A method for preparing carbon nitride nanotube composite hydrogen storage material

Through the preparation of carbon nitride nanotube composite materials, the problem of hydrogen storage materials in harsh conditions is solved, and the absorption and release of high-efficiency hydrogen is achieved. It has high hydrogen storage capacity and long life, which is suitable for commercial applications.

CN118579726BActive Publication Date: 2024-11-19SHANGHAI SUPERHIGH ENVIRONMENTAL PROTECTION TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074261.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing hydrogen storage materials have harsh hydrogen storage conditions, unstable structure, low hydrogen absorption and release speed and complex preparation process, which limit the safe and efficient storage and release of hydrogen.

Method used

Using a preparation method of carbon nitride nanotube composite hydrogen storage material, the adsorption of carbon nanotubes is enhanced by mechanical ball milling, wet treatment and nitriding treatment, combined with dispersed components of aromatic compounds, polyols and organic solvents, and through Agitate and heat to form a composite material to achieve efficient hydrogen storage and release.

Benefits of technology

It achieves efficient absorption and release of hydrogen under mild conditions (0.3Mpa pressure, 270K temperature and 24V voltage), with high hydrogen storage capacity, long service life and good hydrogen absorption and discharge characteristics, and is suitable for commercial and practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118579726B_ABST
    Figure CN118579726B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of hydrogen storage materials, and specifically discloses a method for preparing a carbon nanotube nitride composite hydrogen storage material. The method comprises the following steps: (1) placing carbon nanotubes in a ball mill for mechanical ball milling; (2) performing wet treatment on the carbon nanotubes after ball milling and then drying; (3) placing the dried carbon nanotubes in a muffle furnace for nitridation treatment to obtain carbon nanotubes; (4) adding aromatic compounds, polyols and organic solvents to a reactor, and obtaining dispersed components after sufficient mixing; (5) adding carbon nanotubes and magnesium nitride to the reactor, stirring evenly and continuing to stir and heat, and after the reaction is completed, the product is formed and packaged to obtain the carbon nanotube nitride composite hydrogen storage material of the present invention. The carbon nanotube nitride composite hydrogen storage material prepared by the method of the present invention has mild hydrogen storage conditions, high hydrogen storage capacity, long service life and can exhibit good hydrogen absorption and release characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen storage materials, and in particular relates to a method for preparing a carbon nitride nanotube composite hydrogen storage material. Background Art

[0002] The utilization of hydrogen energy mainly includes three important links: preparation, storage and transportation. Driven by inexhaustible solar energy, the photocatalytic hydrogen production technology that uses water to produce hydrogen has shown great potential due to its low cost and environmental friendliness. However, hydrogen and oxygen are prone to react and explode after mixing, and the commonly used pressure tank hydrogen storage has low safety and convenience. The existing traditional technical methods cannot safely store and transport hydrogen to meet future needs. The bottleneck of hydrogen storage technology limits its large-scale application. Therefore, storing hydrogen in a small, light, convenient and safe hydrogen storage material and realizing efficient storage and release of hydrogen are the conditions for hydrogen to be widely used in the future. At present, the main factor restricting the promotion and development of hydrogen energy is the difficulty in finding a hydrogen storage material with excellent performance. Traditional low-temperature hydrogen storage, high-pressure hydrogen storage and room temperature new material hydrogen storage have strict requirements on hydrogen storage conditions and the hydrogen storage material itself, which is not conducive to promotion.

[0003] Fortunately, the progress in the preparation technology of large-scale carbon nanomaterials has brought new opportunities for hydrogen storage. Among them, carbon nanotubes have hollow tubular structures, large specific surface area, large surface activity and excellent physical and chemical properties, which provide natural and excellent conditions for hydrogen storage. Since Dillon et al. pioneered the use of single-walled carbon nanotubes for hydrogen storage in 1977, as a metal-free and inexpensive material, the hydrogen storage performance of carbon nanotubes has gradually attracted widespread attention from researchers. The unique metallicity and one-dimensional structure of carbon nanotubes give them strong electron transport properties, and they have obvious advantages such as simple hydrogen storage methods and easy absorption and release of hydrogen molecules. In addition, carbon nanotubes have strong compressive strength, good mechanical properties and chemical properties, so they are widely used in photocatalysis, chemical sensing and energy storage, but their inherent hydrophobicity must be oxidized on their surface to form defects, increase the polarity of carbon nanotubes and thus improve the adsorption of hydrogen, such as hydroxyl, carboxyl and other functional groups. However, the introduction of too many oxygen-containing functional groups will reduce the rate of hydrogen absorption and desorption to a certain extent, and the dangling bonds brought by the functional groups on the surface of carbon nanotubes will cause the energy of carbon nanotubes to be too high, resulting in structural instability and agglomeration.

