A negative electrode composite material and preparation method thereof, dry negative electrode sheet and lithium battery
By coating the surface of the active material of the dry-process negative electrode with an inorganic protective layer, the problem of surface defects of the active material during the preparation of the dry negative electrode is solved, thereby improving the first discharge efficiency and cycle performance of the lithium battery.
Patent Information
- Application Number
- CN202411070132.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
During the preparation of dry anodes, the morphology and particle surface structure of the anode active material are damaged by collisions, resulting in surface defects that affect the first discharge efficiency and cycle life of lithium batteries.
An inorganic coating layer with a thickness of 0.5~50 nm and a Young's modulus of 20 GPa or more is coated on the surface of the negative electrode active material. The coating layer contains metal oxides, lithium-containing solid electrolyte compounds, lithium-containing inorganic bases or inorganic lithium salts, and is formed by liquid phase or gas phase deposition.
It protects the negative electrode active material, avoids defects in the preparation process, improves the first discharge efficiency and cycle performance of lithium batteries, and enhances the mechanical stability and cycle life of batteries.
Smart Images

Figure CN118588940B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of batteries, and in particular, to a negative electrode composite material and a preparation method thereof, a dry-process negative electrode sheet and a lithium battery. Background Art
[0002] With the rapid development of the new energy vehicle industry, the current battery production process can no longer meet the needs of new energy vehicles. Production issues such as speed, safety, and environmental protection have once again become the focus of industry attention. Dry electrode technology is to mix the dry powder of active material with the corresponding conductive agent and binder, and to prepare the powder directly into an electrode film by fiberizing the binder through air flow milling, and then to compound the electrode film with the current collector to prepare the required dry electrode. The dry electrode process does not require the addition of various solvents, which reduces the complexity of the process and improves the environmental protection and safety characteristics of the electrode sheet preparation process; reduces the preparation of electrode slurry and the coating process of electrode sheets, greatly improves production efficiency and reduces production costs. In addition, dry electrode technology can prepare thick electrode systems that cannot be completed by traditional wet coating processes, providing technical support for the design and development of energy-density batteries. Therefore, dry electrode technology has become one of the future trends in the battery industry.
[0003] However, the current dry-process negative electrode still has the following problems: On the one hand, the negative electrode active material is usually a soft carbon material or silicon-based material. During the process of mixing with the binder dry powder for fiberization, the morphology of the negative electrode active material and the surface structure of the particles are destroyed due to the collision in the air flow mill, causing a large number of defects on the surface of the negative electrode active material. Compared with the wet-process negative electrode, the dry-process negative electrode process is complicated, and the surface defects of the negative electrode active material are exposed to the electrolyte, resulting in an increase in the irreversible consumption of active lithium during the formation process, which reduces the first discharge efficiency of the battery. In addition, defects will also increase the consumption of electrolyte during the cycle and shorten the cycle life of the battery.
[0004] One way to solve the above problems is to add film-forming additives to the electrolyte to improve SEI film formation during the formation process. However, this method will increase the thickness of the SEI film and cannot avoid the consumption of active lithium. At the same time, the defects on the surface of the negative electrode active material particles caused by the fibrillation of the binder are not uniform. The SEI film formed in the area with denser defect distribution is thick, while the SEI film formed in the non-defective area is thin. The large difference in SEI film thickness leads to inconsistent lithium ion conduction rate, resulting in local polarization and performance degradation, which in turn affects the performance of the entire electrode and battery cell. Summary of the invention
[0005] The purpose of the present disclosure is to provide a negative electrode composite material and a preparation method thereof, a dry-process negative electrode plate and a lithium battery. The negative electrode composite material can protect the negative electrode active material, avoid defects in the negative electrode active material during the binder fiberization process, and thus improve the initial discharge efficiency and cycle performance of the lithium battery; at the same time, it can alleviate the surface damage to the negative electrode active material during the hot pressing composite process of the dry-process negative electrode film and the current collector, thereby increasing the cycle performance of the battery.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a negative electrode composite material, which includes a negative electrode active material and an inorganic coating layer coated on the surface of the negative electrode active material, and the thickness of the inorganic coating layer is 0.5~50nm; the Young's modulus of the negative electrode composite material is above 20GPa.
[0007] Optionally, the Young's modulus of the negative electrode composite material is 20-450 GPa; and the thickness of the inorganic coating layer is 5-30 nm.
[0008] Optionally, the D50 particle size of the negative electrode composite material is 0.1-50 μm.
[0009] Optionally, the inorganic coating layer comprises one or more of a metal oxide, a lithium-containing solid electrolyte compound, a lithium-containing inorganic base and an inorganic lithium salt;
[0010] The metal element of the metal oxide is selected from one or more of Group IA, Group IIIA, Group IVA, Group IIB and Group IVB metal elements;
[0011] The lithium-containing solid electrolyte compound is selected from doped or undoped lithium lanthanum zirconium oxide compounds, and the doping element is selected from one or more metal elements of Group IIIA, Group IVB and Group VB.
[0012] Optionally, the metal oxide is selected from one or more of titanium oxide, aluminum oxide, sodium oxide, zinc oxide, tin oxide, indium oxide and zirconium oxide;
[0013] The lithium-containing solid electrolyte compound is selected from one or more of lithium lanthanum zirconium oxide compounds, lithium lanthanum zirconium titanium oxides, lithium lanthanum zirconium tantalum oxides, lithium lanthanum zirconium aluminum oxides and lithium lanthanum zirconium niobium oxides;
[0014] The lithium-containing inorganic base is selected from lithium hydroxide;
[0015] The inorganic lithium salt is selected from one or more of lithium aluminate, lithium metaphosphate, lithium phosphate, lithium iron phosphate, lithium manganese phosphate, lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium carbonate, lithium sulfate, lithium sulfite, lithium hypochlorite, lithium fluoride, lithium iodide, lithium selenide, lithium indium, lithium nitride, lithium sulfide and lithium phosphide.
