A flame retardant toughening agent containing phosphorus and silicon elements and its preparation method and application
By developing flame retardant toughener containing phosphorus and silicon elements, the synergistic action of phosphorus and silicon elements and the flexible structure of silicone are used to solve the flame retardant properties and mechanical properties of polycarbonate materials, and high transparency is achieved and excellent flame retardant performance, suitable for industrial production.
Patent Information
- Application Number
- CN202411069827.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The flame retardant properties of commercially available polycarbonate materials are limited, easily produce drips, poor fire safety performance, and existing phospho-silicon synergistic flame retardants have a great impact on the transparency and mechanical properties of the material, and cannot meet the high transparency. and excellent flame retardant requirements.
Develop a flame retardant toughener containing phosphorus and silicon elements, which plays flame retardant roles in both the condensed phase and the gas phase, and enhances the carbonization stability and free radical capture ability of the polymer through the synergistic action of phosphorus and silicon elements, and The flexible structure of silicone improves mechanical properties, and the preparation process is simple and suitable for industrial production.
It realizes the high transparency, excellent flame retardant performance and improved mechanical properties of polycarbonate composite materials, meets the application needs of high transparency and high flame retardant performance, and is also suitable for industrial production.
Smart Images

Figure CN118580276B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame retardancy, and in particular relates to a flame retardant toughening agent containing phosphorus and silicon elements, and a preparation method and application thereof. Background Art
[0002] As one of the five commonly used engineering plastics, polycarbonate is widely used in new energy batteries, automobiles, aerospace and other fields due to its advantages such as high transparency, excellent mechanical properties, and low production cost. Although commercially available polycarbonate materials have certain flame retardancy and can reach V-2 level in the UL-94 vertical combustion test, their flame retardancy is limited and dripping is easily generated during heating and combustion, so their fire safety performance is poor, which also seriously limits the expansion of their application fields. Therefore, it is necessary to perform flame retardant modification on commercially available polycarbonate to improve its fire safety performance.
[0003] In recent years, the flame retardant modification of polycarbonate has made great progress, and the most representative one is the multi-element synergistic flame retardant system, including phosphorus-nitrogen synergy, boron-silicon synergy, phosphorus-silicon synergy and multi-element synergy. Among them, the phosphorus-silicon synergistic flame retardant system has received widespread attention. As a representative of emerging flame retardants, phosphorus-based flame retardants are widely used in the flame retardant modification of various polymers including polycarbonate. This is because phosphorus can play a flame retardant role in both the gas phase and the condensed phase, so it has a high flame retardant efficiency. In the condensed phase, phosphorus-containing flame retardants are thermally decomposed to form multivalent polyphosphoric acid, which can promote the premature degradation of the polymer, dehydration and carbonization, and form a dense and stable carbon layer on the surface to prevent the exchange of heat and combustion products; in the gas phase, phosphorus-containing flame retardants are thermally decomposed to form phosphorus-containing free radicals, which can capture active H· and OH· free radicals and interrupt the combustion chain reaction. Silicon-based flame retardants mainly play a role in the condensed phase. The silicon element in the carbon layer, including silicon-carbon and silicon-oxygen bonds, can significantly improve the oxidation resistance of the carbon layer, thereby greatly improving the stability and barrier effect of the carbon layer. Although the phosphorus-silicon synergistic flame retardant system has excellent flame retardant efficiency, up to now, the relevant research on its application in polycarbonate composites is still limited, and representative flame retardants and research results are difficult to meet the flame retardant needs of polycarbonate. Wang Biaobing's research group at Changzhou University used 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), aminophenyl silicone oil and other raw materials to synthesize a flame retardant containing phosphorus and silicon elements, and applied it to commercially available bisphenol A polycarbonate. The multi-element synergistic flame retardant effect, mainly phosphorus and silicon elements, made the prepared polycarbonate composite material show excellent flame retardant properties in tests such as limiting oxygen index, UL-94 vertical