A method for preparing a highly efficient hydrogenation catalyst and its application in the synthesis of gamma-butyrolactone
By combining modified biomass carbon and hydroxylated boron nitride nanosheets, combining copper oxide, nickel oxide and ruthenium oxide, the problems of decreasing catalyst activity and poor stability are solved, and γ-butyrolactone is achieved Efficient synthesis improves the performance and selectivity of the catalyst.
Patent Information
- Application Number
- CN202410630107.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-21
AI Technical Summary
The existing catalysts have problems of decreased activity, poor stability and high production costs in γ-butyrolactone synthesis, especially the high carbon adhesion and thermal stability of nickel-based catalysts and copper-based catalysts during use, which affects the Catalyst properties.
Modified biomass charcoal is used as a support, and the specific surface area and stability of the catalyst are improved by combining phosphorus doping and hydroxylated boron nitride nanosheets. enhances catalytic activity and selectivity.
It improves the active site exposure and surfactivity of the catalyst, extends the service life of the catalyst, improves the selectivity and conversion of γ-butyrolactone, reduces the generation of side reactions, and significantly improves the overall performance of the catalyst.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gamma-butyrolactone preparation, and in particular to a method for preparing a high-efficiency hydrogenation catalyst and application of the catalyst in synthesizing gamma-butyrolactone. Background Art
[0002] γ-Butyrolactone is an important organic chemical raw material with a wide range of uses. It is considered to be the most promising substitute for fluorinated organic solvents. It and its downstream products are involved in the fields of petrochemicals, textiles, fine chemicals, and medicine. With the rapid development of my country's petrochemical industry, the demand for γ-butyrolactone has also increased.
[0003] At present, γ-butyrolactone is mainly prepared by hydrogenation of maleic anhydride, which is low in cost. The preparation of γ-butyrolactone by hydrogenation of maleic anhydride is a typical selective hydrogenation reaction. With different degrees of hydrogenation, the products of maleic anhydride hydrogenation include succinic anhydride, γ-butyrolactone, tetrahydrofuran and 1,4-butanediol. Therefore, the key to preparing γ-butyrolactone by hydrogenation of maleic anhydride is to select a catalyst with high catalytic activity, good selectivity and control of the degree of hydrogenation. Maleic anhydride hydrogenation catalysts mainly include nickel-based catalysts, copper-based catalysts and precious metal catalysts. Nickel-based catalysts have good dispersibility, high catalytic activity and mild reaction conditions. However, high carbon materials in the catalytic process will adhere to the catalyst surface during use, resulting in a decrease in catalyst activity, thereby affecting the activity of the catalyst. Although copper-based catalysts have good hydrogenation performance, their thermal stability is poor, resulting in a short life of the catalyst. Precious metal catalysts have high catalytic activity, but they are expensive. Therefore, in specific use, based on production cost and catalytic activity considerations, multiple types of catalysts are often used in combination.
[0004] Patent application number 201911036521.1 provides a method for preparing γ-butyrolactone by liquid phase hydrogenation of maleic anhydride. The catalytic active components of the catalyst used in the method are copper oxide and nickel oxide, and the carrier is silicon oxide. In the catalyst, the metal ions have a strong interaction with the carrier, so that the catalytic active components cannot be well dispersed on the surface of the carrier, thereby affecting the stability of the catalyst, and further affecting the stability and catalytic activity of the catalyst. Based on the above problems, it is necessary to provide a new catalyst. Summary of the invention
[0005] The technical problem to be solved by the present invention is: in view of the deficiencies in the prior art, a method for preparing a high-efficiency catalytic hydrogenation catalyst and application of the catalyst in synthesizing gamma-butyrolactone are provided. The catalyst prepared by the present invention has a large specific surface area, high catalytic activity and good catalytic stability, and can well improve the conversion rate of raw materials and the selectivity of gamma-butyrolactone when used in synthesizing gamma-butyrolactone.
