Epoxy resin coating wellbore equipment and manufacturing method thereof
By applying a modified fluorosilic epoxy resin coating on the inner wall of the wellbore, the problem of wax and rust of the wellbore is solved, which extends the service life and improves oil production efficiency and mechanical properties, and reduces maintenance costs.
Patent Information
- Application Number
- CN202410971518.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The wellbore of the oil well is prone to wax and rust, and has a short service life, which leads to reduced oil pump efficiency and accelerated equipment corrosion, increasing production costs and safety risks.
The inner wall of the wellbore is used to apply an epoxy resin-containing coating, and the modified fluorosilic epoxy resin, amine-based curing agent, corrosion-resistant filler and anti-wax agent to form a wear-resistant and corrosion-resistant coating to reduce wax and Rust phenomenon.
It effectively extends the service life of wellbore equipment, improves oil production efficiency, reduces maintenance costs, and improves mechanical properties and corrosion resistance.
Smart Images

Figure CN118580749B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil production equipment, and in particular relates to epoxy resin coating wellbore equipment and a manufacturing method thereof. Background Art
[0002] The statements in this section merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] During the exploitation of oil wells, the presence of paraffin in crude oil will cause wax deposition in the wellbore, resulting in blockage of the oil pipeline, reduced oil pump efficiency, increased energy consumption of pumping equipment, and increased equipment failure rate. Under certain conditions (such as lowered temperature), the paraffin component in crude oil will crystallize and precipitate, attaching to the inner wall of the wellbore to form wax deposition. Waxing will increase the roughness of the inner wall of the wellbore, thereby increasing friction; the mud and sand in the formation will enter the wellbore with the fluid, forming a rough surface and increasing friction. In addition, crude oil contains a large amount of corrosive substances such as hydrogen sulfide, which will accelerate the corrosion and rusting of metal equipment such as the wellbore. All of the above reasons have a very adverse impact on the production efficiency of oil wells, and the service life of equipment is reduced, which increases safety costs, time costs and economic costs for enterprises.
[0004] At present, the industry uses physical or chemical methods to reduce the wax deposition in the wellbore, thereby improving the rust resistance and wear resistance of the wellbore equipment. For example, a high temperature environment is created to accelerate the dissolution of the crystalline wax in the oil wellbore; a brush-like structure is used to prevent wax deposition, but the effect is minimal and it cannot prevent the wellbore from rusting; or a wax remover is used to promote the melting of the crystalline wax, but this has the problems of poor safety and complicated operation, and poor penetration effect on some wells with high impurities. Summary of the invention
[0005] In order to overcome the deficiencies of the above-mentioned prior art, the present invention aims to solve the problem that the existing wellbore equipment is easy to wax, rust and has a short service life. The present invention provides an epoxy resin coated wellbore equipment and a method for making the same. In the present invention, a coating containing epoxy resin is arranged on the inner wall of the wellbore, and the epoxy resin coating is formed by using epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent, so as to effectively reduce the waxing degree of the wellbore, reduce the rust and friction of the wellbore, and improve the oil production efficiency, which has practical application value.
[0006] To achieve the above objectives, one or more embodiments of the present invention provide the following technical solutions:
[0007] According to a first aspect of the present invention, there is provided an epoxy resin coated wellbore equipment, comprising an oil layer casing 1, wherein a coating 2 containing epoxy resin is disposed on the surface of the oil layer casing 1.
[0008] In a specific embodiment of the present invention, the epoxy resin-containing coating is composed of modified epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent.
[0009] In a specific embodiment of the present invention, the modified epoxy resin is a fluorosilicone epoxy resin, so as to improve the wear resistance and anti-waxing performance of the coating.
[0010] In a specific embodiment of the present invention, the preparation method of the fluorosilicone epoxy resin is:
[0011] Mixing organosiloxane, fluorosilane, anhydrous ethanol and distilled water, stirring and refluxing, adjusting the pH value to 4-5 with hydrochloric acid, and refluxing under reduced pressure distillation to obtain fluorosilicone resin;
[0012] The epoxy resin is diluted with isobutyl alcohol and butyl acetate, and the fluorosilicone resin is added under stirring, and the fluorosilicone resin epoxy resin is obtained by reflux and reduced pressure distillation.
