Silicon-carbon composite negative electrode material and preparation method thereof
By depositing magnesium, silicon and carbon source gases in foam copper, and combining boron source gas and plasma excitation technology, nano-silicon-porous silicon-carbon composites are formed, which solves the problem of poor fast charging performance of new silicon carbon materials and achieves high Capacity, low expansion and good circulation performance improve the overall performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202411047429.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing new silicon carbon materials have shortcomings in fast charging performance. The poor electronic conductivity leads to a decrease in battery performance, and the material expands after doping metal or non-metallic materials, affecting the cycling stability of the battery.
A preparation method is adopted to form a magnesium silicate structure by depositing magnesium, silicon and carbon source gas in foam copper, combining with boron source gas to increase conductivity, and nano-silicon-porous silicon carbon is formed through plasma excitation and passivation reactions. Composites ensure the structural stability and conductivity of the material.
The silicon-carbon composite anode material with high specific capacity, low expansion, good circulation and high temperature storage has been achieved, which significantly improves the fast charging performance of lithium-ion batteries and the overall performance of the battery.
Smart Images

Figure CN118579791B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery materials, and in particular relates to a silicon-carbon composite negative electrode material and a preparation method thereof. Background Art
[0002] The new silicon-carbon is mainly produced by the cracking of silane to generate nano-silicon and deposited in porous carbon. Its specific capacity is mainly provided by nano-silicon (about 3500mAh / g), while porous carbon mainly provides buffer space and its specific capacity is relatively low (200mAh / g). The two are combined to prepare a new silicon-carbon material to achieve a balance in specific capacity, expansion and impedance.
[0003] The current new silicon carbon has defects such as poor electronic conductivity, which reduces its fast charging performance. The main measures to improve the fast charging performance are to dope metals (magnesium, lithium, etc.) or non-metallic materials (nitrogen, boron, etc.) in porous carbon to improve the electronic conductivity of the material. Although the impedance is reduced, the reduction is limited and will cause the material to expand. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a silicon-carbon composite negative electrode material and a preparation method thereof, aiming to solve the problem of poor fast charging performance of battery negative electrode materials.
[0005] To solve the above technical problems, the present invention is implemented as follows: the present invention provides a preparation method for preparing a silicon-carbon composite negative electrode material, the preparation method comprising the steps of:
[0006] S1. Preheating the foamed copper in a vacuum environment, and then introducing a mixed gas to perform a first deposition reaction, wherein the mixed gas is a mixture of a boron source gas, a magnesium source gas, a silicon source gas, and a carbon source gas;
[0007] S2, adding tetrahydrofuran to remove the foamed copper to obtain a porous silicon-carbon composite matrix;
[0008] S3, transferring the porous silicon-carbon composite substrate to a reactor in an inert atmosphere, introducing silane gas to perform a second deposition reaction, and obtaining a nano-silicon-porous silicon-carbon composite;
[0009] S4, introducing a carbon source gas to passivate the nano-silicon-porous silicon-carbon composite, and obtaining the silicon-carbon composite negative electrode material after cooling.
[0010] In some embodiments of the present invention, the volume ratio of each component in the mixed gas is boron source gas: magnesium source gas: silicon source gas: carbon source gas = 1-5: 10-30: 20-40: 20-40.
[0011] In some embodiments of the present invention, the boron source gas is diborane;
[0012] The magnesium source gas is magnesium hydride;
[0013] The silicon source gas includes at least one of monosilane gas, disilane gas, trichlorosilane, tetrachlorosilane, dimethylsilane, and hexachlorodisilane;
[0014] The carbon source gas includes one of acetylene, propyne, ethylene, propylene, methane and ethane.
[0015] In some embodiments of the present invention, the pore size of the copper foam is in the range of 0.1 mm to 10 mm, the porosity is 50% to 90%, and the volume density is 0.1 to 0.5 g / cm3.
[0016] In some embodiments of the present invention, in step S1, the preheating temperature is 1000°C-1400°C, the flow rate of the mixed gas is 100-1000 ml / min, and the reaction time of the first deposition reaction is 1-12 hours.
[0017] In some embodiments of the present invention, in step S3, the step of transferring the porous silicon-carbon composite substrate to a reactor in an inert atmosphere comprises:
[0018] The porous silicon-carbon composite matrix is transferred to a reaction kettle and atomized, wherein the reaction kettle is filled with an inert gas and has gas and temperature regulating capabilities;
[0019] Passing the atomized porous silicon-carbon composite matrix into the reaction kettle for plasma excitation;
[0020] Acquiring a characteristic spectrum of a product of the porous silicon-carbon composite matrix after excitation, and analyzing the characteristic spectrum of the product;
[0021] The internal parameters of the reactor are adjusted according to the analysis results of the characteristic spectrum of the product.
