Preparation method of lightweight automobile chassis adhesive with good sound insulation effect

By compounding liquid rubber-polyurethane emulsion with asphalt in automobile chassis glue, the problems of poor sound insulation, heat resistance and waterproof performance of chassis glue are solved, achieving better noise isolation and thermal management, and improving In-car tranquility and driving safety.

CN118580771BActive Publication Date: 2024-10-01GUANGZHOU HELIOSON CAR CARE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411062442.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing automobile chassis glue has poor sound insulation effect when faced with sand and gravel impact and mechanical transmission vibration noise, and its heat resistance and waterproof performance are insufficient, affecting the sense of quietness in the car and driving safety.

Method used

A preparation method is adopted to react castor oil-based polyol with compounds such as bishydroxybenzene perfluorodiazolone and hydroxyl-terminated polybutadiene acrylonitrile under a nitrogen atmosphere to form a liquid rubber-polyurethane emulsion and asphalt composite. Formulate, add fillers and stabilizers to form a lightweight car chassis glue with good sound insulation effect.

Benefits of technology

It improves the sound insulation, heat resistance and waterproof performance of automobile chassis glue, reduces noise and heat conduction, enhances the elasticity and dynamic mechanical properties of the material, and ensures a wider operating temperature range and better impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of automobile chassis adhesives and discloses a method for preparing a lightweight automobile chassis adhesive with good sound insulation effect. Highly heat-resistant phthalazinone is used to replace traditional small molecule diols, so that the thermal decomposition temperature of polyurethane hard segment and soft segment is significantly improved; terminal hydroxyl polybutadiene acrylonitrile contains a large number of butadiene segments, which have a strong force on the hard segment of polyurethane and require more energy to break; its molecular chain contains two segments of non-polar butadiene and highly polar acrylonitrile, and has the properties of liquid rubber. When subjected to external force, the molecular chain can fully move to form a change that lags behind the external stress, and the absorbed mechanical energy is converted into heat energy and dissipated, creating conditions for the formation of high damping and a wide temperature range of the material, and having a good sound insulation effect; the perfluorinated molecular chain in its structure has hydrophobicity, further improves the waterproof performance, and broadens its application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile chassis adhesives, in particular to a method for preparing a lightweight automobile chassis adhesive with good sound insulation effect. Background Art

[0002] With the rapid development of the domestic automobile industry, people are more and more aware of automobile protection. The automobile chassis is one of the most important parts of the automobile structure. From the time a new car rolls off the production line to the time it is scrapped, the chassis has been bearing the mission of supporting the car body, enduring the most complex and harshest environment, experiencing the attack of sand and gravel rolled up by high-speed rotating wheels, facing rain, snow, mud and other erosion at any time, and occasionally encountering scratches and damage from bumpy roads; at the same time, with the improvement of people's living standards, people also pursue comfort and quietness in the car. Automobile chassis glue is a protective material that is sprayed on exposed parts such as the chassis and wheel hub of the vehicle to form a firm elastic protective layer. However, the existing chassis glue does not reduce the noise caused by the impact of sand and gravel and the vibration noise generated by mechanical transmission. The noise pollution in the car caused by this seriously affects the driving experience and driving safety of the car owner. Therefore, preparing an automobile chassis glue with good sound insulation effect has become a problem that needs to be solved urgently.

[0003] Asphalt resources are abundant, cost-effective, and has high anti-corrosion properties, but asphalt products also have some shortcomings. Pure asphalt has serious performance deficiencies: in winter, the coating is too hard and brittle, with weak adhesion, and will break into pieces when hit by sand and gravel. It may even crack and fall off because the thermal expansion and contraction coefficient is too different from that of the metal substrate. In summer, the coating becomes too soft and sticky, easily attracts dust, and even experiences heat flow. Currently, the commonly used shock-absorbing and sound-insulating material is rubber damping material, but its elasticity and damping properties are easily affected by ambient temperature, and its heat dissipation coefficient is small. It is easy to generate heat under alternating loads, causing thermal stress fatigue and aging, which causes degradation of the elastic damping properties.