[0016] Optionally, the inorganic coating layer further comprises a dispersant, and the dispersant is selected from one or more of carboxymethyl cellulose, polyacrylic acid, polymethyl methacrylate and polyvinyl pyrrolidone;
[0017] The mass ratio of the dispersant to the inorganic material is (0.1~1):1.
[0018] The second aspect of the present disclosure provides a method for preparing the negative electrode composite material described in the first aspect of the present disclosure, the method comprising: allowing particles containing inorganic matter to form an inorganic coating layer on the surface of the negative electrode active material; wherein the Young's modulus of the particles containing inorganic matter is greater than 20 GPa.
[0019] Optionally, the method for forming the inorganic coating layer is selected from one or more of liquid phase mixing solidification method, solid phase mixing depolymerization method, liquid phase deposition method, chemical vapor deposition method, liquid phase spray drying method, vapor phase spray deposition method, ion exchange method, atomic layer deposition method, sol-gel method and magnetron sputtering method.
[0020] Optionally, a dispersant is added when forming the inorganic coating layer, and the dispersant is selected from one or more of carboxymethyl cellulose, polyacrylic acid, polymethyl methacrylate and polyvinyl pyrrolidone.
[0021] The third aspect of the present disclosure provides a dry-process negative electrode plate, which includes a current collector and a negative electrode material layer arranged on at least one surface of the current collector; the negative electrode material layer includes the negative electrode composite material described in the first aspect of the present disclosure, a conductive agent and a fibrous binder, wherein at least a portion of the negative electrode composite material is dispersed in the fibrous binder.
[0022] Optionally, the thickness of the negative electrode material layer is 30-200 μm;
[0023] In the negative electrode material layer, with respect to 80 to 100 parts by mass of the negative electrode composite material, the mass fraction of the binder is 19 or less, and the mass fraction of the conductive agent is 1 or less.
[0024] A fourth aspect of the present disclosure provides a lithium battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; wherein the negative electrode sheet is the dry-process negative electrode sheet described in the third aspect of the present disclosure.
[0025] Through the above technical scheme, the present disclosure provides a negative electrode composite material, which includes a negative electrode active material and an inorganic coating layer coated on the surface of the negative electrode active material. The thickness of the inorganic coating layer is in the range of 0.5~50nm, which can protect the negative electrode active material and avoid the negative electrode active material from generating defects during the binder fiberization process, thereby improving the first discharge efficiency and cycle performance of the lithium battery; at the same time, the Young's modulus of the negative electrode composite material is above 20Gpa, and it has good mechanical stability, which can alleviate the surface damage of the negative electrode active material during the hot pressing composite process of the dry negative electrode film and the current collector, thereby increasing the cycle performance of the battery.
[0026] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0028] Figure 1 This is a SEM image of the dry-process negative electrode material layer obtained in Example 1 of the present disclosure. DETAILED DESCRIPTION
[0029] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0030] The first aspect of the present disclosure provides a negative electrode composite material, which includes a negative electrode active material and an inorganic coating layer coated on the surface of the negative electrode active material, wherein the thickness of the inorganic coating layer is 0.5~50nm; and the Young's modulus of the negative electrode composite material is greater than 20GPa.
[0031] The negative electrode composite material disclosed in the present invention comprises a negative electrode active material and an inorganic coating layer coated on the surface of the negative electrode active material. The thickness of the inorganic coating layer is in the range of 0.5 to 50 nm, which can protect the negative electrode active material and prevent the negative electrode active material from generating defects during the binder fiberization process, thereby improving the initial discharge efficiency and cycle performance of the lithium battery; at the same time, the Young's modulus of the negative electrode composite material is above 20 Gpa, and it has good mechanical stability, which can alleviate the surface damage of the negative electrode active material during the hot pressing composite process of the dry-process negative electrode film and the current collector, thereby increasing the cycle performance of the battery.
[0032] In the present disclosure, an ultrasonic method can be used to test the Young's modulus of the negative electrode composite material. The testing method includes, for example: crushing the negative electrode composite material, pressing the obtained powder into a sample in a mold, sintering the sample under an inert atmosphere, and then leveling the surface to obtain a sample to be determined, and using an ultrasonic pulse method to test the Young's modulus of the sample to be determined, as the Young's modulus of the negative electrode composite material.
[0033] Specifically, the test method of the Young's modulus of the negative electrode composite material is as follows: the negative electrode composite material test sample is crushed into fine powder using a mortar or grinder, and the D50 particle size of the fine powder is 0.1~100μm. Use a mold to press the test sample powder into a specimen of regular shape. Ensure that the inner wall of the mold is smooth to reduce friction and stress concentration. The specimen pressed into a regular shape is sintered, and the sintering treatment is carried out under an inert atmosphere. The sintering temperature and time are determined according to the properties of the sample, usually between 600°C and 1200°C, and the sintering time is 1-6 hours. The temperature should be slowly raised and lowered during the sintering process to avoid cracking or deformation of the sample. The sintered sample is slowly cooled to room temperature. Carefully remove the sintered sample from the mold to ensure that there are no cracks on the surface of the sintered sample. Use sandpaper or a polishing machine to grind and polish the surface of the sintered sample to make its surface smooth and flat to obtain a pending sample. Use precision measuring tools (such as a vernier caliper or micrometer) to measure the geometric dimensions (length, width, height or diameter) of the sample to be determined. Record the dimensional data for subsequent calculation and analysis. Install the sample to be determined in the ultrasonic pulse test device to ensure good contact between the sample to be determined and the test device. Send ultrasonic pulse: Start the ultrasonic pulse generator to send an ultrasonic pulse to the sample to be determined. Receive ultrasonic echo: Use an ultrasonic transducer to receive the echo of the ultrasonic pulse in the sample to be determined and convert it into an electrical signal. Process and analyze the received electrical signal to obtain the Young's modulus of the sample to be determined, which is the Young's modulus of the negative electrode composite material.