[0004] The most direct way to regulate the adsorption performance of carbon nanotubes for hydrogen molecules is to change their surface properties. By modifying the functional groups of carbon nanotubes, such as doping and defects, on the one hand, the diffusion rate of hydrogen affects the kinetics of hydrogen absorption and desorption, thereby reducing the friction between hydrogen molecules and the carbon nanotube wall, thereby enhancing the diffusion rate of hydrogen molecules in the nanochannel; on the other hand, the electronic structure of the nanotube surface is regulated, thereby adjusting the interaction between the nanotube and the hydrogen molecules, and regulating the diffusion rate of hydrogen molecules in the nanochannel. However, as the amount of hydrogen adsorption in the carbon nanotube increases, it affects the further diffusion of hydrogen molecules. Therefore, the diffusion ability of hydrogen on the surface of carbon nanotubes and its interaction with carbon nanotubes jointly determine the hydrogen storage capacity of carbon nanotubes. The functionalization strategy of carbon nanotubes mainly depends on the structure and chemical properties of the material, but there is currently no effective strategy to improve the adsorption and desorption ability of hydrogen molecules on the surface of carbon nanotube-based composite materials. Different preparation methods will also cause great differences in the performance of carbon nanotube-based composite hydrogen storage materials. Carbon nanotube-based composite hydrogen storage materials prepared by existing traditional methods have disadvantages such as high working temperature, poor cycle stability or difficulty in activation to varying degrees, and the preparation process is complicated.

[0005] In summary, it is of great significance to provide a preparation method with high yield, low cost, simple operation, simple and controllable process, and to make the prepared carbon nanotube-based composite hydrogen storage material have mild hydrogen storage conditions (the function of absorbing and releasing hydrogen under the conditions of hydrogen storage pressure of 0.3Mpa, temperature of 270K and voltage of 24V), simple structure, safe and efficient, high hydrogen storage capacity, long service life and good hydrogen absorption and desorption characteristics. Summary of the invention

[0006] In view of this, the present invention provides a method for preparing a carbon nanotube nitride composite hydrogen storage material in order to solve the above problems. The conditions for preparing the hydrogen storage material of the present invention are mild, the equipment is simple and convenient, easy to operate, and suitable for large-scale production. The method of the present invention can be used to prepare a composite hydrogen storage material with mild hydrogen storage conditions (function of absorbing and releasing hydrogen under the conditions of hydrogen storage pressure of 0.3Mpa, temperature of 270K and voltage of 24V), high hydrogen storage capacity, long service life and good hydrogen absorption and release characteristics. Compared with other hydrogen storage materials that require special hydrogen storage conditions such as high temperature and high pressure, it has more commercial and practical conditions.

[0007] Specifically, the following technical solutions are included:

[0008] A method for preparing a carbon nitride nanotube composite hydrogen storage material comprises the following steps:

[0009] (1) Placing carbon nanotubes into a ball mill for mechanical ball milling;

[0010] (2) wet-treating the milled carbon nanotubes and then drying them;

[0011] (3) placing the dried carbon nanotubes in a muffle furnace for nitridation treatment to obtain nitrided carbon nanotubes;

[0012] (4) adding an aromatic compound, a polyol and an organic solvent into a reaction kettle and mixing them thoroughly to obtain a dispersed component;

[0013] (5) Adding carbon nitride nanotubes and magnesium nitride into a reaction kettle, stirring evenly and then continuing to stir and heat, and after the reaction is completed, forming and packaging the product to prepare the carbon nitride nanotube composite hydrogen storage material.

[0014] In some possible implementations, the carbon nanotubes in step (1) are multi-walled carbon nanotubes or single-walled carbon nanotubes with a diameter of <2 nm, more preferably <0.7 nm.

[0015] In some possible implementations, the mechanical ball milling in step (1) is carried out on a star-shaped ball mill under an ammonia atmosphere of 0.3-0.8 MPa, the ball milling medium is 20-50 steel balls, the ball milling time is 10-30 h, and the ball milling speed is 300-500 rpm.

[0016] In some possible implementations, during the ball milling process, the mixing mass ratio of the ball milling medium to the carbon nanotubes is (60-100):1.