[0006] In order to solve the above technical problems, the technical solution of the present invention is:
[0007] A method for preparing a high-efficiency catalytic hydrogenation catalyst comprises the following steps:
[0008] preparing modified biochar;
[0009] The modified biomass carbon is used to load the catalytic active components.
[0010] Preferably, the method for preparing modified biochar comprises the following steps:
[0011] S1: Soaking the crushed and dried plant skin in a phosphoric acid solution;
[0012] S2: After soaking, take out, dry and then calcine to obtain phosphorus-doped biochar;
[0013] S3: Evenly mix the hydroxylated boron nitride nanosheet dispersion and the phosphorus-doped biochar obtained above, add the ethanol solution of ethyl orthosilicate and continue stirring, dry and then calcine to obtain modified biochar.
[0014] Preferably, in S1, the concentration of the phosphoric acid solution is 80-90wt%, and the mass ratio of the phosphoric acid solution to the plant skin during soaking is 1:(2-5); and the soaking time is 20-30h.
[0015] Preferably, in S2, the calcination treatment conditions are: inert atmosphere, calcination at 800-850°C for 50-60 min, and the heating rate during calcination is 5-10°C / min.
[0016] Preferably, in S3, the hydroxylated boron nitride nanosheet dispersion is prepared by dispersing hydroxylated boron nitride nanosheets in anhydrous ethanol, and the concentration of the hydroxylated boron nitride nanosheet dispersion is 2-5 g / L; the ethanol solution of tetraethyl orthosilicate is prepared by mixing tetraethyl orthosilicate, ethanol and water, and the volume ratio of tetraethyl orthosilicate, ethanol and water is 1:(40-50):(2-5); the mass ratio of the hydroxylated boron nitride nanosheet dispersion, phosphorus-doped biomass and the ethanol solution of tetraethyl orthosilicate is 10:(2-5):(5-10); the conditions for the roasting treatment are: inert atmosphere, 500-600°C, roasting time of 6-10h, and heating rate during roasting of 1-5°C / min.
[0017] Preferably, the modified biochar is used to load the catalytic active components, which specifically includes the following steps:
[0018] (1) dissolving an active component precursor in water to prepare a first precursor solution;
[0019] (2) placing the modified biochar in a first precursor solution for a first immersion treatment;
[0020] (3) After the first impregnation, the product is taken out and dried, and finally calcined to obtain an intermediate;
[0021] (4) The intermediate is placed in a ruthenium precursor solution for a second impregnation treatment, then dried, and finally subjected to a second calcination treatment to obtain a catalyst.
[0022] Preferably, in step (1), the active component precursor is a mixture of a copper precursor and a nickel precursor, and further, the copper precursor is selected from one of copper nitrate, copper sulfate and copper chloride; the nickel precursor is selected from one of nickel nitrate, nickel sulfate and nickel chloride; and the concentration of the precursor solution is 1-5 mg / ml.
[0023] Preferably, in step (2), the temperature of the first immersion treatment is room temperature, and the time of the first immersion treatment is 20-30 hours.
[0024] Preferably, in step (3), the conditions of the primary calcination treatment are: calcination in an inert atmosphere at 300-400° C. for 2-3 h; and a heating rate during calcination of 2-8° C. / min.
[0025] Preferably, in step (4), the concentration of ruthenium trichloride in the ruthenium precursor solution is 30-40 mg / L, and the molar ratio of sodium borohydride to ruthenium trichloride is (3-5):1;
[0026] The temperature of the secondary immersion treatment is room temperature and the time is 10-30h;
[0027] The conditions of the secondary calcination are: inert atmosphere, 200-300° C., 1-2 h;
[0028] In the catalyst, the contents of copper oxide, nickel oxide and ruthenium oxide are 5-10wt%, 5-10wt% and 0.01-0.05wt% respectively, and the rest is modified activated carbon.
[0029] Furthermore, in order to better solve the problems pointed out in the background technology, the present invention also discloses the following technical solutions:
[0030] Application of a high-efficiency catalytic hydrogenation catalyst in the synthesis of gamma-butyrolactone comprises the following steps:
[0031] Maleic anhydride and hydrogen are added into a fixed bed reactor containing the above catalyst for contact reaction, and the product after the reaction is cooled to obtain gamma-butyrolactone.
