A deep profile control and water plugging material and preparation method thereof
By using epoxidized SiO2 fibers, cross-linked polyaniline and polymeric aluminum chloride in deep dissection modifiers, the glue formation time is extended and the stability is improved, and the problem of excessively fast glue formation of deep dissection modifiers is solved, and the deep dissection modifiers are achieved Improved driving effect and high temperature stability.
Patent Information
- Application Number
- CN202411073140.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The current deep-dead dissection agent is too fast to form glue, resulting in unsatisfactory deep-deaneous dissection effect, difficult to effectively seal the position and the impact surface, and insufficient high-temperature resistance.
Epoxy SiO2 fiber is used as the basic framework, and the glue formation time is extended by cross-linking polyaniline and polymerized aluminum chloride, and structural stability is improved, and a high-temperature resistant deep dissection and water blocking material is formed.
The gel formation is delayed for more than 10 days, ensuring that the driving material is deeply penetrated into the reservoir, and the gel formed can still reach more than 85% of the initial gel formation viscosity in 200 days, and has excellent high temperature stability.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil production, and particularly relates to a deep profile control and water plugging material and a preparation method thereof. Background Art
[0002] In the late stage of oilfield exploitation, most of the remaining oil in the reservoir is stored in the low permeability area. Therefore, it is a key task to improve the water injection sweep efficiency of low permeability reservoirs and to control the profile of low permeability reservoirs. In low permeability reservoirs, the contradiction between the injection performance of profile control agents and their deep profile control technology, and the contradiction between the plugging strength of water channel and the injection performance of profile control agents are prominent. How to achieve deep profile control of oil reservoirs and control the plugging position and sweep surface of profile control agents is very important for stabilizing oil and controlling water in heterogeneous oil fields.
[0003] The deep profile control technology mainly adjusts the vertical and horizontal contradictions in the deep reservoir by using chemical profile control agents to plug the deep part, which can make the injected fluid flow from the high permeability layer with high suction volume to the medium and low permeability layer with low suction volume in the deep formation, so as to expand the sweep coefficient of the deep injected fluid and displace the unswept and unused residual oil formed due to the difference in physical properties of the deep formation. Generally speaking, the action radius of the deep profile control technology needs to be larger, and the high temperature resistance performance of the plugging agent after plugging is high. At the same time, in order to achieve deep profile control, it is necessary to extend the gelling time of the chemical plugging agent. At present, the deep profile control and water plugging materials in the existing technology generally have the problem of too fast gelling speed, and the actual application in the deep profile control process is not ideal. Summary of the invention
[0004] In view of the problem that deep profile control agents in the prior art generally have a gelling speed that is too fast, the present invention provides a deep profile control and water plugging material, which takes epoxidized SiO2 fiber as the basic skeleton and cross-links polyaniline and polyaluminum chloride on its surface. It can not only effectively slow down the gelling rate of the hydrolysis process, prolong the gelling time, and improve the deep profile control performance, but also effectively improve the structural stability inside the profile control agent system.
[0005] A first aspect of the present invention provides a method for preparing a deep profile control and water plugging material, comprising the following steps:
[0006] S1: SiO2 fiber is prepared by electrospinning process, and after spinning, it is modified by 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized SiO2 fiber;
[0007] S2: adding polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence, stirring sufficiently to react, filtering and drying to obtain precursor A;
[0008] S3: Precursor A, epoxidized SiO2 fiber, nitric acid and ammonium persulfate are added to water in sequence, stirred sufficiently for reaction, and then washed, filtered and dried to obtain precursor B;
[0009] S4: Precursor B, urea and deionized water are mixed and stirred, sealed and allowed to stand for aging, and then vacuum dried to obtain a deep profile control and water plugging material.
[0010] Furthermore, in step S1, tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid and ethanol are mixed, stirred for 3 to 4 hours, and then a 10 wt % aqueous solution of polyvinyl pyrrolidone is added to hydrolyze for 8 to 10 hours to obtain a spinning solution, which is then electrospun to prepare SiO2 fibers.
[0011] Furthermore, the mass ratio of tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid and ethanol is 2:1:0.1:10; and the concentration of hydrochloric acid is 1 mol / L.
