion process comprises: adjusting the pipe pressure and die head pressure of the extruded resin melt by adjusting the rotation speed of the feeding metering pump.

6. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 1, characterized in that: The extrusion process includes: controlling the flow width of the resin by adjusting a width-adjustable die.

7. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 1, characterized in that: The sheet casting process includes: the extruded resin melt is received by a quenching roller to form a sheet casting, and the thickness of the sheet casting is regulated by multi-point electrical bolts.

8. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 1, characterized in that: The overall extrusion line speed of the extrusion process is 180-260 m / min.

9. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin as claimed in claim 5, characterized in that: The speed range of the feeding metering pump is 30-60rpm.

10. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 5, characterized in that: The pipeline pressure range is 20-40 bar.

11. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 5, characterized in that: The die pressure ranges from 80 to 150 bar.

12. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 6, characterized in that: The fluid width is 1.5m-1.8m, with a deviation of no more than ±0.1%.

13. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 7, characterized in that: The temperature range of the chill roll is 70-100°C.

14. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 7, characterized in that: The multi-point electrical bolts include: 50-100 electrical bolts distributed on the width of the casting, wherein the number of bolts in the edge area of ​​the casting is 20-40, and the bolt temperature is 230-250°C; the number of bolts in the central part of the casting is 30-60, and the bolt temperature is 210-240°C.

15. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 7, characterized in that: The cast sheet enters the longitudinal drawing process under the action of traction force, and the traction force range is 280-350N.

16. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The longitudinal drawing preheating is divided into 5-8 temperature control zones, and the zone temperature range is 120-133°C.

17. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The longitudinal stretching is divided into 3-6 temperature control zones, the zone temperature range is 130-142°C, and the longitudinal stretching ratio is 4-6.

18. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The longitudinal drawing and shaping is divided into 2-4 temperature control zones, and the zone temperature range is 130-145°C.

19. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The transverse drawing preheating is divided into 5-8 temperature control zones with a total length of 10-15m and a zone temperature range of 150-170°C.

20. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The transverse stretching is divided into 2-4 temperature control zones with a total length of 10-15m and a zone temperature range of 160-170°C.

21. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The transverse stretching shaping is divided into 5-8 temperature control zones with a total length of 10-17m. The zone temperature range is 160-175°C, and the total length of the heating zone of the entire transverse stretching section is 40-50m.

22. The method for preparing a biaxially oriented film of a highly isotactic narrow molecular weight distribution polypropylene resin according to claim 1, characterized in that: The high temperature wide guide rail spacing includes: the sheet entry width range is 560-775mm, the exit width range is 5600-6200mm, and the stretching ratio is 1:8-1:

10.