[0017] The carbon nanotubes subjected to the above-mentioned ball milling treatment will cause surface defects and cracks, thereby increasing the specific surface area of ​​the material, which is beneficial to enhancing the adsorption of the carbon nanotubes and increasing their hydrogen storage capacity; in particular, the above-mentioned ball milling treatment is carried out in an ammonia atmosphere. During the ball milling process, ammonia will be converted into nitrogen due to the influence of temperature, which is more beneficial to improving the hydrogen storage effect of the carbon nanotubes.

[0018] In some possible implementations, the wet treatment in step (2) is to place the milled carbon nanotubes into a pressure cooker and inject deionized water into the pressure cooker and heat it to 90-120° C., and repeat the heating for more than three times, with each heating being kept constant for 30-120 minutes.

[0019] In step (2), the present invention does not have any special limitation on the drying process, and the drying process may be carried out using a process well known to those skilled in the art.

[0020] In some possible implementations, the nitridation treatment in step (3) is to place the dried carbon nanotubes in a muffle furnace for high-temperature treatment at 500-650° C., and nitrogen is injected into the sealed furnace chamber of the muffle furnace to allow the carbon nanotubes to be nitrided in a heated environment.

[0021] In step (3), the present invention does not have any special limitation on the process of nitrogen perfusion, and the process can be carried out using a process well known to those skilled in the art.

[0022] In the present invention, the carbon nanotubes are nitrided to enhance the atomic activity and free force field on the material surface. Furthermore, the micropores of the carbon nanotubes after ball milling and nitridation can adsorb a large amount of gas because the pore walls of this material have adsorptive properties, which can increase the gas density and store hydrogen by capillary action and surface adsorption.

[0023] In some possible implementations, the volume ratio of the aromatic compound, the polyol, and the organic solvent in the dispersed component of step (4) is (3.5-6): (2-4): (1.5-3).

[0024] In some possible implementations, the aromatic compound is benzene; the polyol is polyethylene glycol or polypropylene glycol with a molecular weight of 200-600; and the organic solvent is methanol.

[0025] In some possible implementations, in step (4), the stirring paddle is driven by a motor to rotate so that the materials are fully and evenly mixed, the rotation speed is 100-150 rpm, and the stirring time is 30-40 hours. The stirring process causes convection of the mixed materials. The rotation of the stirring paddle drives the materials to form a circulation flow in the kettle, so that the materials are fully mixed.

[0026] In some possible implementations, in step (5), the mass ratio of carbon nitride nanotubes to magnesium nitride is (8-15):1.

[0027] In the reaction system of the present invention, magnesium nitride is an ionic compound and will react with water to produce ammonia. By adding an aromatic compound, it is possible to avoid unnecessary chemical reactions caused by the contact between the nitride and water during the reaction.

[0028] In some possible implementations, in step (5), the stirring is driven by a turbine agitator in the reactor to rotate and stir, first stirring at a speed of 40-80 rpm for 3-10 h, and then increasing the speed to 150-220 rpm for 7-15 h, thereby achieving multiple shearing effects on the carbon nanotubes, cutting them into smaller structures to fully increase their contact area.

[0029] In some possible implementations, in step (5), the heating is to first heat the reaction system to 35-55°C, and react at a rotation speed of 90-110 rpm for 1-3 h; then heat it to 60-70°C, and react at a rotation speed of 50-70 rpm for 0.5-1.5 h; then continue to heat it to 75-90°C, and react at a rotation speed of 20-40 rpm for 20-30 h.

[0030] In some possible implementations, in step (5), the process of product molding and packaging is to first lay the molding template flat on the operating table, then press the material obtained after the heating reaction into the template channel, and after compaction, cover it with a layer of microporous filter plate with a thickness of 20 mm. After the material in the channel shrinks and hardens, the surface is coated with a nano breathable membrane to complete the product packaging.

[0031] In some possible implementations, the hole may be circular or square, which can be adjusted according to actual needs.

[0032] In the above process, the filter plate needs to be compacted with tooling on all sides, and the operating table mold frame corresponding to the microporous filter plate is covered with micropores for releasing nitrogen from under the operating table. Nitrogen is sprayed into the template from the micropores to further nitride the material in the template, ensuring that the pore structure morphology inside the carbon nanotube pore diameter and the tube wall cavity is full, and the void size and distribution are reasonable.