[0022] In some embodiments of the present invention, the step of analyzing the characteristic spectrum of the product includes:
[0023] Acquire standard characteristic spectra in the selected wavelength range;
[0024] Calculating the spectral standard factor within the selected wavelength range and drawing a response curve, wherein the spectral standard factor is the ratio of the standard characteristic spectrum to the standard light intensity, and the response curve is a relationship curve between each wavelength within the wavelength range and the spectral standard factor;
[0025] Substitute the characteristic spectrum of the product into the response curve to obtain the analysis result of the characteristic spectrum of the product.
[0026] In some embodiments of the present invention, in the step S3, the step of introducing silane gas to perform a second deposition reaction includes:
[0027] Introducing silane gas into the reactor to carry out the second deposition reaction, the reaction time is 60-600 min, and the reaction temperature is 400-600° C.;
[0028] Obtaining real-time information of reactants in the reactor;
[0029] The reaction parameters of the second deposition reaction are adjusted according to the real-time information, wherein the reaction parameters include radio frequency power, reaction temperature and pressure in the reactor.
[0030] In some embodiments of the present invention, step S4 specifically includes:
[0031] Discharging the silane gas in the reactor and setting the temperature of the reactor to 600-900° C.;
[0032] The carbon source gas is introduced to carry out a passivation reaction, and the reaction time is 60 to 600 minutes;
[0033] According to the preset cooling curve, the target temperature and cooling rate of each stage are set, wherein the target temperature and cooling rate of any two stages are different.
[0034] The present invention also provides a silicon-carbon composite negative electrode material, which is prepared by the preparation method as described above, and the silicon-carbon composite negative electrode material comprises:
[0035] The inner core is porous silicon carbon, and the inner core has a porous structure;
[0036] A nano silicon layer, located in the pore structure;
[0037] A carbon coating layer is coated on the outer surface of the inner core and the nano silicon layer.
[0038] Compared with the prior art, the silicon-carbon composite negative electrode material and the preparation method thereof in the present invention have the following beneficial effects:
[0039] Magnesium and silicon are deposited in copper foam to form magnesium silicate to improve the structural stability of the material. Boron source improves the electronic conductivity of the material. Carbon source is coated on the surface of nano-silicon to improve the electronic conductivity and prevent oxidation. The synergistic effect between boron, silicon, carbon and magnesium is brought into play to achieve a performance balance between specific capacity, expansion and rate. Using copper foam as a template, taking advantage of its large pore size and pore volume, large-pore boron-magnesium doped porous silicon carbon is prepared, which has the advantages of low expansion and low impedance. Passivation and carbon coating on the surface of its core reduce gas production and improve the initial efficiency of the material. Silicon-carbon composite negative electrode materials are used in lithium-ion batteries, with the advantages of high specific capacity, low expansion, good cycle, and good high-temperature storage, which effectively improves the fast charging performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 Schematic diagram of the process of silicon-carbon composite negative electrode material in one embodiment of the present invention;
[0041] Figure 2 yes Figure 1 Schematic diagram of the specific steps of step S3;
[0042] Figure 3 This is a SEM image of the silicon-carbon composite negative electrode material in Example 1 of the present invention. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0044] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0045] Embodiment 1:
[0046] Please refer to Figure 1 and Figure 2 The present invention proposes a preparation method for preparing a silicon-carbon composite negative electrode material, and the steps of the preparation method include:
[0047] Step S1, preheating the foam copper in a vacuum environment, and then introducing a mixed gas to perform a first deposition reaction, wherein the mixed gas is a mixture of a boron source gas, a magnesium source gas, a silicon source gas, and a carbon source gas.
[0048] Magnesium and silicon are deposited in copper foam to form magnesium silicate to improve the structural stability of the material, the boron source improves the electronic conductivity of the material, and the carbon source is coated on the surface of nano-silicon to improve the electronic conductivity and prevent it from being oxidized. The synergistic effect between boron, silicon, carbon and magnesium is brought into play to achieve a performance balance between specific capacity, expansion and rate. Using copper foam as a template and its large pore size and pore volume, large-pore boron-magnesium-doped porous silicon carbon is prepared, which has the advantages of low expansion and low impedance.