[0004] The chassis of automobiles needs to experience very harsh environments and is often attacked by heat from exhaust emissions and mechanical friction. It needs to be not only resistant to high temperatures but also waterproof. The polyurethane molecular chain contains a large number of polar groups with strong intermolecular forces and hydrogen bonds, which can effectively protect the chassis from being hit by road gravel and produce good sound insulation effects. The present invention aims to synthesize a heat-resistant and waterproof polyurethane resin, which is compounded with asphalt to not only reduce the conduction of noise during driving and increase driving tranquility, but also prevent heat conduction from the chassis iron plate, making the cab warm in winter and cool in summer. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a lightweight automobile chassis adhesive with good sound insulation effect, thereby solving the problems of poor sound insulation effect, heat resistance and waterproof performance of the existing automobile chassis adhesive.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a lightweight automobile chassis adhesive with good sound insulation effect comprises the following steps:

[0008] Step (1): under nitrogen atmosphere, castor oil-based polyol is added to the reaction kettle, and the mixture is distilled under reduced pressure at a temperature of 110-125°C and a pressure of 0.05-0.08 MPa for 2-4 hours, then the temperature is lowered to 40-50°C, dibutyltin dilaurate catalyst, trimethylolpropane and isophorone diisocyanate are added, the temperature is raised to 75-90°C and the mixture is reacted for 1-3 hours, and then a compound having the structural formula The dihydroxybenzene perfluorophthalazinone and terminal hydroxy polybutadiene acrylonitrile are reacted for 0.5-1h, during which acetone is added to reduce the viscosity, and then the temperature is lowered to 45-55°C, triethylamine is added to adjust the pH to 8-9, deionized water is added, and after stirring evenly, a liquid rubber-polyurethane emulsion is obtained.

[0009] Step (2): Place the asphalt dispersion and the liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 150-250 r / min, add filler and calcium zinc stabilizer, disperse them at 800-1000 r / min for 10-20 min, finally add defoamer, wetting dispersant and rust inhibitor, stir them at 200-400 r / min for 5-15 min, and after high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect.

[0010] Furthermore, in step (1), the ratio of castor oil-based polyol, dibutyltin dilaurate catalyst, trimethylolpropane, isophorone diisocyanate, dihydroxyphenylperfluorophthalazinone, and terminal hydroxyl polybutadiene acrylonitrile is 100 g: (4-8) g: (3-5) g: (25-40) g: (1-5) g: (2-10) g.

[0011] Furthermore, in step (2), the filler is any one of talcum powder, hollow glass microspheres or light calcium carbonate.

[0012] Furthermore, in step (2), the ratio of asphalt dispersion, liquid rubber-polyurethane emulsion, filler, and calcium zinc stabilizer is (40-60) g: (3-15) g: (35-50) g: (1-3) g.

[0013] Furthermore, the method for preparing the bishydroxybenzene perfluorophthalazinone in step (1) comprises the following steps:

[0014] Step S1: Under a nitrogen atmosphere, add 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and dimethyl sulfoxide to a reaction flask, stir evenly, add dibromoperfluoro compound and potassium hydroxide, stir to react, and after the reaction is completed, cool to room temperature, extract with chloroform and deionized water, concentrate the organic phase, and dry to obtain bismethoxyphenylperfluorophthalazinone. The preparation reaction formula is as follows:

[0015]

[0016] Step S2: Under nitrogen atmosphere, add bis(methoxyphenylperfluorophthalazinone) and dichloromethane to a reaction flask, stir evenly, add boron tribromide, react at 0-20°C for 12-24h, extract with ethyl acetate and deionized water, concentrate the organic phase, and dry to obtain bis(hydroxyphenylperfluorophthalazinone). The preparation reaction formula is as follows:

[0017]

[0018] Furthermore, in step S1, the dibrominated perfluoro compound is any one of 1,4-dibromooctafluorobutane, 1,6-dibromoperfluorohexane or 1,8-dibromohexafluorooctane.

[0019] Furthermore, in step S1, the ratio of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone, dibromoperfluoro compound, and potassium hydroxide is (2.1-2.3) mol: 1 mol: (2.4-3.3) mol.

[0020] Furthermore, in step S1, the reaction temperature is 75-90° C., and the reaction time is 3-8 h.

[0021] Furthermore, in step S2, the ratio of bismethoxyphenylperfluorophthalazinone to boron tribromide is 1 mol: (2.5-4) mol.