[0032] Preferably, the diameter of the fixed bed reactor is 10-20 mm, the filling height is 5-8 cm; the molar ratio of maleic anhydride to hydrogen is 1:(10-20); the liquid hourly space velocity of maleic anhydride is 0.5-1 h -1; The temperature of the contact reaction is 200-300°C and the pressure is 0.2MPa.
[0033] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0034] The invention provides a catalyst, which is prepared by compounding hydroxylated boron nitride nanosheets, phosphorus-modified biomass carbon and silicon dioxide. The hydroxylated boron nitride nanosheets have a high specific surface area and good chemical stability, and can increase the specific surface area of the catalyst, improve the exposure of active sites, and thus improve the catalytic activity; the phosphorus-modified biomass carbon is used as a heteroatom doping material to introduce active sites and improve the surface activity of the catalyst; silicon dioxide is used as a supporting material to improve the stability and mechanical strength of the catalyst, and an appropriate amount of silicon dioxide can increase the specific surface area of the catalyst and improve the dispersibility of the active sites, thereby improving the catalytic activity.
[0035] The present invention uses phosphorus element to in-situ dope biochar. Phosphorus doping can increase the acid-base properties of the catalyst surface and improve the surface characteristics of the catalyst. In addition, phosphorus element, as an active center, can provide additional active sites to promote the adsorption and conversion of reactants, thereby improving catalytic activity, reducing the occurrence of side reactions, and improving the selectivity of target products.
[0036] The present invention uses copper oxide, nickel oxide, and ruthenium oxide as catalytic active components. The three oxides have different active sites on their surfaces, which work synergistically with each other to improve the overall performance of the catalyst. In addition, copper oxide, ruthenium oxide, and nickel oxide can stabilize the active sites of each other, thereby improving the stability and anti-poisoning of the catalyst and extending the service life of the catalyst. DETAILED DESCRIPTION
[0037] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0038] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0039] In the following embodiments, orange peel is selected as the plant peel, and hydroxyboron nitride nanosheets are prepared by treating purchased boron nitride nanosheets with a sodium hydroxide solution; specifically, boron nitride nanosheets (purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a thickness of 50-400nm, a sheet size of 0.5-5μm, and a purity of 99wt%) and sodium hydroxide solution (5mol / L) are mixed in a ratio of 0.5g:100ml and then immersed at 120°C for 20h to prepare the product.
[0040] Unless otherwise specified, other raw materials in the following examples are commercially available.
[0041] The preparation process of the catalyst is described in detail through Examples 1-3.
[0042] Example 1
[0043] S1: mixing 80 wt% phosphoric acid solution and orange peel in a mass ratio of 1:2 and soaking for 24 hours;
[0044] S2: After soaking, the solid was dried at 120°C until the weight of the solid did not change. The dried solid was placed in a muffle furnace, heated to 800°C at a rate of 6°C / min under an inert atmosphere and calcined for 60 min to obtain phosphorus-modified biochar;
[0045] S3: 100 g of 2 g / L hydroxylated boron nitride nanosheet dispersion and 20 g of the phosphorus-doped biochar obtained above were mixed evenly, 80 g of ethyl orthosilicate ethanol solution (the volume ratio of ethyl orthosilicate, ethanol and water was 1:40:2) was added, and stirring was continued for 20 min. After that, the mixture was dried at 100 ° C for 10 h and placed in a muffle furnace. Under an inert atmosphere, the temperature was increased to 500 ° C at a heating rate of 2 ° C / min and calcined for 6 h to obtain modified biochar;
[0046] S4: Dissolve copper nitrate and nickel nitrate in deionized water to prepare a precursor solution with a concentration of 2 mg / ml, place the modified biochar in the precursor solution, and immerse it at room temperature for 24 hours; after the immersion, dry and remove the solvent, and finally place the dried solid in a muffle furnace, heat it to 400°C at a rate of 5°C / min under an inert atmosphere, and calcine it for 2 hours to obtain an intermediate;
[0047] S5: placing the above intermediate in a ruthenium precursor solution (the concentration of ruthenium trichloride is 40 mg / L; the molar ratio of sodium borohydride to ruthenium trichloride is 5:1), immersing for 24 hours at room temperature, then drying, and finally placing in a muffle furnace, calcining at 250° C. for 1 hour in an inert atmosphere to obtain a catalyst;
[0048] In the above process, the conditions are controlled so that the contents of copper oxide, nickel oxide and ruthenium oxide in the catalyst are 5wt%, 5wt% and 0.01wt% respectively, and the rest is modified activated carbon.