combustion, and cone calorimeter. However, the addition of flame retardants has a great influence on the transparency of the composite material and reduces the tensile and impact properties of the composite material. Chinese invention patent CN116444970A discloses a phosphaphenanthrene / siloxane dibasic macromolecular flame retardant toughened polycarbonate material, which has good impact resistance and flame retardant properties, but its anti-dripping performance is achieved by adding fluorinated polymers such as polytetrafluoroethylene; in addition, the addition of anti-dripping agents such as polytetrafluoroethylene will have a negative impact on the transparency of polycarbonate composite materials, and cannot meet the application requirements for high transparency of flame retardant polycarbonate materials. Therefore, the development of new flame retardants containing phosphorus and silicon elements with simple preparation, high flame retardant efficiency and low addition amount, as well as the preparation of new flame retardant polycarbonate composite materials with excellent flame retardancy and mechanical properties, has become an urgent need in the field of flame retardant polymer technology. Summary of the invention
[0004] The present invention aims to provide a flame retardant and toughening agent containing phosphorus and silicon elements, and a preparation method and application thereof. Phosphorus can play a flame retardant role in both the condensed phase and the gas phase. In the condensed phase, the presence of phosphorus promotes the carbonization of polymers during combustion, while in the gas phase, phosphorus-containing free radicals play a role in quenching active free radicals during combustion. In addition, silicon can promote the carbonization of polymers during combustion through a synergistic flame retardant effect, and can significantly improve the stability of the carbon layer, thereby inhibiting combustion and protecting the matrix. The flexible structure of siloxane in the flame retardant structure of the present invention can play the role of a plasticizer, thereby improving the mechanical properties of the polymer, that is, the toughening effect. The preparation process of the flame retardant and toughening agent is simple, the conditions are relatively mild, the yield is high, and it is suitable for flame retardant treatment of different polymer matrices, so it is more suitable for industrial production and application.
[0005] The flame retardant toughening agent containing phosphorus and silicon elements of the present invention has a chemical structure as shown in the following formula (I):
[0006] ,
[0007] In formula (I), R is selected from any one of the following structures:
[0008] .
[0009] The preparation method of the flame retardant toughening agent containing phosphorus and silicon elements of the present invention comprises the following steps:
[0010] Under the protection of inert gas, the phosphorus-containing compound and 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane are stirred and mixed in a reactor, and the system is heated to 160-200 ° C for reaction for 12-24 hours; after the reaction is completed, the reaction mixture is transferred to an open container, heated to 180 ° C under inert gas purge, and stirred for 12 hours to obtain the target product.
[0011] The phosphorus-containing compound is selected from any one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphine, diphenyl phosphite, dibenzyl phosphite, dimethyl phosphite, diethyl phosphite, di-n-butyl phosphite and di-tert-butyl phosphite.
[0012] The molar ratio of 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane to the phosphorus-containing compound is 1:2.5-2.8.
[0013] The inert gas is any one of nitrogen, argon or helium.
[0014] The application of the flame retardant and toughening agent containing phosphorus and silicon elements in the present invention is to add the flame retardant and toughening agent as an auxiliary agent into the polycarbonate system, which can improve the flame retardant property and mechanical property of the material at the same time.
[0015] Furthermore, the added amount of the flame retardant toughening agent is 4%-8% of the total mass of the composite material system.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1. The chemical structure of the flame retardant toughening agent in the present invention contains both phosphorus and silicon elements. Phosphorus can play a flame retardant role in both the condensed phase and the gas phase. In the condensed phase, the presence of phosphorus promotes the carbonization of the polymer during combustion, while in the gas phase, phosphorus-containing free radicals play a role in quenching the active free radicals during combustion. In addition, silicon can not only promote the carbonization of the polymer during combustion through a synergistic flame retardant effect, but also significantly improve the stability of the carbon layer.
[0018] 2. The flexible structure of siloxane in the chemical structure of the flame retardant toughening agent in the present invention can act as a plasticizer, thereby improving the impact resistance of the polymer and exerting a toughening effect.