[0022] By adopting the above technical solution, the beneficial effects of the present invention are:

[0023] The invention firstly reacts 4-(4-methoxyphenyl)-1-(2H)-phthalazinone with a dibromoperfluoro compound under the action of potassium hydroxide to obtain bismethoxyphenylperfluorophthalazinone, then removes the methoxy group under the action of boron tribromide to obtain bishydroxyphenylperfluorophthalazinone, then polymerizes castor oil-based polyol and isophorone diisocyanate under the action of an initiator, uses bishydroxyphenylperfluorophthalazinone and terminal hydroxyl polybutadiene acrylonitrile as chain extenders to obtain liquid rubber-polyurethane emulsion, and finally mixes with asphalt, filler and the like to obtain a lightweight automobile chassis adhesive with good sound insulation effect.

[0024] Phthalocyanine has a twisted, non-coplanar structure, which greatly affects the relative movement between the polyurethane macromolecular fragments, causing the molecular chains to entangle with each other, which can increase the proportion of hard segments in the molecular skeleton of the polyurethane material, and the highly heat-resistant nitrogen heterocyclic structure replaces the traditional small molecule diol, which significantly increases the thermal decomposition temperature of its hard and soft segments; on the other hand, terminal hydroxyl polybutadiene acrylonitrile contains a large number of butadiene segments, which have a strong interaction with the hard segments of the polyurethane, and require more energy to break, so it can remain stable at a higher temperature; the perfluorinated molecular chain in its structure has hydrophobic properties, the carbon-fluorine bond has a short bond length and a large bond energy, and the atomic electron cloud has a stronger shielding property for the CC bond than the H atom, so that the prepared composite material has a low surface free energy, and a very thin molecular layer can be formed on the surface of the material, thereby reducing the surface energy and preventing water droplets from staying on the surface, thereby achieving a hydrophobic effect; at the same time, its long chain can be entangled and tightly connected with the polyurethane matrix, so that the molecular chain produces intermolecular association, forming a supramolecular network structure, and further improving the waterproof performance.

[0025] The molecular structure of the polyurethane resin after chain extension by dihydroxybenzene perfluorophthalazinone and terminal hydroxyl polybutadiene acrylonitrile has a large steric hindrance, and its macromolecular chain contains a large number of polar groups, such as ester groups, ether groups, carbamate groups, urea groups, biuret groups and allophanate groups, which have strong intermolecular forces and hydrogen bonds, making it elastic, with good shock absorption and dynamic mechanical properties and a wide operating temperature range; at the same time, the terminal hydroxyl polybutadiene acrylonitrile molecular chain contains two chain segments, non-polar butadiene and highly polar acrylonitrile, and has the properties of liquid rubber. When subjected to external force, the molecular chain can fully move, forming a change that lags behind the external stress, converting the absorbed mechanical energy into heat energy and dissipating it, creating conditions for the formation of high damping and a wide temperature range of the material, and broadening its application range. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] 4-(4-Methoxyphenyl)-1-(2H)-phthalazinone, CAS number is 57353-93-2.

[0028] 1,4-Dibromooctafluorobutane, CAS number is 335-48-8.

[0029] 1,6-Dibromoperfluorohexane, CAS number is 918-22-9.

[0030] 1,8-Dibromohexafluorooctane, CAS number is 8125-58-8. Example 1

[0031] (1) Under nitrogen atmosphere, 88 mmol of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and 600 mL of dimethyl sulfoxide were added to a reaction flask. After stirring, 40 mmol of 1,4-dibromooctafluorobutane and 112 mmol of potassium hydroxide were added. The mixture was reacted at 85 °C for 5 h. The mixture was cooled to room temperature, extracted with chloroform and deionized water, and the organic phase was concentrated and dried to obtain dimethoxyphenylperfluorophthalazinone.

[0032] (2) Under nitrogen atmosphere, 35 mmol of bis(methoxyphenyl)perfluorophthalazinone and 1450 mL of dichloromethane were added to a reaction flask. After stirring, 112 mmol of boron tribromide was added. The mixture was reacted at 5°C for 16 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and dried to obtain bis(hydroxyphenyl)perfluorophthalazinone.

[0033] (3) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to the reactor and distilled under reduced pressure at a temperature of 115 °C and a pressure of 0.06 MPa for 3 h. The temperature was then reduced to 45 °C, and 5 g of dibutyltin dilaurate catalyst, 4 g of trimethylolpropane and 35 g of isophorone diisocyanate were added. The temperature was raised to 80 °C and the reaction was continued for 2 h. Subsequently, 1 g of dihydroxyphenylperfluorophthalazinone and 2 g of terminal hydroxy polybutadiene acrylonitrile were added and the reaction was continued for 0.5 h. During this period, acetone was added to reduce the viscosity. The temperature was then reduced to 50 °C, triethylamine was added to adjust the pH to 9, and deionized water was added. After stirring, a liquid rubber-polyurethane emulsion was obtained.