[0013] In a specific embodiment of the present invention, the amine curing agent is a polyetherimide curing agent, which can further improve the mechanical properties of the epoxy resin, enhance its bending and strength, and improve the wear resistance and chemical stability of the coating.
[0014] In a specific embodiment of the present invention, the corrosion-resistant filler includes glass flakes, carbon fiber, graphene or nano zinc oxide.
[0015] In a specific embodiment of the present invention, the anti-waxing agent includes a fluorinated surfactant, aluminum and sodium hydroxide, an oil-based wax remover, a water-based wax remover, and an emulsion-type wax remover;
[0016] Preferred is a fluorinated surfactant; more preferred is Capstone FS-10.
[0017] Fluorinated surfactants have their hydrophobic tails partially fluorinated or completely replaced by fluorine molecules. Compared to the corresponding hydrocarbon surfactants, fluorinated surfactants have different properties such as lower surface tension, better interfacial tension reduction efficiency, oleophobic and hydrophobic properties, high thermal stability and better chemical resistance, and can be used in fire protection, household products, foaming, coatings and paint preparation.
[0018] In a specific embodiment of the present invention, the epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent are added in amounts of 100 parts, 40-45 parts, 10-13 parts and 7-10 parts respectively;
[0019] Preferably, the added amounts of the epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent are 100 parts, 42 parts, 10 parts and 8 parts respectively.
[0020] In a specific embodiment of the present invention, the thickness of the coating is 0.5 mm-2 mm.
[0021] A second aspect of the present invention provides a method for preparing an epoxy resin coating, comprising:
[0022] S1: Prepare 100 parts of fluorosilicone epoxy resin, 40-45 parts of polyetherimide curing agent, 10-13 parts of nano zinc oxide, and 7-10 parts of fluorinated surfactant respectively;
[0023] S2: dissolving nano zinc oxide in ethyl acetate, adding fluorinated surfactant dropwise while stirring, and stirring to mix evenly;
[0024] S3: Add polyetherimide curing agent to fluorosilicone epoxy resin at 45-60°C, mix well, and continue stirring for 10 minutes;
[0025] S4: gradually adding the mixture of nano zinc oxide and fluorinated surfactant to the mixture obtained in S3, stirring for 15 minutes to obtain a coating containing epoxy resin; and performing ultrasonic defoaming;
[0026] S5: After removing dirt from the surface of the oil layer casing, the coating obtained in S4 is evenly coated on the surface of the oil layer casing by spraying or dipping;
[0027] S6: Cured at 70-90°C for 2-4 hours and then cured at 110-130°C for 2-4 hours to form a smooth and hard protective layer.
[0028] In a specific embodiment of the present invention, the method comprises:
[0029] S1: Prepare 100 parts of fluorosilicone epoxy resin, 42.5 parts of polyetherimide curing agent, 10 parts of nano zinc oxide, and 7.5 parts of fluorinated surfactant respectively;
[0030] S2: dissolving nano zinc oxide in ethyl acetate, adding fluorinated surfactant dropwise while stirring, and stirring to mix evenly;
[0031] S3: Add polyetherimide curing agent to fluorosilicone epoxy resin at 45-60°C, mix well, and continue stirring for 10 minutes;
[0032] S4: gradually adding the mixture of nano zinc oxide and fluorinated surfactant to the mixture obtained in S3, stirring for 15 minutes to obtain a coating containing epoxy resin; and performing ultrasonic defoaming;
[0033] S5: After removing dirt from the surface of the oil layer casing, the coating obtained in S4 is evenly coated on the surface of the oil layer casing by spraying or dipping;
[0034] S6: Cured at 80°C for 2-4 hours and then cured at 125°C for 2-4 hours to form a smooth and hard protective layer.
[0035] One or more of the above technical solutions have the following beneficial effects:
[0036] The present invention provides an epoxy resin coating which effectively inhibits wax deposition and rusting of wellbore equipment. By optimizing the coating, the mechanical properties (wear resistance) and corrosion resistance of the wellbore equipment are effectively improved, and rusting is reduced. The wax deposition phenomenon is effectively prevented, the mining efficiency is improved, the service life of the wellbore equipment is extended, and the maintenance cost is reduced.