[0033] The beneficial effects of the technical solution provided by the embodiment of the present invention include at least:

[0034] (1) The composite hydrogen storage material prepared by the method of the present invention has mild hydrogen storage conditions (hydrogen storage pressure of 0.3Mpa, temperature of 270K and voltage of 24V), which is more suitable for commercial use than other hydrogen storage materials that require special hydrogen storage conditions such as high temperature and high pressure;

[0035] (2) The composite hydrogen storage material prepared by the method of the present invention can simultaneously use surface adsorption hydrogen storage and capillary action hydrogen storage, and has a higher hydrogen storage density and lighter weight, so it is easy to carry and can improve its commercial application potential;

[0036] (3) The composite hydrogen storage material prepared by the method of the present invention has high mechanical properties and high specific surface area, large volume pores, and long service life. In addition, the preparation process is mild, the equipment is simple and easy to operate, and it is suitable for large-scale production, which also provides great convenience for future commercial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1-Figure 4 They are respectively the particle pore width curves of the hydrogen storage materials provided in Examples 1-4;

[0038] Figure 5-Figure 8 They are respectively the cumulative pore volume curves of the hydrogen storage materials provided in Examples 1-4;

[0039] Figure 9-11 They are respectively the particle pore width curves of the hydrogen storage materials provided in Comparative Examples 1-3;

[0040] Figure 12-14 They are the cumulative pore volume curves of the hydrogen storage materials provided in Comparative Examples 1-3 respectively. DETAILED DESCRIPTION

[0041] In order to make the technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below.

[0042] Embodiment 1:

[0043] (1) Multi-walled carbon nanotubes MWCNT-KKD-001 (diameter <2 nm) were placed in a ball mill and milled in a star-shaped ball mill (80L model produced by Nanjing University) under a 0.3 MPa ammonia atmosphere. The ball milling medium was 20 steel balls, the ball milling time was 10 h, the ball milling speed was 300 rpm, and the mixing mass ratio of the ball milling medium to the carbon nanotubes was 60:1.

[0044] (2) placing the milled carbon nanotubes into a pressure cooker and injecting deionized water into the pressure cooker and heating to 90°C, repeatedly heating for three times, maintaining the temperature for 30, 60 and 120 minutes each time, and then drying;

[0045] (3) placing the dried carbon nanotubes in a muffle furnace for high temperature treatment at 500° C., and injecting nitrogen into the closed furnace chamber of the muffle furnace to nitride the carbon nanotubes in a heated environment to obtain nitrided carbon nanotubes;

[0046] (4) Add 4.2 L of benzene, 3.1 L of polyethylene glycol (molecular weight 200) and 2.9 L of methanol into the reactor, and drive the stirring paddle to rotate by a motor to mix the materials thoroughly and evenly. The speed is 100 rpm and the stirring time is 40 h. After thorough mixing, dispersed components are obtained.

[0047] (5) 9.2 kg of carbon nitride nanotubes and 0.8 kg of magnesium nitride were added to a reactor, and the stirring and rotation were driven by a turbine agitator in the reactor. The mixture was stirred at a speed of 40 rpm for 10 h, and then increased to 220 rpm for 8 h. After stirring evenly, stirring and heating were continued. The reaction system was first heated to 35°C and reacted at a speed of 90 rpm for 3 h; then heated to 65°C and reacted at a speed of 70 rpm for 1 h; then heated to 90°C and reacted at a speed of 30 rpm for 25 h. After the reaction was completed, the molded template was first spread on the operating table, and the material obtained after the heating reaction was pressed into the template pores. After compaction, a microporous filter plate with a thickness of 20 mm was covered. After the material in the pores shrank and hardened, a nano breathable membrane was coated on the surface to complete product packaging, thereby preparing the carbon nitride nanotube composite hydrogen storage material A described in the present invention.

[0048] Embodiment 2:

[0049] (1) Multi-walled carbon nanotubes MWCNT-KKD-001 (diameter <2 nm) were placed in a ball mill and milled in a star-shaped ball mill (80L model produced by Nanjing University) under a 0.5 MPa ammonia atmosphere. The ball milling medium was 30 steel balls, the ball milling time was 15 h, the ball milling speed was 350 rpm, and the mixing mass ratio of the ball milling medium to the carbon nanotubes was 70:1.

[0050] (2) placing the milled carbon nanotubes into a pressure cooker and injecting deionized water into the pressure cooker and heating to 100°C, repeatedly heating for three times, maintaining the temperature for 30, 60 and 120 minutes each time, and then drying;

[0051] (3) placing the dried carbon nanotubes in a muffle furnace for high temperature treatment at 550° C., and injecting nitrogen into the closed furnace chamber of the muffle furnace to nitride the carbon nanotubes in a heated environment to obtain nitrided carbon nanotubes;

[0052] (4) Add 3.5 L of benzene, 2.7 L of polypropylene glycol (molecular weight 300) and 2 L of methanol into the reactor, and drive the stirring paddle to rotate by a motor to mix the materials thoroughly and evenly. The speed is 120 rpm and the stirring time is 35 h. After thorough mixing, dispersed components are obtained.