[0049] Example 2
[0050] S1: mixing 80 wt% phosphoric acid solution and orange peel in a mass ratio of 1:3 and soaking for 24 hours;
[0051] S2: After soaking, the solid was dried at 120°C until the weight of the solid did not change. The dried solid was placed in a muffle furnace, heated to 800°C at a rate of 8°C / min under an inert atmosphere and calcined for 60 min to obtain phosphorus-modified biochar;
[0052] S3: 100 g of 4 g / L hydroxylated boron nitride nanosheet dispersion and 30 g of the phosphorus-doped biochar obtained above were mixed evenly, 60 g of ethyl orthosilicate ethanol solution (the volume ratio of ethyl orthosilicate, ethanol and water was 1:40:3) was added, and stirring was continued for 20 min. After that, the mixture was dried at 100 ° C for 10 h and placed in a muffle furnace. Under an inert atmosphere, the mixture was heated to 500 ° C at a heating rate of 2 ° C / min and calcined for 6 h to obtain modified biochar;
[0053] S4: Dissolve copper nitrate and nickel nitrate in deionized water to prepare a precursor solution with a concentration of 3 mg / ml, place the modified biochar in the precursor solution, and immerse it at room temperature for 24 hours; after the immersion, dry and remove the solvent, and finally place the dried solid in a muffle furnace, heat it to 400°C at a rate of 5°C / min under an inert atmosphere, and calcine it for 2 hours to obtain an intermediate;
[0054] S5: placing the above intermediate in a ruthenium precursor solution (the concentration of ruthenium trichloride is 40 mg / L; the molar ratio of sodium borohydride to ruthenium trichloride is 5:1), immersing for 24 hours at room temperature, then drying, and finally placing in a muffle furnace, calcining at 250° C. for 1 hour in an inert atmosphere to obtain a catalyst;
[0055] In the above process, the conditions are controlled so that the contents of copper oxide, nickel oxide and ruthenium oxide in the catalyst are 6wt%, 8wt% and 0.01wt% respectively, and the rest is modified activated carbon.
[0056] Example 3
[0057] S1: mixing 80 wt % phosphoric acid solution and orange peel in a mass ratio of 1:5 and soaking for 24 hours;
[0058] S2: After soaking, the solid was dried at 120°C until the solid weight did not change. The dried solid was placed in a muffle furnace, heated to 800°C at a rate of 7°C / min under an inert atmosphere and calcined for 60 min to obtain phosphorus-modified biochar;
[0059] S3: 100 g of 5 g / L hydroxylated boron nitride nanosheet dispersion and 50 g of the phosphorus-doped biochar obtained above were mixed evenly, 80 g of ethyl orthosilicate ethanol solution (the volume ratio of ethyl orthosilicate, ethanol and water was 1:50:5) was added, and the mixture was stirred for 20 min, and then dried at 100 ° C for 10 h and placed in a muffle furnace. Under an inert atmosphere, the mixture was heated to 500 ° C at a heating rate of 5 ° C / min and calcined for 8 h to obtain modified biochar;
[0060] S4: Dissolve copper nitrate and nickel nitrate in deionized water to prepare a precursor solution with a concentration of 4 mg / ml, place the modified biochar in the precursor solution, and immerse it at room temperature for 24 hours; after the immersion, dry and remove the solvent, and finally place the dried solid in a muffle furnace, heat it to 400°C at a rate of 6°C / min under an inert atmosphere, and calcine it for 2 hours to obtain an intermediate;
[0061] S5: placing the above intermediate in a ruthenium precursor solution (the concentration of ruthenium trichloride is 40 mg / L; the molar ratio of sodium borohydride to ruthenium trichloride is 5:1), immersing for 24 hours at room temperature, then drying, and finally placing in a muffle furnace, calcining at 250° C. for 1 hour in an inert atmosphere to obtain a catalyst;
[0062] In the above process, the conditions are controlled so that the contents of copper oxide, nickel oxide and ruthenium oxide in the catalyst are 8wt%, 5wt% and 0.01wt% respectively, and the rest is modified activated carbon.