[0049] Preheating can increase the surface activity of copper foam, which is beneficial for the better deposition of each source gas in the mixed gas on the surface of copper foam, improving the deposition efficiency and the adhesion of the material, thereby obtaining a composite material with a dense and stable structure. The preheating operation can also reduce the activation energy of the deposition reaction, so that elements such as silicon and carbon in the mixed gas can more easily undergo chemical reactions and physical deposition on the surface of copper foam, thereby promoting the first deposition reaction.
[0050] The volume ratio of each component in the mixed gas is 2:20:30:30:30. The boron source gas is diborane gas, the magnesium source gas is magnesium hydride gas, the silicon source gas is monosilane gas, the carbon source gas is acetylene gas, and the flow rate of the mixed gas is 500 ml / min.
[0051] The specifications of the copper foam used are 2mm pore size, 60% porosity, 0.3g / cm3 volume density, 100g mass of copper foam, vacuuming of copper foam, the reaction temperature of the first deposition reaction is 1200℃, and the reaction time is 6 hours. The proportion of different components is set to ensure that the silicon-carbon composite negative electrode material has a high capacity while improving its conductivity, structural stability and cycle life.
[0052] The appropriate pore size helps to provide stronger structural support capabilities, ensure the integrity and stability of the material during deposition and subsequent processing, and is also conducive to the uniform deposition of silicon and carbon source gases, avoiding the formation of large holes or defects in the material, thereby improving the mechanical strength and electrochemical properties of the material. High porosity can provide more channels, facilitate the rapid transmission of lithium ions, reduce the internal resistance of electrode materials, and improve the rate performance of batteries. As a low-density material, copper foam has good uniformity and excellent electronic conductivity, which can ensure uniform coverage of silicon-carbon composite materials during the deposition process, avoid the problem of inconsistent material properties, and at the same time utilize the high electronic conductivity of copper itself to improve the rate performance.
[0053] Step S2: adding tetrahydrofuran to remove the foamed copper to obtain a porous silicon-carbon composite matrix.
[0054] 1000g of tetrahydrofuran solution is added, and the deposited copper foam is immersed in tetrahydrofuran for 48 hours. Tetrahydrofuran is an effective organic solvent that can dissolve and remove the copper foam, so that the copper component in the silicon-carbon composite matrix is completely removed. This removal method is simple to operate and can ensure the efficiency and integrity of the removal process.
[0055] Moreover, in the process of removing the copper foam, tetrahydrofuran can maintain the porous structure of the silicon-carbon composite matrix, which is conducive to the rapid transmission of lithium ions and the efficient conduction of electrons, improving the electrochemical performance of electrode materials. Porous silicon-carbon composite matrices usually have a large specific surface area, which helps to increase the active sites for lithium ion embedding / de-embedding, improve the capacity and rate performance of the material, and a larger specific surface area can also provide more contact interfaces, improving the conductivity of the material and the overall performance of the battery.
[0056] Step S3, transferring the porous silicon-carbon composite substrate to a reaction vessel with an inert atmosphere, introducing silane gas to perform a second deposition reaction, and obtaining a nano-silicon-porous silicon-carbon composite.
[0057] The porous silicon-carbon composite matrix soaked in tetrahydrofuran removes most of the foamed copper, but there is still a risk of residual foamed copper. The remaining foamed copper has a high conductivity, which is different from the conductivity of the porous silicon-carbon composite matrix. Excessive residual copper ions will lead to uneven conduction paths, affecting the stability of the overall conductivity of the material, not only increasing the internal resistance of the material, but also causing local hot spots, affecting battery performance.
[0058] Therefore, the following steps are required to detect and eliminate copper ions in the porous silicon-carbon composite matrix.
[0059] Step S3.1, transfer the porous silicon-carbon composite matrix to a reactor and atomize it, wherein an inert gas is introduced into the reactor and the reactor has gas and temperature regulation capabilities. The reactor is made of high temperature and vacuum resistant materials, such as quartz or high temperature alloy materials. The reaction vessel can be a three-dimensional rotating mixer, providing multi-directional mixing action rather than a single axial mixing method. The reactor is equipped with a programmable temperature control and gas flow sensor for precise temperature control and gas flow regulation.
[0060] The reactor is also equipped with a built-in atomizer to atomize the porous silicon-carbon composite matrix into fine droplets to form a uniform aerosol, thereby ensuring that the porous silicon-carbon composite matrix is evenly distributed in the plasma and improving the accuracy and precision of the analysis.
[0061] Step S3.2: The atomized porous silicon-carbon composite substrate is introduced into a reaction vessel for plasma excitation; the equipment for plasma excitation may be a radio frequency inductively coupled plasma equipment, a direct current plasma equipment or a microwave plasma equipment. The excitation process needs to be carried out in an inert atmosphere, and the inert gas may be argon.