[0019] 3. The flame retardant toughening agent in the present invention has good compatibility with polycarbonate, and the prepared flame retardant toughened polycarbonate composite material has high transparency, which can meet the application requirements for high transparency of flame retardant polycarbonate materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 is the infrared spectrum of the target product a in Example 1.
[0022] Figure 2 is the infrared spectrum of the target product b in Example 2.
[0023] Figure 3 This is the infrared spectrum of the target product c in Example 3.
[0024] Figure 4 This is the infrared spectrum of the target product d in Example 4.
[0025] Figure 5 This is the H NMR spectrum of the target product a in Example 1.
[0026] Figure 6 This is the H NMR spectrum of the target product b in Example 2.
[0027] Figure 7 This is the H NMR spectrum of the target product c in Example 3.
[0028] Figure 8 This is the H NMR spectrum of the target product d in Example 4.
[0029] Fig. 9 2 are the thermogravimetric analysis curves of the samples in Comparative Example 1 and Example 7 of the present invention.
[0030] Fig.10 1 is the heat release rate curve of each sample in Comparative Example 1 and Example 6 of the present invention.
[0031] Fig.11 It is the total heat release curve of each sample in Comparative Example 1 and Example 5 of the present invention.
[0032] Fig.12 The CO2 generation rate curves of the samples in Comparative Example 1 and Example 7 of the present invention are shown.
[0033] Fig.13 The UV-visible spectra of the samples in Comparative Example 1 and Example 6 of the present invention are shown in FIG.
[0034] Fig.14 These are real digital photos of the samples in Comparative Example 1 and Example 5 of the present invention. DETAILED DESCRIPTION
[0035] In order to further illustrate the technical solution of the present invention, the preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention. Based on the examples in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Embodiment 1:
[0036] 1. Mix 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane and 9, 10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide at a molar ratio of 1:2.5 under nitrogen protection with magnetic stirring for 5-10 minutes.
[0037] 2. The mixture was heated to 180°C and reacted for 24 hours. The reaction mixture was then transferred to an open container and heated to 180°C under nitrogen purge. The target product a was obtained after stirring for 12 hours. The chemical structure of the target product a is shown below:
[0038] .
[0039] The target product a was analyzed by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 907 (POC), 1072 (Si-O), 1117 (PC&P-O), 1177(P=O), 1517 (P-Ar), 1611 (Ar-Ar), 2960 (-CH3). 1 H-NMR (400 MHz, CDCl3-d6,ppm): 0.00 (s, 9H, (Si-CH3)3), 0.67 (s, 6H, (Si-CH2)3), 1,86 (s, 6H, (-CH2-P)3), 7.97-7.10 (m, 24H, Ar-H). Embodiment 2:
[0040] 1. Mix 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane and diphenylphosphine at a molar ratio of 1:2.6 under nitrogen protection with magnetic stirring for 5-10 minutes.
[0041] 2. The mixture was heated to 160°C and reacted for 24 hours. The reaction mixture was then transferred to an open container and heated to 180°C under nitrogen purge. The target product b was obtained after stirring for 12 hours. The chemical structure of the target product b is shown below:
[0042] .
[0043] The target product b was analyzed by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 1072 (Si-O), 1117 (PC), 1201 (P=O), 1517 (P-Ar), 1610 (Ar-Ar), 2965 (-CH3). 1 H-NMR (400 MHz, CDCl3-d6, ppm): 0.14 (s, 9H, (Si-CH3)3), 1.17 (s, 6H, (Si-CH2)3), 2.52 (s, 6H, (-CH2-P)3), 7.50-7.75 (m,30H, Ar-H). Embodiment 3:
[0044] 1. Mix 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane and diphenyl phosphite at a molar ratio of 1:2.8 under nitrogen protection with magnetic stirring for 5-10 minutes.