[0034] According to an embodiment of the present disclosure, the Young's modulus of the negative electrode composite material is 20-450 GPa, and the thickness of the inorganic coating layer is 5-30 nm. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0035] According to an embodiment of the present disclosure, the D50 particle size of the negative electrode composite material is 0.1-50 μm, preferably 5-40 μm. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0036] According to one embodiment of the present disclosure, the inorganic coating layer comprises one or more of metal oxides, lithium-containing solid electrolyte compounds, lithium-containing inorganic bases and inorganic lithium salts; the metal element of the metal oxide can be selected from one or more of Group IA, Group IIIA, Group IVA, Group IIB and Group IVB metal elements; in a further embodiment, the metal element of Group IA can be selected from sodium; the metal element of Group IIIA can be selected from aluminum and / or indium; the metal element of Group IVA can be selected from tin; the metal element of Group IIB can be selected from zinc; the metal element of Group IVB titanium and / or zirconium. The lithium-containing solid electrolyte compound is selected from doped or undoped lithium lanthanum zirconium oxide compounds, and the doping element can be selected from one or more of Group IIIA, Group IVB and Group VB metal elements; in a further embodiment, the doping element can be selected from aluminum in Group IIIA, titanium in Group IVB, niobium and / or tantalum in Group VB. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0037] According to an embodiment of the present disclosure, the metal oxide can be selected from one or more of titanium oxide, aluminum oxide, sodium oxide, zinc oxide, tin oxide, indium oxide and zirconium oxide. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0038] According to an embodiment of the present disclosure, the lithium-containing solid electrolyte compound is selected from one or more of lithium lanthanum zirconium oxide (LLZO), lithium lanthanum zirconium titanium oxide (LLZTO), lithium lanthanum zirconium tantalum oxide, lithium lanthanum zirconium aluminum oxide and lithium lanthanum zirconium niobium oxide. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0039] According to an embodiment of the present disclosure, the lithium-containing inorganic base is selected from lithium hydroxide. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0040] According to an embodiment of the present disclosure, the inorganic lithium salt is selected from one or more of lithium metaaluminate, lithium metaphosphate, lithium phosphate, lithium iron phosphate, lithium manganese phosphate, lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate, lithium carbonate, lithium sulfate, lithium sulfite, lithium hypochlorite, lithium fluoride, lithium iodide, lithium selenide, lithium indium, lithium nitride, lithium sulfide and lithium phosphide. The above embodiment is conducive to improving the first discharge efficiency and rate performance of the battery and improving the cycle life of the battery.
[0041] According to an embodiment of the present disclosure, the inorganic coating layer further includes a dispersant, and the dispersant is selected from one or more of carboxymethyl cellulose, polyacrylic acid, polymethyl methacrylate and polyvinyl pyrrolidone. The above embodiment is conducive to uniformly dispersing the inorganic material on the surface of the negative electrode active material, and is conducive to obtaining an inorganic coating layer with uniform thickness, which effectively alleviates the problem of local charge and discharge polarization caused by inconsistent SEI thickness during the formation process, thereby increasing the cycle stability of the negative electrode sheet.
[0042] According to an embodiment of the present disclosure, the mass ratio of the dispersant to the inorganic material is (0.1-1):1, preferably (0.3-0.6):1. The above embodiment is conducive to uniformly dispersing the inorganic material on the surface of the negative electrode active material and obtaining an inorganic coating layer with uniform thickness.
[0043] According to an embodiment of the present disclosure, the water contact angle θ of the negative electrode composite material is greater than 60°, preferably 80° to 150°. The above embodiment is conducive to improving the water absorption of the surface of the negative electrode composite material and further improving the cycle life of the battery.
[0044] The second aspect of the present disclosure provides a method for preparing the negative electrode composite material described in the first aspect of the present disclosure, the method comprising: allowing particles containing inorganic matter to form an inorganic coating layer on the surface of the negative electrode active material; wherein the Young's modulus of the particles containing inorganic matter is greater than 20 GPa.
[0045] According to one embodiment of the present disclosure, the method for forming the inorganic coating layer is selected from one or more of liquid phase mixing solidification method, solid phase mixing depolymerization method, liquid phase deposition method, chemical vapor deposition method, liquid phase spray drying method, vapor phase spray deposition method, ion exchange method, atomic layer deposition method, sol-gel method and magnetron sputtering method.
[0046] According to one embodiment of the present disclosure, the formation of the inorganic coating layer also includes adding a dispersant to the system containing the negative electrode active material and the inorganic material, and the dispersant is selected from one or more of carboxymethyl cellulose, polyacrylic acid, polymethyl methacrylate and polyvinyl pyrrolidone. In one embodiment, the dispersant used has a certain Young's modulus, which can increase the Young's modulus of the raw material of the inorganic coating layer and further increase the Young's modulus of the negative electrode composite material. The above embodiment is conducive to uniformly dispersing the inorganic material on the surface of the negative electrode active material, and is conducive to obtaining an inorganic coating layer with uniform thickness, which effectively alleviates the problem of local charge and discharge polarization caused by inconsistent SEI thickness during the formation process, thereby increasing the cycle stability of the negative electrode sheet.
[0047] According to an embodiment of the present disclosure, the mass ratio of the dispersant to the inorganic material is (0.1-1):1, preferably (0.3-0.6):1. The above embodiment is conducive to uniformly dispersing the inorganic material on the surface of the negative electrode active material, and is conducive to obtaining an inorganic coating layer with uniform thickness, which effectively alleviates the problem of local charge and discharge polarization caused by inconsistent SEI thickness during the formation process, thereby increasing the cycle stability of the negative electrode sheet.