[0012] Furthermore, the process parameters of electrospinning are: voltage of 10~20KV, perfusion speed of 10~15μL / min, drum speed of 10~50r / min, receiving distance of 10~20cm, slide table speed of 0~50cm / min, and needle inner diameter of 0.2~0.4mm.
[0013] Furthermore, in step S1, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added to perform a reflux reaction, and the epoxidized SiO2 fiber is obtained after separation and drying.
[0014] Among them, the mass ratio of SiO2 fiber, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and toluene is 1:0.5~2:20~30.
[0015] Furthermore, in step S2, the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:(0.5-2):(0.1-0.2):(30-50).
[0016] Furthermore, in step S2, the reaction is carried out in a water bath at 50-80° C. for 6-8 hours.
[0017] Furthermore, in step S3, the mass ratio of precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate is 1:0.5~1.5:0.1~0.2:0.1~0.3; and the concentration of nitric acid is 1 mol / L.
[0018] Furthermore, in step S3, the reaction is carried out in a water bath at 50-80° C. for 10-12 hours.
[0019] Furthermore, in step S4, the mass ratio of precursor B, urea and deionized water is 10:2-5:50; after sealing, the mixture is aged at room temperature for 24-36 hours.
[0020] Among them, urea mainly plays the role of promoting the hydrolysis of aluminum salt, so that polyaluminum chloride is converted into aluminum gel.
[0021] A second aspect of the present invention provides a deep profile control and water plugging material prepared by the above-mentioned method for preparing the deep profile control and water plugging material.
[0022] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0023] 1. The present invention uses epoxidized SiO2 fiber as the basic skeleton, and introduces aniline molecules into the structure of polyaluminum chloride by cross-linking polyaniline and polyaluminum chloride on its surface, so that the nitrogen atoms of polyaniline are connected to the terminal hydroxyl groups between polyaluminum phosphate layers through hydrogen bonds. The two are tightly combined and evenly attached to the epoxidized SiO2 fiber, which can not only effectively slow down the gelation rate of the hydrolysis process, prolong the gelation time, and improve the deep profile control performance, but also effectively improve the structural stability inside the profile control agent system.
[0024] 2. The deep profile control and water plugging material prepared by the present invention can delay gelation for more than 10 days, which can effectively ensure that the profile control and water plugging material penetrates deep into the reservoir and better exerts the deep profile control and water plugging effect. At the same time, the gel formed by the deep profile control and water plugging material provided by the present invention can still reach more than 85% of the initial gelation viscosity after 200 days, and has excellent stability at high temperature. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0026] Example 1
[0027] This embodiment provides a method for preparing a deep profile control and water plugging material, and the specific steps are as follows:
[0028] S1: Tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid, and ethanol were mixed in a mass ratio of 2:1:0.1:10 (hydrochloric acid concentration was 1 mol / L), stirred for 3 h, and then a 10 wt % polyvinyl pyrrolidone aqueous solution was added for hydrolysis for 10 h to obtain a spinning solution, which was then electrospun to prepare SiO2 fibers;
[0029] The process parameters of electrospinning were: voltage 10 KV, perfusion speed 10 μL / min, drum speed 10 r / min, receiving distance 10 cm, slide table speed 10 cm / min, and needle inner diameter 0.2 mm;
[0030] After spinning, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added, and the mass ratio of SiO2 fiber, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and toluene is 1:0.5:20, and then a reflux reaction is carried out, and the epoxidized SiO2 fiber is obtained after separation and drying;
[0031] S2: Add polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence (the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:0.5:0.1:30), stir well, react in a water bath at 50°C for 8h, filter and dry to obtain precursor A;
[0032] S3: Precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate were added to water in a mass ratio of 1:0.5:0.2:0.3 (the concentration of nitric acid was 1 mol / L), stirred thoroughly, and reacted in a water bath at 50°C for 12 h, and then washed, filtered, and dried to obtain precursor B;
[0033] S4: Precursor B, urea and deionized water are mixed in a mass ratio of 5:1:25 and stirred. After sealing, the mixture is allowed to stand for aging at room temperature for 36 hours. The mixture is then vacuum dried to obtain a deep profile control and water plugging material.