[0045] 2. The mixture was heated to 180°C and reacted for 24 hours. The reaction mixture was then transferred to an open container and heated to 180°C under nitrogen purge. The target product c was obtained after stirring for 12 hours. The chemical structure of the target product c is shown below:
[0046] .
[0047] The target product c was characterized by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 907 (POC), 1072 (Si-O), 1117 (PC&P-O), 1177(P=O), 1610 (Ar-Ar), 2965 (-CH3). 1 H-NMR (400 MHz, CDCl3-d6, ppm): 0.00 (s, 9H, (Si-CH3)3), 0.67 (s, 6H, (Si-CH2)3), 1,86 (s, 6H, (-CH2-P)3), 7.97-7.10 (m,30H, Ar-H). Embodiment 4:
[0048] 1. Mix 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane and dimethyl phosphite at a molar ratio of 1:2.5 under nitrogen protection with magnetic stirring for 5-10 minutes.
[0049] 2. The mixture was heated to 160°C and reacted for 24 hours. The reaction mixture was then transferred to an open container and heated to 180°C under nitrogen purge. The target product d was obtained after stirring for 12 hours. The chemical structure of the target product d is shown below:
[0050] .
[0051] The target product d was characterized by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 2980&2865 (-CH3), 907 (POC), 1072 (Si-O), 1117 (PC&P-O), 1177 (P=O). 1H-NMR (400 MHz, CDCl3-d6, ppm): 0.12 (s, 9H, (Si-CH3)3), 0.87 (s, 6H, (Si-CH2)3), 1.73 (s, 6H, (-CH2-P)3), 3.65 (d, 18H, PO-CH3). Embodiment 5:
[0052] 1. Put the polycarbonate in a vacuum oven and dry it at 80 °C for 24 h. Accurately weigh 48.0 g of the dried polycarbonate and 2.0 g of the flame retardant toughening agent a. Add the polycarbonate and the flame retardant toughening agent a in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240 °C, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0053] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes. Embodiment 6:
[0054] 1. Put the polycarbonate in a vacuum oven and dry it at 80 °C for 24 h. Accurately weigh 47.0 g of the dried polycarbonate and 3.0 g of the flame retardant toughening agent a. Add the polycarbonate and the flame retardant toughening agent a in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240 °C, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0055] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes. Embodiment 7:
[0056] 1. Put the polycarbonate in a vacuum oven and dry it at 80℃ for 24 h. Accurately weigh 46.0g of the dried polycarbonate and 4.0g of the flame retardant and toughening agent a. Add the polycarbonate and the flame retardant and toughening agent a in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240℃, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0057] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes. Embodiment 8:
[0058] 1. Put the polycarbonate in a vacuum oven and dry it at 80 °C for 24 h. Accurately weigh 47.0 g of the dried polycarbonate and 3.0 g of the flame retardant and toughening agent b. Add the polycarbonate and the flame retardant and toughening agent b in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240 °C, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0059] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes. Embodiment 9:
[0060] 1. Put the polycarbonate in a vacuum oven and dry it at 80℃ for 24h. Accurately weigh 47.0g of the dried polycarbonate and 3.0g of the flame retardant and toughening agent C. Add the polycarbonate and the flame retardant and toughening agent C in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240℃, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0061] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes. Embodiment 10:
[0062] 1. Put the polycarbonate in a vacuum oven and dry it at 80 °C for 24 h. Accurately weigh 47.0 g of the dried polycarbonate and 3.0 g of the flame retardant toughening agent d. Add the polycarbonate and the flame retardant toughening agent d in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240 °C, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0063] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes.
[0064] Comparative Example 1: Unmodified polycarbonate material
[0065] 1. Put the polycarbonate in a vacuum oven and dry it at 80 °C for 24 h. Accurately weigh 50.0 g of the dried polycarbonate. Add the polycarbonate in batches to a two-roll internal mixer for melt blending. The blending conditions are: temperature 240 °C, rotor speed 60 rpm, mixing time 10 minutes, to obtain a polycarbonate sample.