[0048] According to one embodiment of the present disclosure, the negative electrode active material may be a conventional negative electrode active material in the art, and the present disclosure does not specifically limit this. For example, the negative electrode active material may be selected from one or more of graphite, silicon carbon and hard carbon materials.
[0049] According to one embodiment of the present disclosure, when preparing a composite material for a dry-process negative electrode, a dispersing solvent may be used for inorganic materials that are unstable in aqueous solution. For example, the dispersing solvent may be a suitable organic solvent such as N-methylpyrrolidone, tetrahydrofuran, ethanol or ethylene carbonate (EC).
[0050] The present disclosure provides a method for preparing a dry-process negative electrode sheet, the method comprising: mixing a negative electrode composite material, a conductive agent and a binder to obtain a mixture, performing a fiberization process and a calendering process on the mixture to obtain a negative electrode material layer; and then compounding the negative electrode material layer with a current collector;
[0051] Wherein, the negative electrode composite material is the negative electrode composite material described in the first aspect of the present disclosure.
[0052] The present invention prepares negative electrode sheets from negative electrode composite materials by dry method, which can avoid the inorganic coating layer of the negative electrode composite material from failing due to water absorption characteristics, or causing the inorganic coating layer to fail due to reaction with water, and avoid the negative electrode composite material from failing and being unable to protect the negative electrode active material. The inorganic coating layer can effectively protect the negative electrode active material through dry method preparation, thereby improving the first discharge efficiency and rate performance of the battery, and improving the cycle life of the battery.
[0053] According to one embodiment of the present disclosure, relative to 80 to 100 parts by mass of the negative electrode composite material, the mass fraction of the binder is 19 or less, and the mass fraction of the conductive agent is 1 or less. In the present disclosure, the binder and the conductive agent are not 0, and can be any value greater than 0, for example, 0.01. The conductive agent can be a conventional conductive agent in the art, for example, it can be one or more of carbon black, carbon nanotubes (CNT), acetylene black and graphene; the binder is a fiberizable compound; preferably, the binder is selected from one or more of polypropylene, polytetrafluoroethylene (PTFE) and styrene-butadiene rubber (SBR).
[0054] According to an embodiment of the present disclosure, the fiberization treatment is a conventional binder fiberization treatment process in the art, which can be processed by a jet mill; the calendering treatment can be a conventional operation in the art, such as preparing a self-supporting film from the fiberized mixed powder by powder extrusion molding or powder roller molding. The above embodiment makes the contact between the conductive agent and the negative electrode composite material closer, so that lithium ions can be better embedded and released on the surface of the negative electrode composite material, thereby improving the conductivity of the electrode and the rate performance of the battery.
[0055] The third aspect of the present disclosure provides a dry-process negative electrode sheet, the dry-process negative electrode sheet comprising a current collector and a negative electrode material layer disposed on at least one surface of the current collector; the negative electrode material layer comprises the negative electrode composite material of the first aspect of the present disclosure, a conductive agent and a fibrous binder, wherein at least part of the negative electrode composite material is dispersed in the fibrous binder. Figure 1 As shown, a large amount of fibrous binder exists in the cross section of the dry-process negative electrode sheet under a SEM electron microscope, and at least part of the negative electrode composite material is dispersed in the fibrous binder.
[0056] According to an embodiment of the present disclosure, the thickness of the negative electrode material layer is 30-200 μm. The above embodiment can improve the battery performance and improve the battery life.
[0057] According to one embodiment of the present disclosure, in the negative electrode material layer, relative to 80 to 100 parts by mass of the negative electrode composite material, the mass fraction of the binder is 19 or less, and the mass fraction of the conductive agent is 1 or less. In the present disclosure, the mass ratio of the negative electrode composite material, the binder and the conductive agent can be calculated by the feed ratio when preparing the dry negative electrode sheet. In the present disclosure, the binder and the conductive agent are not 0, and can be any value greater than 0, for example, 0.01.
[0058] According to one embodiment of the present disclosure, the negative electrode material layer may be disposed on one surface or both surfaces of the current collector.
[0059] A fourth aspect of the present disclosure provides a lithium battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; wherein the negative electrode sheet is the dry-process negative electrode sheet described in the third aspect of the present disclosure.
[0060] According to one embodiment of the present disclosure, the positive electrode plate includes a current collector and a positive electrode active material layer disposed on the current collector; the positive electrode active material layer can be disposed on one surface or both surfaces of the current collector. In one embodiment, the positive electrode plate can be prepared by a wet method. In another embodiment, the positive electrode active material layer can also be prepared by a dry method. The positive electrode active material layer includes a positive electrode active substance. The present disclosure does not specifically limit the positive electrode active substance, and it can be a conventional positive electrode active substance in the art. For example, the positive electrode active substance material includes but is not limited to LiFe x Mn 1-x PO4, LiFePO4, LiCoO2, LiMn2O4, LiNi x Co y Mn z O2 (x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1), LiNi x Co y Al z O2 (x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1).
[0061] According to one embodiment of the present disclosure, the electrolyte is a non-aqueous solvent, which may be a conventional electrolyte in the art, for example, including but not limited to ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethyl carbonate, and butylene carbonate.
[0062] The battery disclosed in the present invention can be assembled by conventional methods in the art. For example, the battery includes a positive electrode, a negative electrode, an electrolyte, a separator and structural parts, and is manufactured according to a conventional manufacturing process.
[0063] The present disclosure is further described in detail by way of examples. Unless otherwise specified, the remaining raw materials can be obtained through commercial sources.