[0062] Step S3.3, obtaining the characteristic spectrum of the product of the porous silicon-carbon composite matrix after excitation, and analyzing the characteristic spectrum of the product. The aerosol particles are excited in the plasma, and each element in the porous silicon-carbon composite matrix emits a characteristic spectrum, which is detected by a spectrometer to achieve qualitative and quantitative analysis of the elements.
[0063] Step S3.4, obtain a standard characteristic spectrum within the selected wavelength range. In the absence of a sample, run the spectrometer to collect background spectrum data. Record the light intensity value of the background spectrum and save the background spectrum data. Select a standard sample for measurement, subtract the background spectrum data from the sample spectrum, and thus obtain a standard characteristic spectrum.
[0064] Step S3.5, calculate the spectral standard factor within the selected wavelength range and draw a response curve, wherein the spectral standard factor is the ratio of the standard characteristic spectrum to the standard light intensity, and the response curve is a relationship curve between each wavelength within the wavelength range and the spectral standard factor.
[0065] In order to improve the accuracy and repeatability of the spectral standard factors, multiple measurements were performed on each standard sample to obtain multiple spectral standard factors, and spectral standard factors with large errors were eliminated to further improve their accuracy. The response curve is a mathematical model that describes the relationship between spectral intensity and the concentration of the detected object. By drawing the response curve, the functional relationship between spectral intensity and concentration can be determined, providing a basis for subsequent concentration calculations and ensuring the accurate range of copper ions.
[0066] Step S3.6, substitute the characteristic spectrum of the product into the response curve to obtain the analysis result of the spectrum of the product. Substitute the spectral intensity of the measured characteristic spectrum of the product into the response curve to calculate the concentration of copper ions in the porous silicon-carbon composite matrix. Correct the concentration according to the response curve and compare and verify with the measurement results of the known standard sample to ensure the accuracy of the result.
[0067] Step S3.7, adjusting the internal parameters of the reactor according to the analysis results of the characteristic spectrum of the product.
[0068] If the copper ion concentration in the analysis result of the characteristic spectrum of the product is not within the preset copper ion concentration range, the gas convection device of the reactor is controlled to pass the etching gas, and the etching gas is used to react with the copper ions in the porous silicon-carbon composite matrix. The etching gas can be hydrogen chloride, chlorine or hydrogen fluoride to generate volatile copper compounds.
[0069] The reaction process between the etching gas and the copper ions is stimulated in the reactor, and the copper ion concentration during the reaction process is monitored. The monitoring method is the same as the copper ion concentration detection method described above, and will not be repeated here.
[0070] When the monitored copper ion concentration is within the preset copper ion concentration range, the input of etching gas is stopped and inert gas is introduced to discharge copper compound gas and etching gas. The above method is used to remove copper ions without affecting the next reaction of the porous silicon-carbon composite matrix, and no impurities remain in the cavity of the reactor, thereby eliminating the influence of excess ions on the second deposition reaction and improving the electrical properties of the silicon-carbon composite negative electrode material.
[0071] Step S3.8, introducing silane gas into the reactor for a second deposition reaction, the silane gas is monosilane gas, the reaction time is 300 minutes, and the reaction temperature is 500° C. The second deposition reaction deposits silicon atoms in the monosilane gas on the surface of the porous silicon-carbon composite matrix, and forms more dense and uniform nano-silicon by plasma vapor deposition, thereby significantly improving the specific capacity, electrochemical performance, structural stability and conductivity of the electrode material, while optimizing the interface reaction and improving the material utilization rate, and comprehensively enhancing the performance and stability of the lithium-ion battery.
[0072] Step S3.9, obtaining real-time information of the reactants in the reactor. The method of obtaining real-time information of the reactants is the same as the method of obtaining the copper ion concentration described above, exciting the continuously generated nanosilicon to obtain the nanosilicon-porous silicon-carbon composite and obtaining its characteristic spectrum to calculate the atomic concentration of each component.
[0073] Step S3.10: adjusting the reaction parameters of the second deposition reaction according to the real-time information, wherein the reaction parameters include radio frequency power, reaction temperature and pressure in the reactor.