[0063] In order to verify the effect of various process parameters in catalyst preparation conditions on the catalyst, a comparative example is given below for detailed description.
[0064] Comparative Example 1
[0065] Compared with Example 1, the difference is that in S1, phosphoric acid solution is not used for immersion, and other conditions are the same as those in Example 1.
[0066] Comparative Example 2
[0067] Compared with Example 1, the difference is that in S1, the mass ratio of the phosphoric acid solution to the orange peel is 2:1, and the other conditions are the same as those in Example 1.
[0068] Comparative Example 3
[0069] Compared with Example 1, the difference is that in S3, the mass ratio of the hydroxylated boron nitride nanosheet dispersion, phosphorus-doped biochar, and ethyl orthosilicate ethanol solution is 10:2:15, and the other conditions are the same as in Example 1.
[0070] Comparative Example 4
[0071] Compared with Example 1, the difference is that in S3, the mass ratio of the hydroxylated boron nitride nanosheet dispersion, phosphorus-doped biochar, and ethyl orthosilicate ethanol solution is 10:7:8, and the other conditions are the same as in Example 1.
[0072] Comparative Example 5
[0073] Compared with Example 1, the difference is that in S3, phosphorus-doped biochar is used as the catalyst carrier, and other conditions are the same as in Example 1.
[0074] Comparative Example 6
[0075] Compared with Example 1, the difference lies in that: in S3, hydroxylated boron nitride nanosheets are used as catalyst carriers, and other conditions are the same as in Example 1.
[0076] Comparative Example 7
[0077] Compared with Example 1, the difference is that in S3, phosphorus-doped biochar and hydroxylated boron nitride nanosheet dispersion are not added, and other conditions are the same as in Example 1.
[0078] Comparative Example 8
[0079] Compared with Example 1, the difference is that in S4, by controlling the amount of copper nitrate, nickel nitrate, ruthenium trichloride and modified biochar, the contents of copper oxide, nickel oxide and ruthenium oxide in the catalyst are 15wt%, 5wt% and 0.01wt% respectively, and the rest is modified activated carbon. Other conditions are the same as in Example 1.
[0080] Comparative Example 9
[0081] Compared with Example 1, the difference is that in S4, by controlling the amount of copper nitrate, nickel nitrate, ruthenium trichloride and modified biochar, the contents of copper oxide, nickel oxide and ruthenium oxide in the catalyst are 5wt%, 15wt% and 0.01wt% respectively, and the rest is modified activated carbon. Other conditions are the same as in Example 1.
[0082] Comparative Example 10
[0083] Compared with Example 1, the difference is that in S4, only copper oxide is added to the catalyst, and by controlling the amount of copper nitrate and modified biochar, the content of copper oxide in the catalyst is 10wt%, and the rest is modified activated carbon. Other conditions are the same as in Example 1.
[0084] Comparative Example 11
[0085] Compared with Example 1, the difference is that in S4, only nickel oxide is added to the catalyst, and by controlling the amount of nickel nitrate and modified biochar, the content of nickel oxide in the catalyst is 10wt%, and the rest is modified activated carbon. Other conditions are the same as in Example 1.