[0064] Atomic layer deposition was performed on an Atomfab instrument; spray drying was performed on a Preci P series spray drying equipment;
[0065] The thickness of the inorganic coating layer was tested on a ThermoFisher Talos F200X transmission electron microscope;
[0066] The D50 particle size of the negative electrode composite material was tested on a Malvern 3000 particle size analyzer.
[0067] The contact angle of the negative electrode composite material was tested on a contact angle meter model SDC-200S.
[0068] The following preparation example is used to prepare a negative electrode composite material for a dry-process negative electrode.
[0069] Preparation Example 1
[0070] The specific preparation method is: mixing graphite powder and water in a mass ratio of 1:5 and stirring to form a uniform slurry; adding LiOH crystals to the slurry, the mass ratio of graphite powder to LiOH crystals is 100:1; spray drying the slurry in which LiOH is dissolved, the spray drying temperature is 100°C, and a negative electrode composite material S1 coated with LiOH is obtained, S1 is graphite with a LiOH coating layer, the thickness of the coating layer is 7nm, and the Young's modulus of the negative electrode composite material S1 is 20GPa.
[0071] Preparation Example 2
[0072] The specific preparation method is: mix graphite powder and water in a mass ratio of 1:5 and stir to form a uniform slurry; add Li2CO3 crystals to the slurry, and the mass ratio of graphite powder to Li2CO3 crystals is 100:1; spray dry the slurry in which Li2CO3 is dissolved, and the spray drying temperature is 100°C to obtain a negative electrode composite material S2 coated with Li2CO3, S2 is graphite with a Li2CO3 coating layer, the thickness of the coating layer is 10nm, and the Young's modulus of the negative electrode composite material S2 is 40GPa.
[0073] Preparation Example 3
[0074] The specific preparation method is as follows: under stirring, add 100g of graphite powder to 130g of 5% lithium acetate aqueous solution, and continue to stir the mixed solution for 1h until the graphite is evenly dispersed to obtain a first mixed solution. Add 67g of 5% ammonium fluoride aqueous solution dropwise to the first mixed solution, stir for 30 min until the reaction is complete, and obtain a second mixed solution. The second mixed solution is spray-dried on a spray drying device at an exhaust temperature of 100°C; the negative electrode composite material S3 is obtained, S3 is graphite with a LiF coating layer, the coating layer thickness is 10nm, and the Young's modulus of the negative electrode composite material S3 is 80GPa.
[0075] Preparation Example 4
[0076] 100g of graphite and 1g of lithium lanthanum zirconium oxide (chemical formula: LiLaZrO4) were evenly dispersed in an aqueous solution, deionized water was added to adjust the suspension to a solid content of 20%, and the negative electrode composite material S4 was obtained by spray drying. The spray drying temperature was 100°C. S4 was graphite with a lithium lanthanum zirconium oxide coating layer. The thickness of the coating layer was 10nm, and the Young's modulus of the negative electrode composite material S4 was 150GPa.
[0077] Preparation Example 5
[0078] Dissolve 1g of carboxymethyl cellulose CMC dispersant in 110g of deionized water solution, and continue stirring until it is evenly dissolved to obtain a first mixed solution; evenly disperse 100g of graphite and 1g of lithium lanthanum zirconium oxide (chemical formula: LiLaZrO4) in the first mixed solution, add deionized water to adjust the suspension to a solid content of 50%, and obtain the negative electrode composite material S5 by spray drying. The spray drying temperature is 100°C. S5 is graphite with a lithium lanthanum zirconium oxide / CMC coating layer. The thickness of the coating layer is 10nm, and the Young's modulus of the negative electrode composite material S5 is 200GPa.
[0079] Preparation Example 6
[0080] The specific preparation method is as follows: the precursors use trimethylaluminum (Al(CH3)3) and deionized water as Al source and O source respectively, the two precursors are stored at 20°C, and high-purity Ar is used as the carrier gas; the order of atomic layer deposition is 0.15s water → 5s high-purity Ar → 0.15s trimethylaluminum → 1s high-purity Ar, and the deposition temperature is 100°C; the negative electrode composite material S6 is obtained, S6 is graphite with an Al2O3 coating layer, the thickness of the coating layer is 30nm, and the Young's modulus of the negative electrode composite material S6 is 430GPa.
[0081] Preparation Example 7
[0082] The specific preparation method is as follows: under stirring, add 100g of graphite powder to 100g of 0.1% lithium acetate aqueous solution, and continue stirring the mixed solution for 1h until the graphite is evenly dispersed to obtain a first mixed solution. Add 100g of 0.1% ammonium fluoride aqueous solution dropwise to the first mixed solution, stir for 30 min until the reaction is complete, and obtain a second mixed solution. Spray dry the second mixed solution on a spray drying device at an exhaust temperature of 100°C to obtain the negative electrode composite material S7, which is graphite with a LiF coating layer, the coating layer thickness is 1nm, and the Young's modulus of the negative electrode composite material S7 is 80GPa.
[0083] Preparation Example 8
[0084] The specific preparation method is as follows: under stirring, add 100g of graphite powder to 100g of 5% lithium acetate aqueous solution, and continue stirring the mixed solution for 1h until the graphite is evenly dispersed to obtain a first mixed solution. Add 100g of 5% ammonium fluoride aqueous solution dropwise to the first mixed solution, stir for 30 min until the reaction is complete, and obtain a second mixed solution. Spray dry the second mixed solution on a spray drying device at an exhaust temperature of 100°C to obtain the negative electrode composite material S8, which is graphite with a LiF coating layer, the coating layer thickness is 50nm, and the Young's modulus of the negative electrode composite material S8 is 80GPa.