[0066] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes.
[0067] Comparative Example 2: DOPO-HQ flame retardant polycarbonate material
[0068] 1. Put the polycarbonate in a vacuum oven and dry it at 80 °C for 24 h. Accurately weigh 47.0 g of the dried polycarbonate and 3.0 g of 10-(2, 5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ). Add the polycarbonate and DOPO-HQ in batches to a double-roll internal mixer for melt blending. The blending conditions are: temperature 240 °C, rotor speed 60 rpm, mixing time 10 minutes, and obtain a polycarbonate sample.
[0069] 2. Add the polycarbonate sample obtained in step 1 to an injection molding machine for injection molding, or use a flat vulcanizer for hot pressing to obtain a polycarbonate sample of a certain shape and size. The conditions for the injection molding machine are: plasticizing temperature 250 ° C, injection pressure 50 bar; the conditions for the flat vulcanizer are: temperature 240 ° C, hot pressing at 5 MPa for 10 minutes, temperature 250 ° C, hot pressing at 10 MPa for 5 minutes.
[0070] The performance test results of the products obtained in the above embodiments and comparative examples are as follows:
[0071] .
[0072] The flame retardant test results of each sample in Table 1 show that the oxygen index of the unmodified polycarbonate is 23.0%, there is no level in the UL-94 vertical burning test, and the tensile strength is 53.5 MPa (Comparative Example 1). The oxygen index of the polycarbonate to which 4.0 wt% (Example 5), 6.0 wt% (Example 6) and 8.0 wt% (Example 7) of the flame retardant toughening agent a are added respectively rises to 27.5%, 28.5% and 30.5%, and both Examples 6 and 7 can pass the UL-94 vertical burning test V-0 level. In addition, the tensile strength and impact strength of Examples 5, 6 and 7 are all improved to a certain extent compared with the unmodified polycarbonate (Comparative Example 1), and the tensile strength and impact strength of Example 6 are increased to 63.7 MPa and 96.6 kJ / m respectively. 2 . In addition, by changing the type of flame retardant curing agent, the oxygen index of the polycarbonate to which 6.0 wt% of flame retardant curing agent b (Example 8), flame retardant curing agent c (Example 9) and flame retardant curing agent d (Example 10) were added respectively increased to 29.0%, 28.5% and 28.0%, and all of them were able to pass the UL-94 vertical combustion test V-0 level. Similarly, the tensile strength and impact strength were greatly improved compared with the unmodified polycarbonate (Comparative Example 1). It is proved that the addition of flame retardants a, b and c has a great effect on improving the mechanical properties of polycarbonate. Compared with the commonly used commercially available flame retardant DOPO-HQ (Comparative Example 2), the oxygen index, UL-94 combustion grade, tensile strength and impact strength of the flame retardant polycarbonate obtained in Comparative Example 2 are inferior to the performance of the flame retardant polycarbonate modified by flame retardants a, b and c provided by the present invention. By replacing different types of polycarbonate, curing agent and curing accelerator, the flame retardant polycarbonate modified by flame retardants a, b and c provided by the present invention also has a similar flame retardant effect. Therefore, the flame retardant polycarbonate synthesized in Examples 5-10 is suitable for applications requiring higher flame retardant properties.
[0073] The thermogravimetric analysis curves of the samples in comparative example 1 and example 7 under air atmosphere are as follows: Fig. 9As shown. It can be seen that the initial decomposition temperature of the flame retardant polycarbonate with 8.0 wt% flame retardant a is almost the same as that of the unmodified polycarbonate, and its carbonization amount is higher than that of the unmodified polycarbonate at high temperature: at 600 ° C, the residual carbon rate of the unmodified polycarbonate is 19.0%, while the residual carbon rate of the flame retardant polycarbonate in Example 7 rises to 29.4%, indicating that the flame retardant a has a certain catalytic carbonization ability.