[0074] By adjusting the output power of the RF power supply, the energy density of the plasma is changed, thereby controlling the deposition rate and the activity of the reactants. By acquiring the characteristic spectrum of the reactants in real time, the reaction progress and the concentration changes of the reactants can be monitored instantly, providing accurate reaction state information. The real-time feedback system can quickly adjust the reaction parameters according to the monitored changes to ensure that the reaction process is always carried out in the optimal state. Optimizing the deposition process of the material can significantly improve the electrochemical performance of the battery, including specific capacity, cycle stability and rate performance. The stability and consistency of the generated nano-silicon-porous silicon-carbon composite structure are improved, which helps to extend the service life of the subsequent batteries made of silicon-carbon composite negative electrode materials.
[0075] Step S4, introducing a carbon source gas to passivate the nano-silicon-porous silicon-carbon composite, and obtaining a silicon-carbon composite negative electrode material after cooling.
[0076] Nano silicon is highly active and easily reacts with electrolytes, resulting in decreased battery performance. Through the passivation reaction, a carbon protective layer is formed on the surface of nano silicon, which can effectively reduce the chemical activity of silicon and reduce the occurrence of side reactions. The carbon layer formed by the passivation reaction can form a conductive network on the surface of silicon particles, improve the overall conductivity of the composite material, and help improve the charging and discharging efficiency of the battery.
[0077] Specifically, the specific steps of step S4 are as follows:
[0078] Step S4.1, discharge the silane gas in the reactor, and set the temperature of the reactor to 700° C. The gas flow control device and the temperature control device of the reactor are used to accurately control the gas flow state and the temperature of the reactor.
[0079] Step S4.2, introducing a carbon source gas for passivation reaction, the reaction time is 300 min; the carbon source gas is acetylene gas.
[0080] Step S4.3, according to the preset cooling curve, set the target temperature and cooling rate of each stage, wherein the target temperature and cooling rate of any two stages are different. To avoid stress and cracks caused by rapid cooling, thereby ensuring the quality and structural integrity of the deposited layer. Step cooling helps to relieve thermal stress and prevent cracking and peeling of the deposited layer. The initial cooling rate can be set to a faster cooling rate, which can be 10°C / min~20°C / min, the intermediate cooling rate can be set to a slower cooling rate, which can be 5°C / min~10°C / min, and the final cooling rate can be set to a very slow cooling rate, which can be 1°C / min~5°C / min.
[0081] Embodiment 2:
[0082] Embodiment 2 of the present invention provides a preparation method for preparing a silicon-carbon composite negative electrode material. The preparation method comprises the following steps:
[0083] Step S1, preheating the foam copper in a vacuum environment, and then introducing a mixed gas to perform a first deposition reaction.
[0084] The volume ratio of each component in the mixed gas is boron source gas: magnesium source gas: silicon source gas: carbon source gas = 1:10:20:20. The boron source gas is diborane gas, the magnesium source gas is magnesium hydride gas, the silicon source gas is disilane gas, the carbon source gas is ethylene gas, and the flow rate of the mixed gas is 100 ml / min.
[0085] The specifications of the copper foam used are pore diameter 0.1 mm, porosity 50%, and volume density 0.2 g / cm 3The mass of the copper foam is 100 g, the copper foam is evacuated, the reaction temperature of the first deposition reaction is 1000° C., and the reaction time is 12 hours.
[0086] Step S2: adding tetrahydrofuran to remove the foamed copper to obtain a porous silicon-carbon composite matrix.
[0087] 1000 g of tetrahydrofuran solution was added, and the deposited copper foam was immersed in tetrahydrofuran for 48 h.
[0088] Step S3, transferring the porous silicon-carbon composite substrate to a reactor with an inert atmosphere, introducing silane gas for a second deposition reaction, and obtaining a nano-silicon-porous silicon-carbon composite. The silane gas is disilane gas, the reaction temperature of the second deposition reaction is 400° C., and the reaction time is 600 min.
[0089] The steps for removing copper ions from the porous silicon-carbon composite matrix in Example 2 are substantially the same as those in Example 1, with only adaptive adjustments being made, and thus will not be described in detail.
[0090] Step S4: introducing carbon source gas to passivate the nano-silicon-porous silicon-carbon composite, and obtaining a silicon-carbon composite negative electrode material after cooling. The carbon source gas is acetylene gas, the reaction temperature of the passivation reaction is 600-600°C, and the reaction time is 600 min.
[0091] The cooling steps in Example 2 are substantially the same as those in Example 1, with only adaptive adjustments being made, and thus will not be described in detail.
[0092] Embodiment 3:
[0093] Embodiment 3 of the present invention provides a preparation method for preparing a silicon-carbon composite negative electrode material. The preparation method comprises the following steps:
[0094] Step S1, preheating the foam copper in a vacuum environment, and then introducing a mixed gas to perform a first deposition reaction.