[0085] Preparation Example 9
[0086] The specific preparation method is as follows: dissolve 0.2 g of carboxymethyl cellulose CMC dispersant in 110 g of deionized water solution, and continue stirring until dissolved evenly to obtain a first mixed solution; add 101 g of LiOH crystals and graphite powder to the first mixed solution, and disperse evenly to obtain a second mixed solution, wherein the mass ratio of graphite powder to LiOH crystals is 100:1; spray dry the second mixed solution at a spray drying temperature of 100°C to obtain a negative electrode composite material S9 coated with LiOH / CMC, wherein S9 is graphite with a LiOH / CMC coating layer, the thickness of the coating layer is 11 nm, and the Young's modulus of the negative electrode composite material S9 is 22 GPa.
[0087] Preparation Example 10
[0088] The specific preparation method is as follows: dissolve 1 g of carboxymethyl cellulose CMC dispersant in 110 g of deionized water solution, and continue stirring until dissolved evenly to obtain a first mixed solution; add 101 g of LiOH crystals and graphite powder to the first mixed solution, and disperse evenly to obtain a second mixed solution, wherein the mass ratio of graphite powder to LiOH crystals is 100:1; spray dry the second mixed solution at a spray drying temperature of 100°C to obtain a negative electrode composite material S10 coated with LiOH / CMC, wherein S10 is graphite with a LiOH / CMC coating layer, the thickness of the coating layer is 15 nm, and the Young's modulus of the negative electrode composite material S10 is 20 GPa.
[0089] Preparation Example 11
[0090] The specific preparation method is as follows: dissolve 0.2 g of carboxymethyl cellulose CMC dispersant in 110 g of deionized water solution, and continue stirring until dissolved evenly to obtain a first mixed solution; add 101 g of silicon carbide crystals (SiC) and graphite powder to the first mixed solution, and disperse evenly to obtain a second dispersed mixed solution, wherein the mass ratio of graphite powder to silicon carbide crystals (SiC) is 100:1; spray dry the second mixed solution at a spray drying temperature of 100°C to obtain a negative electrode composite material S11 coated with SiC / CMC, wherein S11 is graphite with a SiC / CMC coating layer, the thickness of the coating layer is 40 nm, and the Young's modulus of the negative electrode composite material S11 is 500 GPa.
[0091] Preparation Example 12
[0092] The specific preparation method is: mix graphite powder, LiFePO4, NMP, and PVDF in a mass ratio of 100:2:70:1 to obtain a mixed solution of LiFePO4 and graphite; spray dry on a spray drying equipment at an exhaust air temperature of 220°C to obtain the negative electrode composite material S12, which is graphite with a LiFePO4 coating layer, the coating layer has a thickness of 50nm, and the Young's modulus of the negative electrode composite material S12 is 15GPa.
[0093] Preparation Example 13
[0094] The specific preparation method is: mix graphite powder, LiMnPO4, NMP, and PVDF in a mass ratio of 100:2:70:1 to obtain a mixed solution of LiMnPO4 and graphite; spray dry on a spray drying equipment at an exhaust air temperature of 220°C to obtain the negative electrode composite material S13, S13 is graphite with a LiMnPO4 coating layer, the coating layer has a thickness of 60nm, and the Young's modulus of the negative electrode composite material S13 is 12GPa.
[0095] Preparation Example 14
[0096] The specific preparation method is as follows: under stirring, add 100g of graphite powder to 100g of 0.02% lithium acetate aqueous solution, and continue stirring the mixed solution for 1h until the graphite is evenly dispersed to obtain a first mixed solution. Add 100g of 0.02% ammonium fluoride aqueous solution dropwise to the first mixed solution, stir for 30 min until the reaction is complete, and obtain a second mixed solution. Spray dry the second mixed solution on a spray drying device at an exhaust temperature of 100°C; obtain the negative electrode composite material S14, which is graphite with a LiF coating layer, the coating layer thickness is 0.3nm, and the Young's modulus of the negative electrode composite material S14 is 80GPa.
[0097] Preparation Example 15
[0098] The specific preparation method is as follows: under stirring, add 100g of graphite powder to 110g of 5% lithium acetate aqueous solution, and continue stirring the mixed solution for 1h until the graphite is evenly dispersed to obtain a first mixed solution. Add 110g of 5% ammonium fluoride aqueous solution dropwise to the first mixed solution, stir for 30 min until the reaction is complete, and obtain a second mixed solution. The second mixed solution is spray-dried on a spray drying device at an exhaust temperature of 100°C; the negative electrode composite material S15 is obtained, S15 is graphite with a LiF coating layer, the coating layer thickness is 60nm, and the Young's modulus of the negative electrode composite material S15 is 80GPa.
[0099] The following examples and comparative examples are used to prepare laminated batteries.
[0100] Example 1
[0101] The negative electrode composite material S1 obtained in Preparation Example 1 was used to prepare a dry-process negative electrode for a lithium-ion battery by a dry process. The preparation method is as follows:
[0102] (1) The negative electrode composite material S1, the conductive agent (Super-P-Li), and the binder (PTFE) are mixed in a mass ratio of 97:1:2, and the PTFE is fiberized by a jet mill to obtain a mixed powder. The mixed powder is calendered by a calender to obtain a dry-process negative electrode material layer with a thickness of 150 μm, and then the dry-process negative electrode material layer is composited with a current collector copper foil to obtain a dry-process negative electrode sheet for a lithium-ion battery;
[0103] (2) After mixing the positive electrode active material lithium iron phosphate (LiFePO4), the conductive agent (CNT), and the binder (PVDF) in a mass ratio of 97:1:2, the powder and NMP are stirred into a positive electrode slurry in a homogenizer and evenly coated on an aluminum foil;
[0104] Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 1:1:1, and 2% vinylene carbonate (VC) was added to prepare an electrolyte containing 1M LiPF6.
[0105] A polypropylene separator was selected, and the negative electrode sheet, separator, and positive electrode sheet were stacked in the order of stacking to form a 2Ah stacked battery. The SEM image of the dry-process negative electrode material layer obtained in this embodiment is shown in FIG. Figure 1 As shown, there are a lot of fibrous binders in the dry-process negative electrode material layer.