[0034] (4) Place 50 g of asphalt dispersion and 3 g of liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 200 r / min, add 45 g of talcum powder and 2 g of calcium zinc stabilizer, disperse them at 950 r / min for 15 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir at 300 r / min for 10 min. After high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect. Example 2

[0035] (1) Under nitrogen atmosphere, 178.5 mmol of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and 850 mL of dimethyl sulfoxide were added to a reaction flask. After stirring, 85 mmol of 1,6-dibromoperfluorohexane and 204 mmol of potassium hydroxide were added. The mixture was reacted at 90 °C for 3 h. The mixture was cooled to room temperature, extracted with chloroform and deionized water, and the organic phase was concentrated and dried to obtain dimethoxyphenylperfluorophthalazinone.

[0036] (2) Under nitrogen atmosphere, 70 mmol of bis(methoxyphenyl)perfluorophthalazinone and 2100 mL of dichloromethane were added to a reaction flask. After stirring, 175 mmol of boron tribromide was added. The mixture was reacted at 20°C for 12 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and dried to obtain bis(hydroxyphenyl)perfluorophthalazinone.

[0037] (3) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to the reactor, and the mixture was distilled under reduced pressure at a temperature of 125 °C and a pressure of 0.08 MPa for 2 h. The temperature was then reduced to 50 °C, and 4 g of dibutyltin dilaurate catalyst, 3 g of trimethylolpropane and 25 g of isophorone diisocyanate were added. The mixture was heated to 90 °C and reacted for 1 h. Subsequently, 2 g of dihydroxyphenylperfluorophthalazinone and 4 g of terminal hydroxy polybutadiene acrylonitrile were added and the reaction was continued for 1 h. During this period, acetone was added to reduce the viscosity. The mixture was then cooled to 55 °C, triethylamine was added to adjust the pH to 8, and deionized water was added. The mixture was stirred evenly to obtain a liquid rubber-polyurethane emulsion.

[0038] (4) Place 40 g of asphalt dispersion and 6 g of liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 250 r / min, add 35 g of hollow glass microspheres and 3 g of calcium zinc stabilizer, disperse them at 1000 r / min for 10 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir at 400 r / min for 5 min. After high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect. Example 3

[0039] (1) Under nitrogen atmosphere, 69 mmol of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and 600 mL of dimethyl sulfoxide were added to a reaction flask. After stirring, 30 mmol of 1,8-dibromohexafluorooctane and 99 mmol of potassium hydroxide were added. The mixture was reacted at 75 °C for 8 h. The mixture was cooled to room temperature, extracted with chloroform and deionized water, and the organic phase was concentrated and dried to obtain dimethoxyphenylperfluorophthalazinone.

[0040] (2) Under nitrogen atmosphere, 25 mmol of bis(methoxyphenyl)perfluorophthalazinone and 1125 mL of dichloromethane were added to a reaction flask. After stirring, 100 mmol of boron tribromide was added. The mixture was reacted at 0°C for 24 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and dried to obtain bis(hydroxyphenyl)perfluorophthalazinone.

[0041] (3) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to the reactor, and the mixture was distilled under reduced pressure at a temperature of 110 °C and a pressure of 0.05 MPa for 4 h. The temperature was then reduced to 40 °C, and 8 g of dibutyltin dilaurate catalyst, 5 g of trimethylolpropane and 40 g of isophorone diisocyanate were added. The mixture was heated to 75 °C and reacted for 3 h. Subsequently, 3 g of dihydroxyphenylperfluorophthalazinone and 6 g of terminal hydroxy polybutadiene acrylonitrile were added, and the reaction was continued for 0.5 h. During the reaction, acetone was added to reduce the viscosity. The mixture was then cooled to 45 °C, triethylamine was added to adjust the pH to 9, and deionized water was added. The mixture was stirred evenly to obtain a liquid rubber-polyurethane emulsion.