[0095] The volume ratio of each component in the mixed gas is 5:30:40:40:5. The boron source gas is diborane gas, the magnesium source gas is magnesium hydride gas, the silicon source gas is trichlorosilane gas, the carbon source gas is propylene gas, and the flow rate of the mixed gas is 1000 ml / min.
[0096] The specifications of the copper foam used are pore diameter 10 mm, porosity 90%, and volume density 0.1 g / cm 3 The mass of the copper foam is 100 g, the copper foam is evacuated, the reaction temperature of the first deposition reaction is 1400° C., and the reaction time is 1 hour.
[0097] Step S2: adding tetrahydrofuran to remove the foamed copper to obtain a porous silicon-carbon composite matrix.
[0098] 1000 g of tetrahydrofuran solution was added, and the deposited copper foam was immersed in tetrahydrofuran for 48 h.
[0099] Step S3, transferring the porous silicon-carbon composite substrate to a reactor with an inert atmosphere, introducing silane gas for a second deposition reaction, and obtaining a nano-silicon-porous silicon-carbon composite. The silane gas is trichlorosilane gas, the reaction temperature of the second deposition reaction is 600° C., and the reaction time is 60 min.
[0100] The steps for removing copper ions from the porous silicon-carbon composite matrix in Example 3 are substantially the same as those in Example 1, with only adaptive adjustments being made, and thus will not be described in detail.
[0101] Step S4: introducing carbon source gas to passivate the nano-silicon-porous silicon-carbon composite, and obtaining a silicon-carbon composite negative electrode material after cooling. The carbon source gas is propylene gas, the reaction temperature of the passivation reaction is 900-600°C, and the reaction time is 60 minutes.
[0102] The cooling step in Example 3 is substantially the same as that in Example 1, with only adaptive adjustments being made, and thus will not be described in detail.
[0103] Comparative Example 1:
[0104] The difference from Example 1 is that the foam copper is replaced by porous carbon in step S1, and the rest is the same as Example 1.
[0105] Comparative Example 2:
[0106] The difference from Example 1 is that in step S1, diborane and magnesium hydride are not introduced, but only disilane gas and ethylene gas are introduced. The rest is the same as Example 1.
[0107] Experiment 1: Morphology determination of silicon-carbon composite negative electrode materials.
[0108] The silicon-carbon composite negative electrode materials in Examples 1-3 and Comparative Examples 1-2 were subjected to SEM testing.
[0109] Table 1, morphology comparison table of each embodiment and comparative example:
[0110]
[0111] According to Table 1, the particle sizes of Examples 1-3 and Comparative Example 2 are uniformly distributed, have a porous structure on the surface, and have fine powder materials bonded on the surface. However, in Comparative Example 1, copper foam is not used as a template, so it is difficult to form particles with uniform size and a porous structure.
[0112] Figure 3This is the SEM picture of Example 1. The silicon-carbon composite negative electrode material of Example 1 presents a granular structure with a porous structure on the surface, and fine powder material is bonded on the surface with a particle size between 5µm and 10μm.
[0113] Experiment 2: Electrical performance test.
[0114] (1) Physical and chemical properties test:
[0115] The specific surface area and tap density of each silicon-carbon composite material were tested with reference to the national standard GB / T 38823-2020 "Silicon Carbon", and the electrical conductivity of each material was tested using a four-probe tester; the test results are shown in Table 2 below.
[0116] (2) Button battery test:
[0117] The silicon-carbon composite negative electrode materials in Examples 1-3 and Comparative Examples 1-2 were used as negative electrode materials for lithium-ion batteries to prepare button batteries, and the preparation method was as follows:
[0118] Add binder, conductive agent and solvent to the composite material, stir to make slurry, coat on copper foil, dry and roll to get negative electrode sheet; the binder used is polyvinylidene fluoride (PVDF), the conductive agent is conductive carbon black (SP), the solvent is N-methylpyrrolidone (NMP), the amount ratio of composite material, SP, PVDF and NMP is 90g:1g:4g:220mL; the electrolyte is lithium hexafluorophosphate (LiPF6), the mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with a volume ratio of 1:1 is used as solvent, and the electrolyte concentration is 1mol / L; the metal lithium sheet is the counter electrode, and the diaphragm is a polypropylene (PP) film. The button cell is assembled in an argon-filled glove box.