[0053] (5) 7.8 kg of carbon nitride nanotubes and 0.6 kg of magnesium nitride were added to a reactor, and the stirring was driven by a turbine agitator in the reactor. The mixture was stirred at 50 rpm for 8 h, and then increased to 200 rpm for 10 h. After the mixture was evenly stirred, the stirring and heating were continued. The reaction system was first heated to 40°C and reacted at 100 rpm for 2 h; then heated to 60°C and reacted at 50 rpm for 0.5 h; then heated to 75°C and reacted at 40 rpm for 20 h. After the reaction was completed, the molded template was first spread on the operating table, and the material obtained after the heating reaction was pressed into the template pores. After compaction, a microporous filter plate with a thickness of 20 mm was covered. After the material in the pores shrank and hardened, a nano-breathable membrane was coated on the surface to complete the product packaging, thereby preparing the carbon nitride nanotube composite hydrogen storage material B described in the present invention.

[0054] Embodiment 3:

[0055] (1) Multi-walled carbon nanotubes MWCNT-KKD-001 (diameter <2 nm) were placed in a ball mill and milled in a star-shaped ball mill (80L model produced by Nanjing University) under an ammonia atmosphere of 0.8 MPa. The ball milling medium was 40 steel balls, the ball milling time was 20 h, the ball milling speed was 400 rpm, and the mixing mass ratio of the ball milling medium to the carbon nanotubes was 80:1.

[0056] (2) placing the milled carbon nanotubes into a pressure cooker and injecting deionized water into the pressure cooker and heating to 110°C, repeatedly heating for three times, maintaining the temperature for 30, 60 and 120 minutes each time, and then drying;

[0057] (3) placing the dried carbon nanotubes in a muffle furnace for high temperature treatment at 600° C., and injecting nitrogen into the closed furnace chamber of the muffle furnace to nitride the carbon nanotubes in a heated environment to obtain nitrided carbon nanotubes;

[0058] (4) Add 6 L of benzene, 3.6 L of polyethylene glycol (molecular weight 400) and 2.5 L of methanol into the reactor, and drive the stirring paddle to rotate by a motor to mix the materials thoroughly and evenly. The speed is 150 rpm and the stirring time is 30 h. After thorough mixing, dispersed components are obtained.

[0059] (5) 12 kg of carbon nitride nanotubes and 1.5 kg of magnesium nitride are added to a reactor, and the turbine agitator in the reactor is used to drive the stirring and rotation. The stirring is first performed at a speed of 80 rpm for 5 h, and then the speed is increased to 180 rpm for 12 h. After the stirring is uniform, the stirring and heating are continued. The reaction system is first heated to 45°C and reacted at a speed of 110 rpm for 1 h; then the temperature is increased to 60°C and reacted at a speed of 55 rpm for 1.5 h; then the temperature is continued to be increased to 80°C and reacted at a speed of 20 rpm for 30 h. After the reaction is completed, the forming template is first spread flat on the operating table, and then the material obtained after the heating reaction is pressed into the template pores. After compaction, a microporous filter plate with a thickness of 20 mm is covered. After the material in the pores shrinks and hardens, the surface is coated with a nano breathable membrane to complete the product packaging, thereby preparing the carbon nitride nanotube composite hydrogen storage material C of the present invention.

[0060] Embodiment 4:

[0061] (1) Multi-walled carbon nanotubes MWCNT-KKD-001 (diameter <2 nm) were placed in a ball mill and milled in a star-shaped ball mill (80L model produced by Nanjing University) under an ammonia atmosphere of 0.8 MPa. The ball milling medium was 50 steel balls, the ball milling time was 20 h, the ball milling speed was 500 rpm, and the mixing mass ratio of the ball milling medium to the carbon nanotubes was 100:1.

[0062] (2) placing the milled carbon nanotubes into a pressure cooker and injecting deionized water into the pressure cooker and heating to 120°C, repeatedly heating for three times, maintaining the temperature for 30, 60 and 120 minutes each time, and then drying;

[0063] (3) placing the dried carbon nanotubes in a muffle furnace for high temperature treatment at 650° C., and injecting nitrogen into the closed furnace chamber of the muffle furnace to nitride the carbon nanotubes in a heated environment to obtain nitrided carbon nanotubes;

[0064] (4) Add 3.5 L of benzene, 2.5 L of polyethylene glycol (molecular weight 600) and 1.8 L of methanol into the reactor, and drive the stirring paddle to rotate by a motor to mix the materials thoroughly and evenly. The speed is 130 rpm and the stirring time is 35 h. After thorough mixing, dispersed components are obtained.