[0037] In the present invention, nano zinc oxide cooperates with fluorinated surfactant to effectively reduce the brittleness and poor mechanical properties caused by epoxy resin curing, and reduce the friction coefficient. At the same time, it is found that the epoxy resin coating provided by the present invention can effectively shorten the initial setting time of the coating without affecting the mechanical properties and corrosion resistance, and has practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a schematic diagram of the wellbore equipment structure and coating structure according to an embodiment of the present invention.
[0039] Figure 2 This is the corrosion resistance performance test result of the present invention.
[0040] Figure numerals: 1. Oil-conducting layer casing; 2. Coating containing epoxy resin. DETAILED DESCRIPTION
[0041] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0042] It should be noted that the terms used herein are for describing specific embodiments only and are not intended to be limiting of exemplary embodiments according to the present invention.
[0043] In the present invention, diphenyldiethoxysilane, CAS No.: 2553-19-7, was purchased from Maclean.
[0044] In the present invention, methyltriethoxysilane, CAS No.: 2031-67-6, was purchased from Maclean.
[0045] In the present invention, fluorosilane, CAS No.: 420-56-4, was purchased from Maclean.
[0046] In the present invention, epoxy resin NPEL-128 (industrial grade) was purchased from Shanghai Gongcheng Chemical Co., Ltd.
[0047] In the present invention, nano zinc oxide, CAS No.: 1314-13-2, is purchased from Aladdin, and when the size is 50±10nm, the item number is: Z112849; when the size of nano zinc oxide is 30±10nm, the item number is: Z112847.
[0048] In the present invention, Capstone FS-10, brand name: Capstone Capstone® FS-10, supplier is Chemours, purchased from Jintenglong Chemical.
[0049] In the present invention, the fluorosilicone epoxy resin is a modified epoxy resin. Epoxy resin has excellent adhesion, excellent electrical insulation, good mechanical properties, good corrosion resistance and chemical resistance, and is widely used in many fields such as civil engineering, electrical and electronic, coatings and plastics. However, the porosity and brittleness of epoxy resin limit its application, resulting in its mechanical properties and chemical resistance to be further improved. In the present invention, aminosiloxane and several siloxane coupling agents and fluorosilane are heated and hydrolyzed and condensed under certain pH conditions to react to generate fluorosilicone resin. Fluorosilicone resin is used as a modifier to modify epoxy resin, and the amino group in the fluorosilicone resin undergoes a ring-opening polymerization reaction with the epoxy group in the epoxy resin to obtain a fluorosilicone epoxy resin, which greatly improves the adhesion, hardness, impact resistance, heat resistance, water resistance and weather resistance of the paint film, making it more suitable for the needs of industrial production.
[0050] Specifically, the preparation method of fluorosilicone epoxy resin is as follows: diphenyldiethoxysilane, methyltriethoxysilane, fluorosilane, anhydrous ethanol and distilled water are mixed, placed in a reaction kettle, stirred and refluxed, the pH value is adjusted to 4-5 with 30% hydrochloric acid, the reflux temperature is controlled at 60-70°C, the reflux time is controlled at 2h, and after the reaction is completed, reduced pressure distillation (80°C, 0.5mmhg) is performed to obtain fluorosilicone resin, wherein the molar ratio of diphenyldiethoxysilane, methyltriethoxysilane, fluorosilane and anhydrous ethanol is 5:3:5:8, 40g of diphenyldiethoxysilane is used, and the volume of distilled water is twice the volume of the above mixture. Dissolve 10g of epoxy resin in isobutyl alcohol and butyl acetate, add 1g of fluorosilicone resin under stirring, add 0.1g of KH792 to catalyze the reaction, control the temperature and time of the reflux reaction, the reflux temperature is controlled at 60-70°C, and the reflux time is controlled at 4h; after the reaction is completed, perform reduced pressure distillation (80°C, 0.5mmhg) to obtain fluorosilicone epoxy resin.