[0086] Comparative Example 12
[0087] Compared with Example 1, the difference is that in S5, the heating rate is controlled to be 10°C / min, and the other conditions are the same as those in Example 1.
[0088] The performance of the catalysts prepared in the above examples and comparative examples was characterized, and the characterization results are shown in Table 1.
[0089] Table 1
[0090]
[0091]
[0092] It can be seen from the above test results that, compared with the comparative example, the catalyst prepared in the present invention has a higher specific surface area.
[0093] The specific surface areas of the catalysts obtained in Comparative Examples 1 and 2 are lower than those in Example 1. This is mainly because no phosphorus is doped in Comparative Example 1, and the specific surface area of the obtained biochar is slightly lowered, while excessive phosphorus doping in Comparative Example 2 leads to instability of the biochar structure and changes in the pore structure, thereby reducing the specific surface area of the biochar.
[0094] The catalysts of Comparative Examples 3-4 respectively increase the amount of silicon oxide and phosphorus-doped biochar in the carrier, but the specific surface area of the catalyst also decreases. This is mainly because excessive silicon dioxide and excessive phosphorus-doped modified biochar will cause a stacking effect, thereby affecting the specific surface area of the catalyst.
[0095] The specific surface area of the catalysts of Comparative Examples 5-7 is also somewhat lower than that of Example 1. This is mainly because the hydroxylated boron nitride nanosheets have a higher specific surface area, the phosphorus-doped biochar has a porous structure, and the silica particles are small and also have a higher specific surface area. The carrier prepared by the composite of the three has good dispersibility and a higher specific surface area than a single carrier.
[0096] In Comparative Examples 8-12, as the loading amount of active components increases, the specific surface area of the catalyst also decreases.
[0097] In Comparative Example 13, the heating rate was too fast during the calcination of the catalyst, and the specific surface area of the catalyst decreased. This is mainly because, although the heating rate was too fast, the growth of particles was inhibited to a certain extent, so that the active component particles remained smaller, but it also led to poor dispersion between the particles, causing the active component particles to pile up, thereby reducing the specific surface area of the catalyst.
[0098] In summary, the present invention obtains a catalyst with a high specific surface area by optimizing the composition of the carrier, the composition of the catalyst active components and the preparation process parameters.
[0099] In order to verify the catalytic activity and catalytic stability of the catalysts prepared in the above examples and comparative examples, the following application examples are given for detailed description.
[0100] Application Examples 1-3
[0101] The catalysts prepared in Examples 1-3 were respectively loaded into a fixed bed reactor with a diameter of 10 mm, and the loading height was 5 cm. Maleic anhydride and hydrogen were respectively added into the fixed bed reactor loaded with the catalyst, and the molar ratio of maleic anhydride to hydrogen was 1:15. The liquid hourly space velocity of maleic anhydride was 0.7 h -1 The contact reaction was carried out at a temperature of 220°C and a pressure of 0.2 MPa for 2 hours. After the reaction, the product was cooled to obtain γ-butyrolactone, and the catalytic activity of the catalyst was tested after continuous reaction for 3000 hours.
[0102] Comparative Application Examples 1-12
[0103] The catalysts prepared in Comparative Examples 1-13 were respectively loaded into a fixed bed reactor with a diameter of 10 mm, and the loading height was 5 cm. Maleic anhydride and hydrogen were respectively added to the fixed bed reactor loaded with the catalyst, and the molar ratio of maleic anhydride to hydrogen was 1:15. The liquid hourly space velocity of maleic anhydride was 0.7 h -1 The contact reaction was carried out at a temperature of 220°C and a pressure of 1 MPa for 2 hours. After the reaction, the product was cooled to obtain γ-butyrolactone, and the catalytic activity of the catalyst was tested after continuous reaction for 3000 hours.
[0104] The conversion rates of γ-butyrolactone and maleic anhydride in the above application examples and comparative application examples were analyzed by gas chromatography. The test results are shown in Table 2.