[0074] The heat release rate curves of the samples in Comparative Example 1 and Example 6 are as follows: Fig.10 As shown. It can be seen that the peak heat release rate of unmodified polycarbonate is about 503.5 kW / m 2 The peak heat release rate of the flame retardant polycarbonate with 6.0 wt% flame retardant a is 316.2 kW / m 2 , which was reduced by 37.2% compared with the unmodified polycarbonate, indicating that flame retardant a has good flame retardant properties.
[0075] The total heat release curves of the samples in Comparative Example 1 and Example 5 are as follows: Fig.11 It can be seen that within 0-300 s, the total heat release value of the unmodified polycarbonate is about 62.4 MJ / m 2 The total heat release values of the flame retardant polycarbonate with 4.0 wt% flame retardant a added were 46.0 MJ / m 2 , which was decreased by 26.3% compared with the unmodified polycarbonate, further indicating that flame retardant a has good flame retardant properties.
[0076] The CO2 generation rate curves of the samples in Comparative Example 1 and Example 7 are as follows: Fig.12 It can be seen that within 0-300 s, the total CO2 production of the unmodified polycarbonate is about 0.93 kg / kg, and the total CO2 production of the flame-retardant polycarbonate with 8.0 wt% flame retardant a is 0.55 kg / kg, which is 40.9% lower than that of the unmodified polycarbonate, indicating that flame retardant a has good performance in inhibiting the emission of CO2 (greenhouse gas).
[0077] The UV-visible spectra of the samples in Comparative Example 1 and Example 6 are as follows: Fig.13 As shown. It can be seen that in the wavelength range of 300-800 nm, the transmittance of the flame-retardant polycarbonate with 6.0 wt% flame retardant a is slightly lower than that of the unmodified polycarbonate. At a wavelength of 800 nm, the transmittance of the flame-retardant polycarbonate with 6.0 wt% flame retardant a is 86.7%, and the transmittance of the unmodified polycarbonate is 87.8%, indicating that the effect of flame retardant a on the transparency of polycarbonate materials can be ignored.
[0078] The actual digital photos of the samples (all with a thickness of 1 mm) in Comparative Example 1 and Example 5 are as follows: Fig.14 As shown in the figure, both the unmodified polycarbonate and the flame-retardant polycarbonate with 4.0 wt% flame retardant a added have good transparency, and when the polycarbonate material is placed on the text, the details are clearly visible.
[0079] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An application of a flame retardant toughening agent containing phosphorus and silicon, characterized in that: The flame retardant toughening agent is added as an auxiliary agent to the polycarbonate system to improve the flame retardant properties and mechanical properties of the material at the same time; The chemical structure of the phosphorus and silicon flame retardant toughening agent is shown in the following formula (I): , In formula (I), R is selected from any one of the following structures: ; The added amount of the flame retardant toughening agent is 6%-8% of the total mass of the composite material system.
2. The use according to claim 1, characterized in that The phosphorus and silicon flame retardant toughening agent is prepared by a method comprising the following steps: Step 1: under the protection of inert gas, add the phosphorus-containing compound and 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane into a reactor and heat to react; Step 2: After the reaction in step 1 is completed, the reaction mixture is transferred to an open container and continued to be heated under an inert gas purge to obtain the target product; The phosphorus-containing compound is selected from any one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphine, diphenyl phosphite and dimethyl phosphite.
3. The use according to claim 2, characterized in that: The molar ratio of 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane to the phosphorus-containing compound is 1:2.5-2.
8.
4. The use according to claim 2, characterized in that: In step 1, the reaction temperature of the phosphorus-containing compound and 2, 4, 6-trimethyl-2, 4, 6-trivinylcyclotrisiloxane is 160-200° C., and the reaction time is 12-24 hours.
5. The use according to claim 2, characterized in that: In step 2, the mixture is heated to 180° C. and stirred for reaction for 12 hours under an inert gas purge.
6. The use according to claim 2, characterized in that: The inert gas is any one of nitrogen, argon or helium.