[0065] (5) 20 kg of carbon nitride nanotubes and 2 kg of magnesium nitride were added to a reactor, and the turbine agitator in the reactor was used to drive the stirring and rotation. The stirring was first performed at a speed of 60 rpm for 5 h, and then the speed was increased to 150 rpm for 15 h. After the stirring was uniform, the stirring and heating were continued. The reaction system was first heated to 55°C and reacted at a speed of 90 rpm for 2 h; then the temperature was increased to 65°C and reacted at a speed of 65 rpm for 1 h; then the temperature was continued to be increased to 75°C and reacted at a speed of 30 rpm for 25 h. After the reaction was completed, the forming template was first spread flat on the operating table, and then the material obtained after the heating reaction was pressed into the template pores. After compaction, a microporous filter plate with a thickness of 20 mm was covered. After the material in the pores shrank and hardened, a nano breathable membrane was coated on the surface to complete the product packaging, and the carbon nitride nanotube composite hydrogen storage material D of the present invention was prepared.

[0066] Comparative Example 1: Compared with Example 1, the difference is that in step (1), multi-walled carbon nanotubes are MWCNT-S33198 (diameter>10 nm) and are ball-milled in an argon atmosphere.

[0067] Comparative Example 2: Compared with Example 1, the difference is that the dispersed component in step (4) is formed by uniformly mixing 2L of benzene, 5L of polyethylene glycol and 1L of methanol; and the mass ratio of carbon nitride nanotubes to magnesium nitride in step (5) is 20:1.

[0068] Comparative Example 3: Compared with Example 1, the difference is that in step (5), the heating is to directly heat the system to 90°C and react at a speed of 30 rpm for 29 hours; when the product is formed and packaged, after the material in the channel shrinks and hardens, the nano breathable membrane is not coated on its surface.

[0069] Performance Testing:

[0070] The particle pore width curve and cumulative pore volume curve of the hydrogen storage materials prepared in the above Examples 1-4 and Comparative Examples 1-3 measured by the micropore method under the conditions of hydrogen storage pressure of 0.3Mpa, temperature of 270K and voltage of 24V are shown in the accompanying drawings of the specification.

[0071] about Figure 1-14 The gap width displayed on the horizontal axis is the particle size width, in nm. The units of the vertical axis on the left are all cc / g, and the units of the vertical axis on the right (if any) are all cc / nm / g.

[0072] from Figure 1 and Figure 5 It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Example 1 is 0 when the particle size width is 0.3-0.8nm, the peak value of the left coordinate is 0.084cc / g when the particle size width is 0.8-1nm, the peak value of the left coordinate is 0.00cc / g when the particle size width is 1.5-1.8nm, and the peak value of the left coordinate is 0.01cc / g when the particle size width is 1.8-2nm. The cumulative pore volume is 980cc / g, and the hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 8.75wt%; Figure 1 , its horizontal values ​​are 0.00, 0.40, 0.80, 1.20, 1.60, 2.00, 2.40, increasing to 4.00, and the last value is 4.27. The vertical coordinates on the left are 0.0000, 0.4000, 0.8000, 1.2000, 1.3400 from bottom to top, and the vertical coordinates on the right are 0.0000, 1.7313, 3.4627, 5.1940, 5.8000 from bottom to top;

[0073] from Figure 2 and Figure 6 It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Example 2 is 0 when the particle size width is 0.3-0.8nm, the peak value of the left coordinate is 0.09cc / g when the particle size width is 0.8-1nm, and the peak value of the left coordinate is 0.012cc / g when the particle size width is 1.6-2nm. The cumulative pore volume is 920cc / g, and the hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 8.21wt%; Figure 2 , its horizontal values ​​are 0.00, 0.40, 0.80, 1.20, 1.60, 2.00, 2.40, increasing to 4.00, and the last value is 4.27. The vertical coordinates on the left are 0.0000, 0.4000, 0.8000, 0.1200, 0.1600 from bottom to top, and the vertical coordinates on the right are 0.0000, 0.0750, 0.1500, 0.2250, 0.3000 from bottom to top;

[0074] about Figure 6 , its horizontal coordinates are 0.00, 0.40, 0.80, 1.09, and the vertical coordinates on the left are 0.00, 40.00, 80.00, 120.00, and increase to 840.00 from bottom to top;