[0105] Maleic anhydride conversion rate (%) = [(the amount of maleic anhydride in the raw material - the amount of maleic anhydride remaining after the reaction) / the amount of maleic anhydride in the raw material] × 100%.
[0106] γ-butyrolactone selectivity (%) = [amount of γ-butyrolactone / (amount of maleic anhydride in the raw material - amount of maleic anhydride remaining after the reaction)] × 100%
[0107] Table 2
[0108]
[0109] The test results in Table 2 show that the catalyst of the present invention has high catalytic activity, and after being used for 3000 hours, the catalytic activity does not decrease significantly, and the stability is good.
[0110] It can be seen from the comparison between Application Examples 1-2 and Application Example 1 that an appropriate amount of phosphorus doping can effectively improve the activity and stability of the catalyst, but excessive phosphorus doping will reduce the catalytic activity and stability of the catalyst. This is mainly because phosphorus doping can increase the acid-base properties of the catalyst surface. As an active center, phosphorus can provide additional active sites to promote the adsorption and conversion of reactants, thereby improving catalytic activity. In addition, phosphorus doping can regulate the adsorption behavior of reactants, reduce the production of side reactions, and improve the selectivity of target products. The presence of phosphorus can also form a protective layer on the catalyst surface, inhibit the aggregation of metal active components, and prevent the deactivation of the catalyst. However, excessive phosphorus doping will affect the distribution and availability of active sites on the catalyst surface, thereby reducing the efficiency of adsorption and activation of reactant molecules.
[0111] It can be seen from the comparison of comparative application examples 3-7 and application example 1 that the catalyst prepared by the present invention with hydroxylated boron nitride nanosheets, phosphorus-doped biochar and silicon dioxide in a suitable ratio as a carrier not only has high catalytic activity but also good stability. In comparative application examples 3 and 4, the amount of silicon dioxide and phosphorus-doped biochar added is too much, and the catalytic activity and catalytic stability of the catalyst are reduced. This is mainly because excessive phosphorus-modified biochar will affect the specific surface area of the catalyst, reduce the exposure of active sites, and affect the activity of the catalyst. Excessive silicon dioxide may cause the looseness of the catalyst pore structure, reduce the specific surface area, and reduce the activity of the catalyst. The catalysts in comparative application examples 5-7 use a single type of carrier, and the catalytic activity of the catalyst is also reduced.
[0112] It can be seen from the comparative application examples 8-11 and the application examples that the present invention uses copper oxide, nickel oxide, and ruthenium oxide in a suitable ratio as catalytic active components, and the obtained catalyst has not only high catalytic activity but also good catalytic stability. Excessive addition of copper oxide, ruthenium oxide, and nickel oxide easily causes accumulation of catalytic active components, thereby reducing the catalytic activity and catalytic stability of the catalyst.
[0113] It can be seen from the comparison between Comparative Application Example 12 and Example 1 that a suitable heating rate will also affect the performance of the catalyst. A suitable heating rate will improve the specific surface area of the catalyst and the dispersibility of the active components, thereby improving the performance of the catalyst.