[0119] The electrochemical performance of button cells containing the silicon-carbon composite negative electrode materials of Examples 1-3 and Comparative Examples 1-2 was tested using a Wuhan Blue Power CT2001A battery tester with a charge and discharge voltage range of 0.005 V to 2.0 V and a charge and discharge rate of 0.1C.
[0120] The negative electrode sheets of the above button batteries were also tested for full-charge expansion. The specific test process was as follows: the thickness D1 of the button battery negative electrode sheets containing the silicon-carbon composite negative electrode materials of Examples 1-3 and Comparative Examples 1-2 after rolling was tested, and then the button battery was fully charged to 100% SOC and the full-charge thickness D2 of the negative electrode sheets was dissected, and then the expansion rate was calculated: the expansion rate was = ((D2-D1) / D1)*100%.
[0121] Table 2. Test results of Experiment 2:
[0122]
[0123] It can be seen from the data in Table 2 that the specific capacity, initial efficiency, powder resistivity, full-charge expansion, DCR and diffusion coefficient of the silicon-carbon composite negative electrode material prepared by the present invention in Examples 1-3 are significantly better than those in Comparative Examples 1-2. The reason is that the pores left by using foam copper as the matrix are larger, which reduces expansion, and at the same time, magnesium is deposited in its porous carbon, and boron doping elements reduce the powder resistivity of the material, reduce polarization, and improve the initial efficiency.
[0124] Experiment 3: Soft pack battery test.
[0125] The silicon-carbon composite negative electrode materials of Examples 1-4 and Comparative Example 1 were mixed with 90% artificial graphite as negative electrode materials to prepare negative electrode sheets. 1 / 3 Co 1 / 3 Mn 1 / 3 O2) as the positive electrode; lithium hexafluorophosphate (LiPF6) as the electrolyte, a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (DEC) in a volume ratio of 1:1 as the solvent, and the electrolyte concentration is 1.3 mol / L; Celgard 2400 membrane is used as the separator to prepare a 5Ah soft-pack battery.
[0126] The following performance tests are performed on each soft pack battery:
[0127] (1) Liquid absorption capacity and liquid retention rate test.
[0128] Use a 1mL burette and absorb 1mL of electrolyte, add a drop on the surface of the electrode, and count until the electrolyte is completely absorbed, and record the time t (seconds). Calculate the theoretical liquid absorption m1 of the electrode according to the electrode parameters, and weigh the weight m2 of the electrode, then place the electrode in the electrolyte and soak it for 24 hours, weigh the weight of the electrode as m3, calculate the liquid absorption m3-m2 of the electrode, and calculate according to the following formula: Liquid retention rate = (m3-m2) * 100% / m1, and use a surface resistance tester to test the surface resistance of the electrode.
[0129] Table 3. Test results of liquid absorption capacity, liquid retention rate and surface resistance.
[0130]
[0131] As can be seen from Table 3, the liquid absorption and retention capacity and surface resistance of the silicon-carbon composite materials obtained in Examples 1-3 are significantly higher than those in Comparative Examples 1-2. The reason is that: the specific surface area of the composite materials of the examples is larger, which improves the liquid absorption and retention capacity of the materials; at the same time, the powder resistivity of the materials of the examples is lower than that of the comparative examples, so that the surface resistance of the electrode sheets is lower than that of the comparative examples.
[0132] (2) Cycle performance and rate test.
[0133] The soft pack batteries A-2 to E-2 were subjected to cycle performance tests and rate tests under the following conditions: charge and discharge voltage range of 2.5 to 4.2 V, temperature of 25 ± 3.0 °C, charge and discharge rate of 0.5C / 1.0C, and cycle number of 500 times. Rate test: Test the constant current ratio of the material under 2C conditions.
[0134] Table 4, Cycle performance test data:
[0135]
[0136] It can be seen from Table 4 that the rate and cycle performance of the soft-pack lithium-ion battery prepared using the silicon-carbon composite material of the present invention are better than those of Comparative Examples 1-2. The reason is that the silicon-carbon composite negative electrode material of the embodiment has low full-charge expansion and high specific surface area, which improves the cycle performance of the material; at the same time, the silicon-carbon composite negative electrode material of the embodiment has low electrode sheet surface resistance, reduces impedance, and improves the constant current ratio.