[0034] Example 2
[0035] This embodiment provides a method for preparing a deep profile control and water plugging material, and the specific steps are as follows:
[0036] S1: Tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid, and ethanol were mixed in a mass ratio of 2:1:0.1:10 (hydrochloric acid concentration was 1 mol / L), stirred for 4 h, and then a 10 wt% polyvinyl pyrrolidone aqueous solution was added for hydrolysis for 8 h to obtain a spinning solution, which was then electrospun to prepare SiO2 fibers;
[0037] The process parameters of electrospinning were: voltage 20 KV, perfusion speed 10 μL / min, drum speed 20 r / min, receiving distance 20 cm, slide table speed 20 cm / min, and needle inner diameter 0.4 mm;
[0038] After spinning, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added, and the mass ratio of SiO2 fiber, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and toluene is 1:1:30, and a reflux reaction is performed. After separation and drying, the epoxidized SiO2 fiber is obtained;
[0039] S2: Add polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence (the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:1:0.2:50), stir well, react in a water bath at 80°C for 6h, filter and dry to obtain precursor A;
[0040] S3: Precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate were added to water in a mass ratio of 1:1:0.1:0.3 (nitric acid concentration was 1 mol / L), stirred thoroughly, reacted in a water bath at 80°C for 10 h, and then washed, filtered, and dried to obtain precursor B;
[0041] S4: Precursor B, urea and deionized water are mixed in a mass ratio of 2:1:10 and stirred. After sealing, the mixture is allowed to stand for aging at room temperature for 36 hours. The mixture is then vacuum dried to obtain a deep profile control and water plugging material.
[0042] Example 3
[0043] This embodiment provides a method for preparing a deep profile control and water plugging material, and the specific steps are as follows:
[0044] S1: Tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid, and ethanol were mixed in a mass ratio of 2:1:0.1:10 (hydrochloric acid concentration was 1 mol / L), stirred for 3 h, and then a 10 wt % polyvinyl pyrrolidone aqueous solution was added for hydrolysis for 8 h to obtain a spinning solution, which was then electrospun to prepare SiO2 fibers;
[0045] The process parameters of electrospinning were: voltage 10 KV, perfusion speed 15 μL / min, drum speed 30 r / min, receiving distance 20 cm, slide table speed 30 cm / min, and needle inner diameter 0.3 mm;
[0046] After spinning, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added, and the mass ratio of SiO2 fiber, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and toluene is 1:0.5:30, and a reflux reaction is performed. After separation and drying, the epoxidized SiO2 fiber is obtained;
[0047] S2: Add polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence (the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:1:0.2:50), stir well, react in a water bath at 60°C for 8h, filter and dry to obtain precursor A;
[0048] S3: Precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate were added to water in a mass ratio of 1:1.5:0.2:0.3 (the concentration of nitric acid was 1 mol / L), stirred thoroughly, and reacted in a water bath at 80°C for 10 h, and then washed, filtered, and dried to obtain precursor B;
[0049] S4: Precursor B, urea and deionized water are mixed in a mass ratio of 10:3:50 and stirred. After sealing, the mixture is allowed to stand for aging at room temperature for 24 hours, and then vacuum dried to obtain a deep profile control and water plugging material.
[0050] Example 4
[0051] This embodiment provides a method for preparing a deep profile control and water plugging material, and the specific steps are as follows:
[0052] S1: Tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid, and ethanol were mixed in a mass ratio of 2:1:0.1:10 (hydrochloric acid concentration was 1 mol / L), stirred for 4 h, and then a 10 wt% aqueous solution of polyvinyl pyrrolidone was added for hydrolysis for 8-10 h to obtain a spinning solution, which was then electrospun to prepare SiO2 fibers;
[0053] The process parameters of electrospinning were: voltage 20 KV, perfusion speed 15 μL / min, drum speed 50 r / min, receiving distance 20 cm, slide table speed 50 cm / min, and needle inner diameter 0.4 mm;
[0054] After spinning, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added, and the mass ratio of SiO2 fiber, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and toluene is 1:2:30, and a reflux reaction is performed. After separation and drying, the epoxidized SiO2 fiber is obtained;
[0055] S2: Add polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence (the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:2:0.2:50), stir well, react in a water bath at 80°C for 8h, filter and dry to obtain precursor A;
[0056] S3: Precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate were added to water in a mass ratio of 1:1.5:0.1:0.2 (the concentration of nitric acid was 1 mol / L), stirred thoroughly, and reacted in a water bath at 60°C for 12 h, and then washed, filtered, and dried to obtain precursor B;
[0057] S4: Precursor B, urea and deionized water are mixed in a mass ratio of 5:2:25 and stirred. After sealing, the mixture is allowed to stand for aging at room temperature for 30 hours. The mixture is then vacuum dried to obtain a deep profile control and water plugging material.