[0042] (4) Place 60 g of asphalt dispersion and 9 g of liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 150 r / min, add 50 g of light calcium carbonate and 1 g of calcium zinc stabilizer, disperse them at 800 r / min for 20 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir at 200 r / min for 15 min. After high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect. Example 4

[0043] (1) Under nitrogen atmosphere, 97.2 mmol of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and 720 mL of dimethyl sulfoxide were added to a reaction flask. After stirring, 45 mmol of 1,4-dibromooctafluorobutane and 126 mmol of potassium hydroxide were added. The mixture was reacted at 85 °C for 7 h. The mixture was cooled to room temperature, extracted with chloroform and deionized water, and the organic phase was concentrated and dried to obtain dimethoxyphenylperfluorophthalazinone.

[0044] (2) Under nitrogen atmosphere, 35 mmol of bis(methoxyphenyl)perfluorophthalazinone and 1260 mL of dichloromethane were added to a reaction flask. After stirring, 112 mmol of boron tribromide was added. The mixture was reacted at 10°C for 24 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and dried to obtain bis(hydroxyphenyl)perfluorophthalazinone.

[0045] (3) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to the reactor, and the mixture was distilled under reduced pressure at a temperature of 120 °C and a pressure of 0.05 MPa for 4 h. The temperature was then reduced to 50 °C, and 7 g of dibutyltin dilaurate catalyst, 5 g of trimethylolpropane and 35 g of isophorone diisocyanate were added. The mixture was heated to 85 °C and reacted for 2 h. Subsequently, 4 g of dihydroxyphenylperfluorophthalazinone and 8 g of terminal hydroxy polybutadiene acrylonitrile were added, and the reaction was continued for 1 h. During this period, acetone was added to reduce the viscosity. The mixture was then cooled to 55 °C, triethylamine was added to adjust the pH to 8, and deionized water was added. The mixture was stirred evenly to obtain a liquid rubber-polyurethane emulsion.

[0046] (4) Place 45 g of asphalt dispersion and 12 g of liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 220 r / min, add 40 g of talcum powder and 2 g of calcium zinc stabilizer, disperse them at 950 r / min for 20 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir at 400 r / min for 15 min. After high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect. Example 5

[0047] (1) Under nitrogen atmosphere, 45 mmol of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and 320 mL of dimethyl sulfoxide were added to a reaction flask. After stirring, 20 mmol of 1,6-dibromoperfluorohexane and 64 mmol of potassium hydroxide were added. The mixture was reacted at 90 °C for 5 h. The mixture was cooled to room temperature, extracted with chloroform and deionized water, and the organic phase was concentrated and dried to obtain dimethoxyphenylperfluorophthalazinone.

[0048] (2) Under nitrogen atmosphere, 15 mmol of bis(methoxyphenyl)perfluorophthalazinone and 620 mL of dichloromethane were added to a reaction flask. After stirring, 54 mmol of boron tribromide was added. The mixture was reacted at 0°C for 24 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and dried to obtain bis(hydroxyphenyl)perfluorophthalazinone.

[0049] (3) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to the reactor, and the mixture was distilled under reduced pressure at a temperature of 115 °C and a pressure of 0.08 MPa for 4 h. The temperature was then reduced to 40 °C, and 8 g of dibutyltin dilaurate catalyst, 5 g of trimethylolpropane and 30 g of isophorone diisocyanate were added. The mixture was heated to 90 °C and reacted for 2 h. Subsequently, 5 g of dihydroxyphenylperfluorophthalazinone and 10 g of terminal hydroxy polybutadiene acrylonitrile were added, and the reaction was continued for 0.5 h. During the reaction, acetone was added to reduce the viscosity. The mixture was then cooled to 50 °C, triethylamine was added to adjust the pH to 9, and deionized water was added. The mixture was stirred evenly to obtain a liquid rubber-polyurethane emulsion.

[0050] (4) Place 55 g of asphalt dispersion and 15 g of liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 250 r / min, add 40 g of hollow glass microspheres and 3 g of calcium zinc stabilizer, disperse them at 950 r / min for 12 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir them at 360 r / min for 15 min, and after high-speed dispersion, spray them evenly on the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect.