[0051] In the present invention, the polyetherimide curing agent can interact with the fluorosilicone epoxy resin to form a cross-linked structure, thereby promoting the curing of the coating; the polyetherimide curing agent and the fluorosilicone epoxy resin can also cooperate with nano zinc oxide and a fluorine-containing surfactant to be dispersed in the cross-linked structure, thereby alleviating the disadvantages of the porosity and brittleness of the epoxy resin, further improving the adhesion of the epoxy resin-containing coating, reducing the friction coefficient, and improving the wear resistance; the interaction of the above three can effectively reduce the solidification time of the coating and save production costs.
[0052] In the present invention, nano zinc oxide is dispersed in the epoxy resin in a physical form and does not chemically react with the epoxy resin, but can improve the chemical corrosion resistance of the epoxy resin coating.
[0053] In the present invention, the fluorinated surfactant is added to the epoxy resin in a physical form and can interact with the epoxy resin through physical adsorption or chemical bonding to improve the surface properties of the coating, reduce the friction coefficient, improve the mechanical properties, and improve the anti-waxing performance.
[0054] Embodiment 1: This embodiment discloses an epoxy resin coated wellbore equipment and a method for manufacturing the same.
[0055] like Figure 1 As shown, a coating 2 containing epoxy resin is provided on the surface of an oil layer casing 1 of the wellbore equipment, and the diameter of the oil layer casing 1 is 5 inches.
[0056] Wherein, the preparation method of the coating containing epoxy resin is:
[0057] S1: prepare 1000g, 425g, 100g, and 75g of fluorosilicone epoxy resin, polyetherimide curing agent, nano zinc oxide, and FS-10 respectively;
[0058] S2: Dissolve nano zinc oxide in the same volume of ethyl acetate (there is no special requirement for the amount, as long as it can play the role of solvent), add FS-10 dropwise while stirring, and stir to mix evenly;
[0059] S3: At 60°C, add polyetherimide curing agent to fluorosilicone epoxy resin, use ethyl acetate as solvent, mix well, and continue stirring for 10 minutes;
[0060] S4: gradually add the mixture of nano zinc oxide and FS-10 to the mixture obtained in S3, and obtain the coating containing epoxy resin after stirring for about 15 minutes; in order to prevent the generation of bubbles, the above materials are treated by ultrasound, and the ultrasound conditions are: 800W, frequency 22kHz, treatment for 60min;
[0061] S5: Use steel grit jetting to remove oil, rust, corrosion and other dirt on the inner wall of the oil layer casing 1; dry the wellbore casing to ensure that the inner wall of the wellbore is dry;
[0062] S6: Use spraying or dipping process to evenly apply the mixed coating paint on the surface of the oil layer casing by 1mm;
[0063] S7: Cured at 80°C for 3 hours and then at 125°C for 2 hours to form a smooth and hard protective layer.
[0064] Through infrared spectrum measurement, it was found that the fluorosilicone epoxy resin had a CF stretching vibration peak at 1255 cm-1, which was a strong absorption; the c=c unsaturated bond stretching vibration in the benzene ring appeared at 1450 cm-1; the absorption peak of the si-O group was shown at 1093 cm-1; and the absorption peak of Si-C was at 823 cm-1, indicating that the epoxy resin had been successfully modified.
[0065] Example 2: The difference from Example 1 is that the fluorosilicone epoxy resin, polyetherimide curing agent, nano zinc oxide, and fluorinated surfactant are 1000g, 400g, 130g, and 80g respectively.
[0066] Comparative Example 1: The difference from Example 1 is that epoxy resin NPEL-128 is used.
[0067] Comparative Example 2: The difference from Example 1 is that the fluorinated surfactant FS-10 is not used.
[0068] Comparative Example 3: The difference from Comparative Example 1 is that the incubation surfactant FS-10 is not used.
[0069] Comparative Example 4: The difference from Comparative Example 1 is that the size of the nano zinc oxide is 30±10 nm.
[0070] In order to verify the improvement effect of the above-mentioned epoxy resin-containing coating on the wellbore device, the epoxy resin-containing coating is applied to the steel pipe of the inner wall material of the oil layer casing 1. Then a salt spray test is used to verify the protective effect of the coating on the inner wall of the oil layer casing 1, and its mechanical properties are tested.