[0058] Comparative Example 1
[0059] This comparative example provides a method for preparing a deep profile control and water plugging material, and the specific steps are as follows:
[0060] S1: Ultrasonic dispersion of nano-SiO2 (spherical, particle size 70 nm) in toluene solvent, then adding 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, the mass ratio of nano-SiO2, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane and toluene is 1:1:30, and then reflux reaction is carried out, and epoxidized SiO2 is obtained after separation and drying;
[0061] S2: Add polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence (the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:1:0.2:50), stir well, react in a water bath at 80°C for 6h, filter and dry to obtain precursor A;
[0062] S3: Precursor A, epoxidized SiO2, nitric acid, and ammonium persulfate were added to water in a mass ratio of 1:1:0.1:0.3 (nitric acid concentration was 1 mol / L), stirred thoroughly, and reacted in a water bath at 80°C for 10 h, and then washed, filtered, and dried to obtain precursor B;
[0063] S4: Precursor B, urea and deionized water are mixed in a mass ratio of 2:1:10 and stirred. After sealing, the mixture is allowed to stand for aging at room temperature for 36 hours. The mixture is then vacuum dried to obtain a deep profile control and water plugging material.
[0064] Comparative Example 2
[0065] This comparative example provides a method for preparing a deep profile control and water plugging material, and the specific steps are as follows:
[0066] S1: Tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid, and ethanol were mixed in a mass ratio of 2:1:0.1:10 (hydrochloric acid concentration was 1 mol / L), stirred for 4 h, and then a 10 wt% polyvinyl pyrrolidone aqueous solution was added for hydrolysis for 8 h to obtain a spinning solution, which was then electrospun to prepare SiO2 fibers;
[0067] The process parameters of electrospinning were: voltage 20 KV, perfusion speed 10 μL / min, drum speed 20 r / min, receiving distance 20 cm, slide table speed 20 cm / min, and needle inner diameter 0.4 mm;
[0068] After spinning, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added, and the mass ratio of SiO2 fiber, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and toluene is 1:1:30, and a reflux reaction is performed. After separation and drying, the epoxidized SiO2 fiber is obtained;
[0069] S2: Add polyaluminium chloride and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence (the mass ratio of polyaluminium chloride, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:0.2:50), stir well, react in a water bath at 80°C for 6h, filter and dry to obtain precursor A;
[0070] S3: Precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate were added to water in a mass ratio of 1:1:0.1:0.3 (nitric acid concentration was 1 mol / L), stirred thoroughly, reacted in a water bath at 80°C for 10 h, and then washed, filtered, and dried to obtain precursor B;
[0071] S4: Precursor B, urea and deionized water are mixed in a mass ratio of 2:1:10 and stirred. After sealing, the mixture is allowed to stand for aging at room temperature for 36 hours. The mixture is then vacuum dried to obtain a deep profile control and water plugging material.
[0072] Performance Test:
[0073] The deep profile control and water plugging materials prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were subjected to performance tests to test gelling time and stability.
[0074] 1. Put the deep profile control and water plugging material into a high-temperature bottle and place it in a constant temperature water bath at 80℃. Take it out every 24 hours to observe the gel fluidity. The viscosity is measured by Brookfield viscometer. The No. 2 rotor is used during the test at a speed of 6r / min. The experimental results are shown in Table 1:
[0075] Table 1
[0076]
[0077] It can be seen from Table 1 that the deep profile control and water plugging material prepared by the present invention can delay gelation for more than 10 days, which can effectively ensure that the profile control and water plugging material penetrates deep into the reservoir and better exerts the deep profile control and water plugging effect.