[0137] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a silicon-carbon composite negative electrode material, characterized in that: For preparing a silicon-carbon composite negative electrode material, the preparation method comprises the following steps: S1. Preheating the foamed copper in a vacuum environment, and then introducing a mixed gas to perform a first deposition reaction, wherein the mixed gas is a mixture of a boron source gas, a magnesium source gas, a silicon source gas, and a carbon source gas; S2, adding tetrahydrofuran to remove the foamed copper to obtain a porous silicon-carbon composite matrix; S3, transferring the porous silicon-carbon composite substrate to a reactor in an inert atmosphere, introducing silane gas to perform a second deposition reaction, and obtaining a nano-silicon-porous silicon-carbon composite; The step of transferring the porous silicon-carbon composite substrate to a reactor in an inert atmosphere comprises: The porous silicon-carbon composite matrix is transferred to a reaction kettle and atomized, wherein an inert gas is introduced into the reaction kettle and the reaction kettle has gas and temperature regulating capabilities; Plasma exciting the atomized porous silicon-carbon composite matrix in the reactor; Acquiring a characteristic spectrum of a product of the porous silicon-carbon composite matrix after excitation, and analyzing the characteristic spectrum of the product; Acquire standard characteristic spectra in the selected wavelength range; Calculating the spectral standard factor within the selected wavelength range and drawing a response curve, wherein the spectral standard factor is the ratio of the standard characteristic spectrum to the standard light intensity, and the response curve is a relationship curve between each wavelength within the wavelength range and the spectral standard factor; Substituting the characteristic spectrum of the product into the response curve to obtain the analysis result of the characteristic spectrum of the product; Adjusting the internal parameters of the reactor according to the analysis results of the characteristic spectrum of the product; If the copper ion concentration in the analysis result of the characteristic spectrum of the product is not within the preset copper ion concentration range, controlling the gas convection device of the reactor to pass an etching gas, wherein the etching gas is used to react with the copper ions in the porous silicon-carbon composite matrix to generate a volatile copper compound; When the monitored copper ion concentration is within a preset copper ion concentration range, the input of the etching gas is stopped and an inert gas is introduced to exhaust the copper compound gas and the etching gas; S4, introducing a carbon source gas to passivate the nano-silicon-porous silicon-carbon composite, and obtaining the silicon-carbon composite negative electrode material after cooling.
2. The method for preparing the silicon-carbon composite negative electrode material according to claim 1, characterized in that: The volume ratio of each component in the mixed gas is boron source gas: magnesium source gas: silicon source gas: carbon source gas=1-5:10-30:20-40:20-40.
3. The method for preparing the silicon-carbon composite negative electrode material according to claim 2, characterized in that: In the step S1, the boron source gas is diborane; The magnesium source gas is magnesium hydride; The silicon source gas includes at least one of monosilane gas, disilane gas, trichlorosilane, tetrachlorosilane, dimethylsilane, and hexachlorodisilane; The carbon source gas includes one of acetylene, propyne, ethylene, propylene, methane and ethane.
4. The method for preparing the silicon-carbon composite negative electrode material according to claim 1, characterized in that: The pore size of the foam copper is in the range of 0.1 mm to 10 mm, the porosity is 50% to 90%, and the volume density is 0.1 to 0.5 g / cm 3 .
5. The method for preparing the silicon-carbon composite negative electrode material according to claim 1, characterized in that: In step S1, the preheating temperature is 1000°C-1400°C, the flow rate of the mixed gas is 100-1000 ml / min, and the reaction time of the first deposition reaction is 1-12 hours.
6. The method for preparing the silicon-carbon composite negative electrode material according to claim 1, characterized in that: In the step S3, the step of introducing silane gas to perform a second deposition reaction includes: Introducing silane gas into the reactor to carry out the second deposition reaction, the reaction time is 60-600 min, and the reaction temperature is 400-600° C.; Obtaining real-time information of reactants in the reactor; The reaction parameters of the second deposition reaction are adjusted according to the real-time information, wherein the reaction parameters include radio frequency power, reaction temperature and pressure in the reactor.
7. The method for preparing the silicon-carbon composite negative electrode material according to claim 1, characterized in that: Step S4 specifically includes: Discharging the silane gas in the reactor and setting the temperature of the reactor to 600-900° C.; The carbon source gas is introduced to carry out a passivation reaction, and the reaction time is 60 to 600 minutes; According to the preset cooling curve, the target temperature and cooling rate of each stage are set, wherein the target temperature and cooling rate of any two stages are different.
8. A silicon-carbon composite negative electrode material, characterized in that: The silicon-carbon composite negative electrode material is prepared by the method for preparing the silicon-carbon composite negative electrode material according to any one of claims 1 to 7, wherein the silicon-carbon composite negative electrode material comprises: The inner core is porous silicon carbon, and the inner core has a porous structure; A nano silicon layer, located in the pore structure; A carbon coating layer is coated on the outer surface of the inner core and the nano silicon layer.