[0051] Comparative Example 1

[0052] (1) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to a reactor, and the mixture was distilled under reduced pressure at a temperature of 115 °C and a pressure of 0.06 MPa for 3 h. The temperature was then lowered to 45 °C, and 5 g of dibutyltin dilaurate catalyst, 4 g of trimethylolpropane and 35 g of isophorone diisocyanate were added. The mixture was heated to 80 °C and reacted for 2 h. Subsequently, 1 g of 1,4-butanediol and 2 g of terminal hydroxyl polybutadiene acrylonitrile were added, and the reaction was continued for 0.5 h. During the reaction, acetone was added to reduce the viscosity. The mixture was then cooled to 50 °C, and triethylamine was added to adjust the pH to 9. Deionized water was added, and the mixture was stirred evenly to obtain a polyurethane emulsion.

[0053] (2) Place 50 g of asphalt dispersion and 3 g of polyurethane emulsion in a vacuum device, first mix them evenly at 200 r / min, add 45 g of talcum powder and 2 g of calcium zinc stabilizer, disperse them at 950 r / min for 15 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir at 300 r / min for 10 min, and after high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive.

[0054] Comparative Example 2

[0055] (1) Under nitrogen atmosphere, 100 g of castor oil-based polyol was added to the reactor, and the mixture was distilled under reduced pressure at a temperature of 115 °C and a pressure of 0.06 MPa for 3 h. The temperature was then reduced to 45 °C, and 5 g of dibutyltin dilaurate catalyst, 4 g of trimethylolpropane and 35 g of isophorone diisocyanate were added. The mixture was heated to 80 °C and reacted for 2 h. Subsequently, 1 g of 1,4-butanediol was added and the reaction was continued for 0.5 h. During this period, acetone was added to reduce the viscosity. The mixture was then cooled to 50 °C, triethylamine was added to adjust the pH to 9, and deionized water was added. The mixture was stirred evenly to obtain a polyurethane emulsion.

[0056] (2) Place 50 g of asphalt dispersion and 3 g of polyurethane emulsion in a vacuum device, first mix them evenly at 200 r / min, add 45 g of talcum powder and 2 g of calcium zinc stabilizer, disperse them at 950 r / min for 15 min, and finally add 0.5 g of defoamer BKY-1970, 0.3 g of wetting dispersant OT-75 and 0.05 g of rust inhibitor WD-40, stir at 300 r / min for 10 min, and after high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive.

[0057] Comparative Example 3

[0058] Place 50g of asphalt dispersion in a vacuum device, add 45g of talcum powder and 2g of calcium zinc stabilizer, disperse at 950r / min for 15min, finally add 0.5g of defoamer BKY-1970, 0.3g of wetting dispersant OT-75 and 0.05g of rust inhibitor WD-40, stir at 300r / min for 10min, and after high-speed dispersion, evenly spray it on the automobile chassis to obtain a lightweight automobile chassis adhesive.

[0059] Preparation of test adhesive film: After the lightweight automobile chassis adhesive is cured at room temperature, a lightweight automobile chassis adhesive film is obtained.

[0060] Heat resistance test: Weigh 5 mg of the prepared lightweight automobile chassis glue, test the temperature at 20-700°C in a nitrogen atmosphere at a heating rate of 20°C / min.

[0061] Table 1 Heat resistance test

[0062] Initial decomposition temperature (℃) Maximum rate thermal decomposition temperature (℃) Example 1 245.8 368.4 Example 2 253.6 375.3 Example 3 261.5 380.1 Example 4 268.1 382.9 Example 5 270.3 385.0 Comparative Example 1 231.7 325.6 Comparative Example 2 224.6 308.4 Comparative Example 3 218.2 300.7

[0063] It can be seen from the test results in the above table that with the increase of the content of dihydroxybenzene perfluorophthalazinone and terminal hydroxyl polybutadiene acrylonitrile, the heat resistance of the lightweight automobile chassis adhesive is gradually enhanced. The initial thermal decomposition temperature in Example 4 is 268.1°C, and the maximum rate thermal decomposition temperature is 382.9°C. This is because, on the one hand, phthalazinone has a twisted, non-coplanar structure, which greatly affects the relative movement between the polyurethane macromolecular fragments, causing the molecular chains to entangle with each other, which can increase the proportion of hard segments in the molecular skeleton of the polyurethane material, and the highly heat-resistant nitrogen heterocyclic structure replaces the traditional small molecule diol, which significantly improves the thermal decomposition temperature of its hard segment and soft segment; on the other hand, terminal hydroxyl polybutadiene acrylonitrile contains a large amount of butadiene segments, which have a strong interaction with the hard segment of the polyurethane, and requires more energy to break, so it can remain stable at a higher temperature.