[0106] Embodiments 2 to 11
[0107] The methods of Examples 2 to 11 are the same as those of Example 1, except that different negative electrode composite materials are used. The specific differences are shown in Table 1.
[0108] Comparative Example 1
[0109] The method of Comparative Example 1 is the same as that of Example 1, except that the negative electrode composite material used in Comparative Example 1 is uncoated graphite powder.
[0110] Comparative Example 2
[0111] (1) The negative electrode composite material S1, the conductive agent (conductive carbon black Super-P-Li), the binder (SBR), the thickener (CMC) were mixed with deionized water in a mass ratio of 97:1:1:1 to prepare a conductive slurry, the conductive slurry was coated on a copper foil to form a negative electrode material layer with a thickness of 150 μm, and the wet negative electrode sheet was prepared after baking;
[0112] (2) After mixing the positive electrode active material lithium iron phosphate (LiFePO4), the conductive agent (CNT), and the binder (polyvinylidene fluoride PVDF) in a mass ratio of 97:1:2, the powder and NMP are stirred into a positive electrode slurry in a homogenizer and evenly coated on an aluminum foil;
[0113] Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 1:1:1, and 2% vinylene carbonate (VC) was added to prepare an electrolyte containing 1M LiPF6.
[0114] A polypropylene separator is selected and the negative electrode sheet, separator and positive electrode sheet are stacked in sequence to form a 2Ah laminated battery.
[0115] Comparative Examples 3~6
[0116] The methods of Comparative Examples 3 to 6 are the same as those of Example 1, except that different negative electrode composite materials are used. The specific differences are shown in Table 1.
[0117] Comparative Example 7
[0118] (1) Uncoated graphite powder, a conductive agent (Super-P-Li), and a binder (PTFE) are mixed in a mass ratio of 97:1:2, and the PTFE is fiberized by a jet mill to obtain a mixed powder. The mixed powder is calendered by a calender to obtain a dry-process negative electrode material layer with a thickness of 150 μm, and the dry-process negative electrode material layer is then composited with a current collector copper foil to obtain a dry-process negative electrode sheet for a lithium-ion battery;
[0119] (2) After mixing the positive electrode active material lithium iron phosphate (LiFePO4), the conductive agent (CNT), and the binder (PVDF) in a mass ratio of 97:1:2, the powder and NMP are stirred into a positive electrode slurry in a homogenizer and evenly coated on an aluminum foil;
[0120] Ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 1:1:1, and 5% VC was added to prepare an electrolyte containing 1M LiPF6.
[0121] A polypropylene separator is selected, and the negative electrode sheet, separator and positive electrode sheet are stacked in sequence to form a 2Ah laminated battery.
[0122] Table 1
[0123]
[0124] Test Case
[0125] The laminated batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 7 were subjected to an initial discharge efficiency test, a charge rate test, and a cycle test. The test methods are as follows. The test results are shown in Table 2.
[0126] First effect test:
[0127] In a constant temperature environment of 25℃, the battery was subjected to a 0.1C / 0.1C cycle test with a voltage range of 2.0V-3.8V (charged at 0.1C to a voltage of 3.8V, left for 10 min, and then discharged at a discharge rate of 0.1C to a voltage of 2.0V, i.e. 1 cycle). The battery's first charge specific capacity and first discharge specific capacity were recorded, and the battery's first charge and discharge efficiency was calculated based on this; battery first discharge efficiency (%) = first charge specific capacity / first discharge specific capacity*100%.
[0128] Charging rate test:
[0129] The battery was charged at 2C to a voltage of 3.8V at 25°C, left for 30 min, and then discharged at a discharge rate of 0.1C to a voltage of 2.0V. This cycle was repeated three times. The charge and discharge data of the third cycle was used to calculate the charge rate of the battery; 2C charge rate (%) = 2C charge capacity / 0.1C charge capacity*100%.
[0130] Cycle test:
[0131] In a constant temperature environment of 25℃, the battery was charged to 3.8V at 1C constant current and left for 10 min; then discharged to 2.0V at 1C constant current and left for 10 min; the cycle was terminated after 1000 times.
[0132] Table 2
[0133]
[0134] According to the data in Table 1, by comparing Examples 1 to 11 with Comparative Example 1, it can be seen that the inorganic coating layer of the present invention comprises an inorganic material having a certain Young's modulus, and the inorganic coating layer has a specific thickness, which can effectively protect the negative electrode active material and prevent the surface defects of the negative electrode active material from being directly exposed to the electrolyte, thereby improving the first discharge efficiency of the battery and improving the cycle life of the battery.
[0135] By comparing Example 1 with Comparative Example 2, it can be seen that since the inorganic coating layer of the negative electrode composite material has water absorption characteristics or can react with water, causing the inorganic coating layer to fail, Example 1 uses a dry method to prepare the negative electrode plate, which avoids the failure of the negative electrode composite material and effectively protects the negative electrode active material, thereby improving the first discharge efficiency of the battery and improving the cycle life of the battery.
[0136] By comparing Examples 1 to 11 with Comparative Examples 3 and 4, it can be seen that Examples 1 to 11 use an inorganic material with a higher Young's modulus to prepare the coating layer. The inorganic material has better mechanical properties and can protect the negative electrode active material during the fiberization process. At the same time, it avoids the water absorption characteristics of some inorganic coating layers or reactions with water, causing the inorganic coating layer to fail, thereby improving the first discharge efficiency of the battery and improving the cycle life of the battery.
[0137] By comparing Example 3 with Comparative Example 5, it can be seen that the thickness of the inorganic coating layer of Comparative Example 5 is too low, and the thickness of the inorganic coating layer of Example 3 is within the disclosed range, which can provide better protection for the negative electrode active material, thereby improving the first discharge efficiency of the battery and improving the cycle life of the battery.