[0071] After taking equal volumes of steel pipes for rust removal and decontamination treatment under the same conditions, one group was used as a control and no coating was sprayed, the second group was sprayed with the coating containing epoxy resin in Example 1, the third group was sprayed with the coating containing epoxy resin in Example 2, the fourth group was sprayed with the coating containing epoxy resin in Comparative Example 1, and the fifth group was sprayed with the coating containing epoxy resin in Comparative Example 2. The sixth group was sprayed with the coating containing epoxy resin in Comparative Example 3. The seventh group was sprayed with the coating containing epoxy resin in Comparative Example 4.
[0072] The salt spray test standard refers to GB / T 10125-2012 "Artificial atmosphere corrosion test salt spray test". Place the samples in the salt spray test chamber to ensure that the samples do not touch each other and keep a certain distance from the chamber wall. The temperature of the test chamber is controlled at 35℃±2℃ and the humidity is close to 100%. After 5 days, the weight change is counted.
[0073] Friction coefficient test: water is used as the medium, using MFT-5000 friction and wear tester, with a loading force of 80N, a rotation speed of 800rpm / min, and a test time of 20min. Wear amount test: water is used as the medium, using MFT-5000 friction and wear tester, with a loading force of 80N, a rotation speed of 800rpm / min, and a test time of 20min. The weight loss is taken as the wear amount.
[0074] Furthermore, in order to verify the protective effect of the coating on the wellbore equipment, the mechanical properties of the above seven groups were also verified.
[0075] The results show that the modified epoxy resin coating can effectively protect the equipment itself and improve the corrosion resistance of wellbore equipment ( Figure 2 ), there is no obvious difference in corrosion resistance by changing the nano zinc oxide or not using fluorinated surfactant.
[0076] Compared with pure epoxy resin coating, fluorosilicone epoxy resin coating is more wear-resistant and has a smaller friction coefficient. By comparison, it can also be found that both fluorosilicone epoxy resin and epoxy resin can effectively reduce the friction coefficient when zinc oxide and FS-10 are added at the same time. This is because zinc oxide and FS-10 work together to improve the flexibility of the curing agent and epoxy resin after cross-linking and curing.
[0077] Compared with pure epoxy coating, steel coated with fluorosilicone epoxy resin has higher mechanical properties (hardness and tensile strength). The introduction of fluorosilicone resin into epoxy coating helps to increase the tensile strength from 480.05MPa to 630.82MPa, which is 31% higher than pure epoxy coating. It was also found that the particle size of zinc oxide has an effect on improving the adhesion of the coating, but considering its effect on the friction coefficient and tensile strength, it was not adopted in the future.
[0078] The mechanical properties test results (Table 1) show that the fluorosilicone epoxy resin coating in Example 1 has good adhesion and mechanical properties.
[0079] Table 1: Mechanical properties test results
[0080]
[0081] During the spraying process, it was found that the initial setting time for groups 2 and 3 was only 20 minutes, while the other groups required more than 30 minutes.
[0082] The wellbore equipment in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention is used for oil production operations.
[0083] During use, the surface of the oil layer casing 1 was dewaxed every one month. It was found that the wax deposition in Example 1 was the least, and that in Comparative Example 2, the wax deposition was the most serious because the fluorinated surfactant was not used and the wax melting effect could not be exerted.
[0084] In addition, the annual output was statistically analyzed, and it was found that the oil production of the wellbore equipment with fluorosilicone epoxy resin coating in Example 1 increased to 0.20 times the original amount after use, and the oil production of the wellbore equipment in Comparative Example 1 and Comparative Example 2 increased to 0.13 times and 0.11 times the original amount after use.
[0085] In terms of service life, the wellbore equipment in Comparative Example 2 began to corrode and break 12 months after being put into production, the wellbore equipment in Comparative Example 1 began to corrode and break 14 months after being put into production, and the wellbore equipment in Example 1 began to corrode and break 18 months after being put into production, effectively extending the service life.