[0064] The chain extender in Comparative Example 1 is a small molecule diol and terminal hydroxyl polybutadiene acrylonitrile, which has a certain heat resistance; Comparative Example 2 contains only a small molecule diol and has average heat resistance; Comparative Example 3 does not contain polyurethane and has the worst heat resistance.

[0065] Water absorption test: Weigh a dry film with a mass of m0, soak it in deionized water for 48 hours, wipe off the moisture on the surface of the coating, weigh the coating mass m1, and the water absorption rate = (m1-m0) / m0×100%.

[0066] Table 2 Waterproof performance test

[0067] Water absorption (%) Example 1 2.15 Example 2 1.36 Example 3 0.84 Example 4 0.47 Example 5 0.31 Comparative Example 1 7.56 Comparative Example 2 8.54 Comparative Example 3 10.52

[0068] It can be seen from the test results in the above table that with the increase of the content of bishydroxybenzene perfluorophthalazinone, the water absorption rate of the automobile chassis glue gradually decreases, wherein the water absorption rate in Example 5 is only 0.31%. This is because bishydroxybenzene perfluorophthalazinone contains perfluorinated molecular chains with hydrophobic properties, the carbon-fluorine bond has a short bond length and a large bond energy, and the atomic electron cloud has a stronger shielding property for the CC bond than the H atom, so that the prepared composite material has a low surface free energy, and a very thin molecular layer can be formed on the surface of the material, thereby reducing the surface energy, so that water droplets cannot stay on the surface, thereby achieving a hydrophobic effect; at the same time, its long chain can be entangled and closely connected with the polyurethane matrix, so that the molecular chain produces intermolecular association, forming a supramolecular network structure, and further improving the waterproof performance.

[0069] Damping and sound insulation performance test: The damping performance of the automobile chassis glue is tested using a dynamic mechanical analyzer. The temperature test range is -50 to 100°C, the heating rate is 3°C / min, and the test frequency is 1Hz.

[0070] Table 3 Damping sound insulation performance test

[0071] tanδ Effective damping area (℃) Example 1 1.248 -15.0 to 54.3 Example 2 1.260 -16.3 to 55.9 Example 3 1.285 -16.9 to 57.4 Example 4 1.301 -17.3 to 58.6 Example 5 1.324 -18.6 to 62.3 Comparative Example 1 0.853 -12.6 to 50.5 Comparative Example 2 0.721 -11.2 to 48.2 Comparative Example 3 0.625 -8.5 to 44.1

[0072] Damping is the characteristic of any system that the vibration amplitude gradually decreases due to external forces and internal reasons of the system when it vibrates. The damping coefficient tanδ can be used to evaluate the sound-absorbing effect of the material on sound waves. A higher damping coefficient means better sound-absorbing performance. From the test results in the above table, it can be seen that with the increase of the content of dihydroxybenzene perfluorophthalazinone and terminal hydroxy polybutadiene acrylonitrile, the damping and sound insulation performance of the automobile chassis adhesive gradually increases. This is because the molecular structure of the polyurethane resin after chain extension has a large steric hindrance, and its macromolecular chain contains a large number of polar groups, such as ester groups, ether groups, and amino groups. The ester group, urea group, biuret group and allophanate group have strong intermolecular forces and hydrogen bonds, making it elastic, with good shock absorption and dynamic mechanical properties and a wide temperature range. At the same time, the hydroxy-terminated polybutadiene acrylonitrile molecular chain contains two segments, non-polar butadiene and highly polar acrylonitrile, which has the properties of liquid rubber. When subjected to external force, the molecular chain can fully move, forming a change that lags behind the external stress, converting the absorbed mechanical energy into heat energy and dissipating it, creating conditions for the formation of high damping and a wide temperature range of the material, and broadening its application range.

[0073] Adhesion test: measured in accordance with GB / T9286-98 standard.

[0074] Impact resistance test: According to GB / T1732-93 standard, a heavy hammer with fixed mass is dropped at a certain height on the test plate coated with the sample to be tested, and the maximum height at which the film is not damaged is observed.