[0075] from Figure 3 and Figure 7It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Example 3 is 0 when the particle size width is 0.3-0.8nm, the peak value of the left coordinate is 0.18cc / g when the particle size width is 0.8-1.4nm, and the peak value of the left coordinate is 0.02cc / g when the particle size width is 2-2.4nm. The cumulative pore volume is 960cc / g, and the hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 8.57wt%; Figure 3 , its horizontal values ​​are 0.00, 0.40, 0.80, 1.20, 1.60, 2.00, 2.40, increasing to 4.00, and the last value is 4.27. The vertical coordinates on the left are 0.0000, 0.4000, 0.8000, 1.0200 from bottom to top, and the vertical coordinates on the right are 0.0000, 1.9843, 3.9686, 5.0600 from bottom to top;

[0076] about Figure 7 , its horizontal coordinates are 0.00, 0.40, 0.80, 1.09, and the vertical coordinates on the left are 0.00, 40.00, 80.00, 120.00, and increase to 920.00 from bottom to top;

[0077] from Figure 4 and Figure 8 It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Example 4 is 0.015cc / g when the particle size width is in the ultra-micropore state of 0.3-0.5nm, the peak value of the left coordinate is 0.11cc / g when the particle size width is 0.8-1.2nm, and the peak value of the left coordinate is 0.05cc / g when the particle size width is 1.2-1.6nm. The cumulative pore volume is 1000cc / g, and the hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 8.93wt%;

[0078] about Figure 4 The horizontal values ​​are 0.00, 0.40, 0.80, 1.20, 1.60, 2.00, 2.40, increasing to 4.00, and the last value is 4.27. The vertical coordinates on the left are 0.0000, 0.0080, 0.0120, 0.0160, increasing to 0.0960 from bottom to top, and the vertical coordinates on the right are 0.0000, 0.0165, 0.02 47, 0.0330, 0.0412, 0.0495, 0.0577, 0.0660, 0.0742, 0.0825, 0.0907, 0.0990, 0.1072, 0.1155, 0.1237, 0.1320, 0.1402, 0.1485, 0.1567, 0.1650, 0.1732, 0.1815, 0.1897, 0.1980;

[0079] about Figure 8 , its horizontal coordinates are 0.00, 0.40, 0.80, 1.09, and the vertical coordinates on the left are 0.00, 40.00, 80.00, 120.00, and increase to 840.00 from bottom to top;

[0080] from Fig. 9 and Fig.12 It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Comparative Example 1 is 0 when the particle size width is 0.3-0.8nm, the peak value of the left coordinate is 0.084cc / g when the particle size width is 0.8-1nm, the peak value of the left coordinate is 0.00cc / g when the particle size width is 1.5-1.8nm, and the peak value of the left coordinate is 0.01cc / g when the particle size width is 1.8-2nm, and the cumulative pore volume is 460cc / g. The hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 4.11wt%;

[0081] from Fig.10 and Fig.13 It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Comparative Example 2 is 0 when the particle size width is 0.3-0.8nm, the peak value of the left coordinate is 0.09cc / g when the particle size width is 0.8-1nm, and the peak value of the left coordinate is 0.012cc / g when the particle size width is 1.6-2nm, and the cumulative pore volume is 560cc / g. The hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 5wt%;

[0082] from Fig.11 and Fig.14 It can be seen that the peak value of the left coordinate of the hydrogen storage material provided in Comparative Example 3 is 0 when the particle size width is 0.3-0.8nm, the peak value of the left coordinate is 0.18cc / g when the particle size width is 0.8-1.4nm, and the peak value of the left coordinate is 0.02cc / g when the particle size width is 2-2.4nm, and the cumulative pore volume is 660cc / g. The hydrogen storage mass capacity of the hydrogen storage material under the test conditions is 5.89wt%; Fig.14 , its horizontal coordinates are 0.00, 0.40, 0.80, 1.09, and the vertical coordinates on the left are 0.00, 40.00, 80.00, 120.00, and increase to 680.00 from bottom to top;

[0083] It can be seen that when the particle width is in a mesoporous state (greater than 2nm), the cumulative pore volume will be greatly reduced; conversely, when the particle width is in a microporous state (less than 2nm), the cumulative pore volume will increase accordingly; it is emphasized that when the particle width is in an ultramicroporous state (less than 0.7nm), the cumulative pore volume will increase significantly. In addition, the carbon nitride nanotube composite hydrogen storage material prepared by the method of the present invention can achieve a hydrogen storage mass capacity of 8.93wt% under the conditions of a hydrogen storage pressure of 0.3Mpa, a temperature of 270K and a voltage of 24V. Further, the inventors have found that the hydrogen storage mass capacity of the composite hydrogen storage material under high pressure (such as 1Mpa pressure) can reach 15.2wt%.