[0114] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for preparing a highly efficient catalytic hydrogenation catalyst, characterized in that: The following steps are involved: preparing modified biochar; The modified biochar is used to load the catalytic active components; The preparation method of modified biochar comprises the following steps: S1: soaking the crushed and dried plant skin in a phosphoric acid solution; the concentration of the phosphoric acid solution is 80-90wt%; the mass ratio of the phosphoric acid solution to the plant skin during soaking is 1:(2-5); the soaking time is 20-30h; S2: After soaking, take out, dry and calcine to obtain phosphorus-doped biochar; the calcination conditions are: inert atmosphere, calcination at 800-850°C for 50-60min, and the heating rate during calcination is 5-10°C / min; S3: uniformly mix the hydroxylated boron nitride nanosheet dispersion and the phosphorus-doped biochar obtained above, add an ethanol solution of tetraethyl orthosilicate and continue stirring, dry and then calcine to obtain modified biochar; the hydroxylated boron nitride nanosheet dispersion is prepared by dispersing hydroxylated boron nitride nanosheets in anhydrous ethanol, and the concentration of the hydroxylated boron nitride nanosheet dispersion is 2-5 g / L; the ethanol solution of tetraethyl orthosilicate is prepared by mixing tetraethyl orthosilicate, ethanol and water, and the volume ratio of tetraethyl orthosilicate, ethanol and water is 1: (40-50): (2-5); the mass ratio of the hydroxylated boron nitride nanosheet dispersion, phosphorus-doped biomass and ethanol solution of tetraethyl orthosilicate is 10: (2-5): (5-10); the calcination treatment conditions are: inert atmosphere, 500-600°C, calcination time is 6-10h, and the heating rate during calcination is 1-5°C / min; The modified biochar is used to load the catalytic active components, including: (1) dissolving an active component precursor in water to prepare a first precursor solution; the active component precursor is a mixture of a copper precursor and a nickel precursor; the concentration of the first precursor solution is 1-5 mg / ml; (2) placing the modified biochar in a first precursor solution for a first immersion treatment; (3) drying after impregnation and finally calcining to obtain an intermediate; (4) placing the intermediate in a ruthenium precursor solution for secondary impregnation treatment, then drying, and finally performing secondary calcination treatment to obtain a catalyst; the concentration of ruthenium trichloride in the ruthenium precursor solution is 30-40 mg / L, and the molar ratio of sodium borohydride to ruthenium trichloride is (3-5):1; in the catalyst, the contents of copper oxide, nickel oxide, and ruthenium oxide are 5-10wt%, 5-10wt%, and 0.01-0.05wt%, respectively, and the rest is modified activated carbon.
2. The method for preparing a high-efficiency catalytic hydrogenation catalyst according to claim 1, characterized in that: In step (1), the copper precursor is selected from one of copper nitrate, copper sulfate and copper chloride; the nickel precursor is selected from one of nickel nitrate, nickel sulfate and nickel chloride.
3. The method for preparing a high-efficiency catalytic hydrogenation catalyst according to claim 1, characterized in that: Include at least one of the following characteristics: In step (2), the temperature of the first immersion treatment is room temperature, and the immersion treatment time is 20-30 hours; In step (3), the conditions of the primary calcination treatment are: calcination in an inert atmosphere at 300-400°C for 2-3h; the heating rate during calcination is 2-8°C / min; In step (4), the temperature of the secondary immersion treatment is room temperature and the time is 10-30 hours; The conditions of the secondary calcination treatment are: inert atmosphere, 200-300° C., 1-2 h.
4. The use of a high-efficiency catalytic hydrogenation catalyst according to any one of claims 1 to 3, characterized in that: include: Maleic anhydride and hydrogen are added into a fixed bed reactor containing the above catalyst for contact reaction, and the product after the reaction is cooled to obtain gamma-butyrolactone.
5. The use of a high-efficiency catalytic hydrogenation catalyst according to claim 4, characterized in that: Include at least one of the following characteristics: The diameter of the fixed bed reactor is 10-20 mm, and the filling height of the catalyst is 5-8 cm; The molar ratio of maleic anhydride to hydrogen is 1:(10-20); The liquid hourly space velocity of maleic anhydride is 0.5-1h -1 ; The contact reaction is carried out at a temperature of 200-300° C. and a pressure of 0.2 MPa.
Citation Information
Patent Citations
Method for preparing gamma-butyrolactone through maleic anhydride liquid phase hydrogenation
CN112742394A
Nickel supported catalyst for liquid phase hydrogenation synthesis of gamma-butyrolactone from maleic anhydride, and preparation method and application thereof
CN106914246A
Catalyst for selectively hydrogenating dimethyl oxalate to produce methyl glycolate and preparation method thereof and application thereof
CN109201059A
Catalyst for preparing succinic anhydride by hydrogenation of maleic anhydride, and preparation method and application thereof
CN112808292A
Catalyst for loading copper on boron nitride composite carrier as well as preparation method and use method of catalyst
CN115722244A