[0075] Table 4 Mechanical properties test

[0076] Adhesion (grade) Impact resistance (cm) Example 1 1 120 Example 2 1 129 Example 3 0 145 Example 4 0 156 Example 5 0 160 Comparative Example 1 2 58 Comparative Example 2 2 45 Comparative Example 3 5 35

[0077] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A method for preparing a lightweight automobile chassis adhesive with good sound insulation effect, characterized in that: The preparation method comprises the following steps: Step (1): under nitrogen atmosphere, castor oil-based polyol is added to the reaction kettle, and the mixture is distilled under reduced pressure at a temperature of 110-125°C and a pressure of 0.05-0.08 MPa for 2-4 hours, then the temperature is lowered to 40-50°C, dibutyltin dilaurate catalyst, trimethylolpropane and isophorone diisocyanate are added, the temperature is raised to 75-90°C and the mixture is reacted for 1-3 hours, and then a compound having the structural formula The bishydroxybenzene perfluorophthalazinone and the terminal hydroxy polybutadiene acrylonitrile are reacted for 0.5-1h, during which acetone is added to reduce the viscosity, and then the temperature is lowered to 45-55°C, triethylamine is added to adjust the pH to 8-9, deionized water is added, and after stirring evenly, a liquid rubber-polyurethane emulsion is obtained; Step (2): Place the asphalt dispersion and the liquid rubber-polyurethane emulsion in a vacuum device, first mix them evenly at 150-250 r / min, add filler and calcium zinc stabilizer, disperse them at 800-1000 r / min for 10-20 min, finally add defoamer, wetting dispersant and rust inhibitor, stir them at 200-400 r / min for 5-15 min, and after high-speed dispersion, evenly spray them onto the automobile chassis to obtain a lightweight automobile chassis adhesive with good sound insulation effect.

2. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 1, characterized in that: In the step (1), the ratio of castor oil-based polyol, dibutyltin dilaurate catalyst, trimethylolpropane, isophorone diisocyanate, dihydroxyphenylperfluorophthalazinone, and terminal hydroxyl polybutadiene acrylonitrile is 100 g: (4-8) g: (3-5) g: (25-40) g: (1-5) g: (2-10) g.

3. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 1, characterized in that: The filler in step (2) is any one of talcum powder, hollow glass microspheres or light calcium carbonate.

4. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 1, characterized in that: In the step (2), the ratio of asphalt dispersion, liquid rubber-polyurethane emulsion, filler and calcium zinc stabilizer is (40-60) g: (3-15) g: (35-50) g: (1-3) g.

5. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 1, characterized in that: The method for preparing the bishydroxybenzene perfluorophthalazinone in step (1) comprises the following steps: Step S1: under a nitrogen atmosphere, 4-(4-methoxyphenyl)-1-(2H)-phthalazinone and dimethyl sulfoxide were added to a reaction flask, and after stirring, dibromoperfluoro compound and potassium hydroxide were added, and the mixture was stirred for reaction. After the reaction was completed, the mixture was cooled to room temperature, extracted with chloroform and deionized water, and the organic phase was concentrated and dried to obtain bismethoxyphenylperfluorophthalazinone; Step S2: under nitrogen atmosphere, add bis(methoxyphenylperfluorophthalazinone) and dichloromethane into a reaction flask, stir evenly, add boron tribromide, react at 0-20°C for 12-24h, extract with ethyl acetate and deionized water, concentrate the organic phase, and dry to obtain bis(hydroxyphenylperfluorophthalazinone).

6. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 5, characterized in that: The dibrominated perfluoro compound in step S1 is any one of 1,4-dibromooctafluorobutane, 1,6-dibromoperfluorohexane or 1,8-dibromohexafluorooctane.

7. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 5, characterized in that: In the step S1, the ratio of 4-(4-methoxyphenyl)-1-(2H)-phthalazinone, dibromoperfluoro compound and potassium hydroxide is (2.1-2.3) mol: 1 mol: (2.4-3.3) mol.

8. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 5, characterized in that: In step S1, the reaction temperature is 75-90° C. and the reaction time is 3-8 h.

9. The method for preparing a lightweight automobile chassis adhesive with good sound insulation effect according to claim 5, characterized in that: In the step S2, the ratio of bismethoxyphenylperfluorophthalazinone to boron tribromide is 1 mol: (2.5-4) mol.

Citation Information

Patent Citations

  • High quality water-based automotive chassis glue and making method thereof

    CN104098863A

  • Preparation method and epoxidation application of phthalazinone bisphenol monomer

    CN110423223A

  • Phthalazinone diamine monomer and preparation method thereof, polyimide and preparation method thereof, and polyimide film

    CN111233842A