[0086] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An epoxy resin coated wellbore equipment, characterized in that: It comprises an oil layer casing (1), the surface of which is provided with a coating (2) containing epoxy resin; The epoxy resin-containing coating is composed of modified epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent; The modified epoxy resin is a fluorosilicone epoxy resin; Amino-containing siloxane, several siloxane coupling agents and fluorosilane are heated and hydrolyzed and condensed under certain pH conditions to generate fluorosilicone resin; fluorosilicone resin is used as a modifier to modify epoxy resin, and the amino groups in the fluorosilicone resin react with the epoxy groups in the epoxy resin to generate fluorosilicone epoxy resin; The anti-wax agent is Capstone FS-10; The corrosion-resistant filler is nano zinc oxide; The added weights of the epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent are 100 parts, 40-45 parts, 10-13 parts and 7-10 parts respectively.
2. The epoxy resin coating wellbore equipment according to claim 1, characterized in that: The amine curing agent is a polyetherimide curing agent.
3. The epoxy resin coating wellbore equipment according to claim 1, characterized in that: The preparation method of the fluorosilicone epoxy resin is: Mixing organosiloxane, fluorosilane, anhydrous ethanol and distilled water, stirring and refluxing, adjusting the pH value to 4-5 with hydrochloric acid, and refluxing under reduced pressure distillation to obtain fluorosilicone resin; The epoxy resin is diluted with isobutyl alcohol and butyl acetate, and the fluorosilicone resin is added under stirring, and the fluorosilicone resin epoxy resin is obtained by reflux and reduced pressure distillation.
4. The epoxy resin coating wellbore equipment according to claim 1, characterized in that: The added weights of the epoxy resin, amine curing agent, corrosion-resistant filler and anti-waxing agent are 100 parts, 42 parts, 10 parts and 8 parts respectively.
5. The epoxy resin coating wellbore equipment according to claim 2, characterized in that: The thickness of the coating is 0.5 mm to 2 mm.
6. A method for preparing an epoxy resin coating, characterized in that: include, S1: Prepare 100 parts of fluorosilicone epoxy resin, 40-45 parts of polyetherimide curing agent, 10-13 parts of nano zinc oxide, and 7-10 parts of FS-10 respectively; S2: Dissolve nano zinc oxide in ethyl acetate, add FS-10 while stirring, and stir to mix evenly; S3: Add polyetherimide curing agent to fluorosilicone epoxy resin at 45-60°C, mix well, and continue stirring for 10 minutes; S4: gradually adding the mixture of nano zinc oxide and FS-10 to the mixture obtained in S3, stirring for 15 minutes to obtain a coating containing epoxy resin; and ultrasonically defoaming; S5: After removing dirt from the surface of the oil layer casing, the coating obtained in S4 is evenly coated on the surface of the oil layer casing by spraying or dipping; S6: Curing at 70-90°C for 2-4 hours and then curing at 110-130°C for 2-4 hours to form a smooth and hard protective layer; The fluorosilicone epoxy resin is prepared by heating and hydrolyzing condensing aminosiloxane, several siloxane coupling agents and fluorosilane under certain pH conditions to generate fluorosilicone resin; the fluorosilicone resin is used as a modifier to modify the epoxy resin, and the amino groups in the fluorosilicone resin and the epoxy groups in the epoxy resin undergo ring-opening polymerization to obtain the fluorosilicone epoxy resin.
7. The method for preparing an epoxy resin coating according to claim 6, characterized in that: include, S1: Prepare 100 parts of fluorosilicone epoxy resin, 42.5 parts of polyetherimide curing agent, 10 parts of nano zinc oxide, and 7.5 parts of FS-10 respectively; S2: Dissolve nano zinc oxide in ethyl acetate, add FS-10 while stirring, and stir to mix evenly; S3: Add polyetherimide curing agent to fluorosilicone epoxy resin at 45-60°C, mix well, and continue stirring for 10 minutes; S4: gradually adding the mixture of nano zinc oxide and FS-10 to the mixture obtained in S3, stirring for 15 minutes to obtain a coating containing epoxy resin; and ultrasonically defoaming; S5: After removing dirt from the surface of the oil layer casing, the coating obtained in S4 is evenly coated on the surface of the oil layer casing by spraying or dipping; S6: Cured at 80°C for 2-4 hours and then cured at 125°C for 2-4 hours to form a smooth and hard protective layer.