[0078] 2. Gel stability: The gels formed by the deep profile control and water plugging materials of Example 2, Comparative Example 1 and Comparative Example 2 (gel viscosity: 13562 mPa·s for Example 2, 11584 mPa·s for Comparative Example 1, and 12688 mPa·s for Comparative Example 2) were placed in a constant temperature oven at 80°C and regularly observed for 200 days. The viscosity was measured using a Brookfield viscometer, with a No. 2 rotor and a rotation speed of 6 r / min. The experimental results are shown in Table 2:
[0079] Table 2
[0080]
[0081] As can be seen from Table 2, the gel formed by the deep profile control and water plugging material provided by the present invention can still reach more than 85% of the initial gelation viscosity after 200 days, while the gel formed by the material in Comparative Example 1 shows a significant decrease in gel viscosity after 50 days, and the gel formed by the material in Comparative Example 2 also shows a significant decrease in gel viscosity after 150 days, indicating that the gel formed by the deep profile control and water plugging material provided by the present invention has excellent stability at high temperature.
Claims
1. A method for preparing a deep profile control and water plugging material, characterized in that: The following steps are involved: S1: SiO2 fiber is prepared by electrospinning process, and after spinning, it is modified by 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized SiO2 fiber; S2: adding polyaluminium chloride, aniline and sodium dodecylbenzene sulfonate to polyvinyl alcohol solvent in sequence, stirring sufficiently to react, filtering and drying to obtain precursor A; S3: Precursor A, epoxidized SiO2 fiber, nitric acid and ammonium persulfate are added to water in sequence, stirred sufficiently for reaction, and then washed, filtered and dried to obtain precursor B; S4: Precursor B, urea and deionized water are mixed and stirred, sealed and allowed to stand for aging, and then vacuum dried to obtain a deep profile control and water plugging material; In step S1, tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid and ethanol are mixed, stirred for 3-4 hours, and then a 10 wt % polyvinyl pyrrolidone aqueous solution is added for hydrolysis for 8-10 hours to obtain a spinning solution, which is then electrospun to prepare SiO2 fibers; The mass ratio of tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, hydrochloric acid, and ethanol is 2:1:0.1:10; In step S1, the SiO2 fiber is ultrasonically dispersed in a toluene solvent, and then 3-(2,3-epoxypropoxy)propyltrimethoxysilane is added to perform a reflux reaction, and then the epoxy SiO2 fiber is obtained after separation and drying; The mass ratio of SiO2 fiber, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, and toluene is 1:0.5~2:20~30; In step S2, the mass ratio of polyaluminium chloride, aniline, sodium dodecylbenzene sulfonate and polyvinyl alcohol is 1:0.5-2:0.1-0.2:30-50; In step S3, the mass ratio of precursor A, epoxidized SiO2 fiber, nitric acid, and ammonium persulfate is 1:0.5~1.5:0.1~0.2:0.1~0.3; In step S4, the mass ratio of precursor B, urea and deionized water is 10:2-5:
50.
2. The method for preparing the deep profile control and water plugging material according to claim 1, characterized in that: The process parameters of electrospinning are: voltage of 10~20KV, perfusion speed of 10~15μL / min, drum speed of 10~50r / min, receiving distance of 10~20cm, slide table speed of 0~50cm / min, and needle inner diameter of 0.2~0.4mm.
3. The method for preparing the deep profile control and water plugging material according to claim 1, characterized in that: In step S2, the reaction is carried out in a water bath at 50-80° C. for 6-8 hours.
4. The method for preparing the deep profile control and water plugging material according to claim 1, characterized in that: In step S3, the reaction is carried out in a water bath at 50-80° C. for 10-12 hours.
5. The method for preparing the deep profile control and water plugging material according to claim 1, characterized in that: In step S4, after sealing, the mixture is aged at room temperature for 24 to 36 hours.
6. The deep profile control and water plugging material prepared by the preparation method of the deep profile control and water plugging material according to any one of claims 1 to 5.
Citation Information
Patent Citations
Fiber composite hydraulic fracturing fluid for shale volume fracturing
CN103602330A
High-strength selective water-plugging profile-modifying agent for low-permeability reservoir and preparation method thereof