[0138] By comparing Example 3 with Comparative Example 6, it can be seen that the thickness of the inorganic coating layer of Comparative Example 6 is too high, and the thickness of the inorganic coating layer of Example 3 is within the disclosed range, thereby avoiding a decrease in the electronic conductivity of the negative electrode and affecting the kinetic performance of the battery, thereby improving the first discharge efficiency of the battery and improving the cycle life of the battery.
[0139] By comparing Examples 1 to 11 with Comparative Example 7, it can be seen that the negative electrode plates of Examples 1 to 11 contain negative electrode composite materials having an inorganic coating layer, which can improve the first discharge efficiency, rate and electrical cycle life of the battery more than the solution of adding a film-forming additive VC to the battery system.
[0140] By comparing Example 3 with Example 7 and Example 8, it can be seen that the thickness of the inorganic coating layer in Example 3 is within the preferred range of the present disclosure, and the first discharge efficiency, rate performance and cycle performance of the battery are better.
[0141] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0142] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0143] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A dry-process negative electrode sheet, characterized in that: The dry-process negative electrode sheet comprises a current collector and a negative electrode material layer disposed on at least one surface of the current collector; the negative electrode material layer comprises a negative electrode composite material, a conductive agent and a fibrous binder, wherein at least part of the negative electrode composite material is dispersed in the fibrous binder; The negative electrode composite material comprises a negative electrode active material and an inorganic coating layer coated on the surface of the negative electrode active material, wherein the thickness of the inorganic coating layer is 0.5 to 50 nm; the Young's modulus of the negative electrode composite material is greater than 20 GPa; the negative electrode active material is selected from one or more of graphite, silicon carbon and hard carbon materials; The method for preparing the dry-process negative electrode sheet comprises: mixing the negative electrode composite material, the conductive agent and the binder to obtain a mixture, performing fiberization and calendering treatment on the mixture using a jet mill to obtain a negative electrode material layer; and then compounding the negative electrode material layer with a current collector.
2. The dry-process negative electrode sheet according to claim 1, wherein: The Young's modulus of the negative electrode composite material is 20-450 GPa; and the thickness of the inorganic coating layer is 5-30 nm.
3. The dry-process negative electrode sheet according to claim 1, wherein: The D50 particle size of the negative electrode composite material is 0.1-50 μm.
4. The dry-process negative electrode sheet according to claim 1, wherein: The inorganic coating layer comprises one or more of a metal oxide, a lithium-containing solid electrolyte compound, a lithium-containing inorganic base and an inorganic lithium salt; The metal element of the metal oxide is selected from one or more of Group IA, Group IIIA, Group IVA, Group IIB and Group IVB metal elements; The lithium-containing solid electrolyte compound is selected from doped or undoped lithium lanthanum zirconium oxide compounds, and the doping element is selected from one or more metal elements of Group IIIA, Group IVB and Group VB.
5. The dry-process negative electrode sheet according to claim 4, wherein: The metal oxide is selected from one or more of titanium oxide, aluminum oxide, sodium oxide, zinc oxide, tin oxide, indium oxide and zirconium oxide; The lithium-containing solid electrolyte compound is selected from one or more of lithium lanthanum zirconium oxide compounds, lithium lanthanum zirconium titanium oxides, lithium lanthanum zirconium tantalum oxides, lithium lanthanum zirconium aluminum oxides and lithium lanthanum zirconium niobium oxides; The lithium-containing inorganic base is selected from lithium hydroxide; The inorganic lithium salt is selected from one or more of lithium aluminate, lithium metaphosphate, lithium phosphate, lithium iron phosphate, lithium manganese phosphate, lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium carbonate, lithium sulfate, lithium sulfite, lithium hypochlorite, lithium fluoride, lithium iodide, lithium selenide, lithium indium, lithium nitride, lithium sulfide and lithium phosphide.
6. The dry-process negative electrode sheet according to claim 1, wherein: The inorganic coating layer further comprises a dispersant, which is selected from one or more of carboxymethyl cellulose, polyacrylic acid, polymethyl methacrylate and polyvinyl pyrrolidone; The mass ratio of the dispersant to the inorganic material in the inorganic coating layer is (0.1-1):
1.
7. The dry-process negative electrode sheet according to claim 1, wherein: The water contact angle θ of the negative electrode composite material is greater than 60°.
8. The dry-process negative electrode sheet according to claim 1, wherein: The method for preparing the negative electrode composite material comprises: allowing particles containing inorganic substances to form an inorganic coating layer on the surface of the negative electrode active material; The Young's modulus of the particles containing inorganic substances is 20 GPa or more.
9. The dry-process negative electrode sheet according to claim 8, wherein: The method for forming the inorganic coating layer is selected from one or more of liquid phase mixing solidification method, solid phase mixing depolymerization method, liquid phase deposition method, chemical vapor deposition method, liquid phase spray drying method, vapor phase spray deposition method, ion exchange method, atomic layer deposition method, sol-gel method and magnetron sputtering method.
10. The dry-process negative electrode sheet according to claim 9, wherein: When forming the inorganic coating layer, a dispersant is also added, and the dispersant is selected from one or more of carboxymethyl cellulose, polyacrylic acid, polymethyl methacrylate and polyvinyl pyrrolidone.
11. The dry-process negative electrode sheet according to claim 1, wherein: The thickness of the negative electrode material layer is 30-200 μm; In the negative electrode material layer, with respect to 80 to 100 parts by mass of the negative electrode composite material, the mass fraction of the binder is 19 or less, and the mass fraction of the conductive agent is 1 or less.
12. A lithium battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; wherein the negative electrode sheet is a dry-process negative electrode sheet as described in any one of claims 1 to 11.