[0084] Note: The volume mass of carbon nitride nanotubes is 2.1 kg / m 3 The calculation method of the hydrogen storage mass capacity of the above hydrogen storage material is as follows: The actual gas molar amount (mol) that 1g carbon nitride nanotube can accommodate = 1g carbon nitride nanotube cumulative pore volume (cc) / standard gas molar volume (22.4L / mol) × 10 -3 , and then the actual hydrogen storage mass that 1g of carbon nitride nanotubes can hold (g) is obtained by multiplying the molar mass of gas that 1g of carbon nitride nanotubes can actually hold (mol) by the molar mass of hydrogen (2g / mol), and from this, the hydrogen storage mass capacity of the hydrogen storage material is calculated = the actual hydrogen storage mass that carbon nitride nanotubes can hold (g) / the mass of carbon nitride nanotubes (g) × 100%, which is numerically equal to the actual hydrogen storage mass that 1g of carbon nitride nanotubes can actually hold (g) × 100%.

[0085] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a carbon nitride nanotube composite hydrogen storage material, characterized in that: The preparation method comprises the following steps: (1) Placing carbon nanotubes into a ball mill for mechanical ball milling; (2) wet-treating the milled carbon nanotubes and then drying them; (3) placing the dried carbon nanotubes in a muffle furnace for nitridation treatment to obtain nitrided carbon nanotubes; (4) adding an aromatic compound, a polyol and an organic solvent into a reaction kettle and mixing them thoroughly to obtain a dispersed component; (5) adding carbon nitride nanotubes and magnesium nitride into a reaction kettle, stirring evenly and then continuing to stir and heat, and after the reaction is completed, forming and packaging the product to prepare the carbon nitride nanotube composite hydrogen storage material; The carbon nanotubes in step (1) have a diameter of less than 2 nm and are subjected to mechanical ball milling in an ammonia atmosphere; The volume ratio of the aromatic compound, the polyol and the organic solvent in the dispersed component of step (4) is (3.5-6): (2-4): (1.5-3); In step (5), the mass ratio of carbon nitride nanotubes to magnesium nitride is (8-15):1; In step (5), the heating is to first heat the reaction system to 35-55°C, react at a speed of 90-110 rpm for 1-3h; then heat to 60-70°C, react at a speed of 50-70 rpm for 0.5-1.5h; then continue to heat to 75-90°C, react at a speed of 20-40 rpm for 20-30h; In step (5), the product molding and packaging process includes shrinking and hardening the hydrogen storage material obtained after the reaction, and then coating the surface of the material with a nano breathable membrane.

2. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: The carbon nanotubes in step (1) are multi-walled carbon nanotubes or single-walled carbon nanotubes.

3. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: In step (1), the mechanical ball milling is carried out in a star-shaped ball mill under an atmosphere of 0.3-0.8 MPa, the ball milling medium is 20-50 steel balls, the ball milling time is 10-30 hours, and the ball milling speed is 300-500 revolutions per minute; during the ball milling treatment, the mixing mass ratio of the ball milling medium to the carbon nanotubes is (60-100):

1.

4. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: In step (2), the wet treatment is to place the milled carbon nanotubes into a pressure cooker and inject deionized water to heat to 90-120° C., and repeat the heating for more than three times, with each heating maintaining a constant temperature for 30-120 minutes.

5. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: In step (3), the nitridation treatment is to place the dried carbon nanotubes into a muffle furnace for high temperature treatment at 500-650°C, and nitrogen is injected into the closed furnace chamber of the muffle furnace to allow the carbon nanotubes to be nitrided in a heated environment.

6. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: The aromatic compound is benzene; the polyol is polyethylene glycol or polypropylene glycol with a molecular weight of 200-600; and the organic solvent is methanol.

7. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 6, characterized in that: In step (4), the stirring paddle is driven by a motor to rotate so that the materials are fully and evenly mixed, the rotation speed is 100-150 rpm, and the stirring time is 30-40 hours.

8. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: In step (5), the stirring is driven by a turbine agitator in the reaction kettle to stir and rotate, first stirring at a speed of 40-80 rpm for 3-10 h, and then increasing the speed to 150-220 rpm for 7-15 h.

9. The method for preparing a carbon nitride nanotube composite hydrogen storage material according to claim 1, characterized in that: In step (5), the process of product molding and packaging is to first lay the molding template flat on the operating table, then press the material obtained after the heating reaction into the template channel, and after compaction, cover it with a layer of microporous filter plate with a thickness of 20 mm. After the material in the channel shrinks and hardens, the surface is coated with a nano breathable membrane to complete the product packaging.