A renewable defluorination agent and its preparation method and application

CN118598322BActive Publication Date: 2024-11-05ZHEJIANG WATER HEALER ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075817.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
2044-08-07

Smart Images

  • Figure CN118598322B_ABST
    Figure CN118598322B_ABST
Patent Text Reader

Abstract

The present invention provides a renewable defluorinating agent and a preparation method and application thereof. The method uses Na2CO3, hydrochloric acid and NaOH to purify photovoltaic wastewater sludge, which can avoid the mixing of impurities when alkali solution leaches silicon elements, thereby obtaining a sodium silicate solution with high purity, further preparing a defluorinating agent matrix, and also improving the resource utilization rate of calcium fluoride sludge in the later stage. The renewable defluorinating agent method provided by the present invention has the characteristics of simple preparation process, good defluorination effect and high regeneration efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a renewable defluorinating agent, in particular to a renewable defluorinating agent and a preparation method and application thereof, and belongs to the field of material science. Background Art

[0002] In recent years, my country has vigorously supported the new energy industry, information technology has developed rapidly, and the photovoltaic industry has developed rapidly. At the same time, a large amount of wastewater sludge has also been generated. Its main components are CaF2, SiO2, CaSO4, precipitants, flocculants, etc., which has caused the problem of difficult disposal and high cost. According to the main components of photovoltaic wastewater sludge, it can be reasonably disposed and resourced, which can not only eliminate the potential pollution of photovoltaic wastewater sludge, but also recycle the mineral elements in it, turning solid waste into treasure and danger into safety, which can create greater social benefits and economic value.

[0003] At present, after the sludge of photovoltaic industry wastewater is purified, CaF2 is mainly used as a substitute for fluorite in the industrial production of fluorine chemical industry according to the purity level. It is also used as an additive or flux in the construction, metallurgy and ceramic industries; but the large amount of silicon element in it has not been fully utilized.

[0004] Therefore, using silicon in photovoltaic wastewater to prepare a renewable defluorination agent has become the current research direction. Summary of the invention

[0005] The invention provides a preparation method of a renewable defluorinating agent. The preparation method uses wastewater sludge as a main raw material and has the characteristics of simple preparation process, good defluorinating effect and high regeneration efficiency.

[0006] The present invention also provides a regenerable defluorinating agent, which has the characteristics of good defluorinating effect and high regeneration efficiency.

[0007] The present invention also provides a device for producing a renewable defluorinating agent, which has the characteristics of high integration and can realize continuous preparation of the defluorinating agent.

[0008] The present invention provides a method for preparing a regenerable defluorinating agent, which comprises the following steps:

[0009] 1) contacting photovoltaic wastewater sludge with a sodium carbonate aqueous solution, and performing solid-liquid separation treatment on the obtained mixed system to obtain solid A;

[0010] 2) contacting the solid A with a hydrochloric acid solution, and performing solid-liquid separation on the obtained mixed system to obtain a solid B;

[0011] 3) contacting the solid B with a sodium hydroxide aqueous solution, and performing solid-liquid separation treatment on the obtained mixed system to obtain calcium fluoride sludge and a sodium silicate aqueous solution;

[0012] 4) mixing the sodium silicate aqueous solution with aluminum hydroxide, zinc hydroxide and sodium hydroxide and stirring the mixture, mixing the obtained mixed system with a template and heating the mixture to a first temperature to obtain a first temperature system;

[0013] 5) mixing the first temperature system with sodium bicarbonate and subjecting the mixture to a first microwave treatment, while simultaneously heating the mixture to a second temperature to obtain a second temperature system;

[0014] 6) performing a second microwave treatment on the second temperature system, and performing a solid-liquid separation treatment on the obtained second microwave system to obtain a liquid phase product and a regenerable defluorination agent matrix;

[0015] 7) contacting the regenerable defluorinating agent matrix with an aqueous solution comprising aluminum ions and iron ions to obtain the regenerated regenerable defluorinating agent;

[0016] The template agent includes morpholine and isopropylamine;

[0017] The first temperature is 70-80°C, and the second temperature is 160-200°C;

[0018] In step 4), the molar ratio of the sodium silicate, the aluminum hydroxide, the zinc hydroxide and the sodium hydroxide is 1: (0.1-0.4): (0.01-0.05): (0.5-1.5).

[0019] The method for preparing the renewable defluorinating agent as described above, wherein, in step 1), the concentration of the sodium carbonate aqueous solution is 2.5-5 mol / L, the contact temperature of the photovoltaic wastewater sludge and the sodium carbonate aqueous solution is 50-80° C., and the contact time is 2-5 h; and / or,

[0020] In step 2), the concentration of the hydrochloric acid solution is 1.5-3.5 mol / L, the contact temperature of the solid A and the hydrochloric acid solution is 20-30° C., and the contact time is 0.5-1 h; and / or,

[0021] In step 3), the concentration of the sodium hydroxide aqueous solution is 10-25 mol / L, the contact temperature of the solid B and the sodium hydroxide aqueous solution is 80-150° C., and the contact time is 3-10 h.

[0022] The method for preparing the regenerable defluorinating agent as described above, wherein the processing power of the first microwave treatment is 300w, and the processing time is 10-40min; and / or;

[0023] The second microwave treatment has a processing power of 400W and a processing time of 30 to 120min; and / or,

[0024] Step 3) further comprises using a nanofiltration membrane to concentrate the sodium silicate aqueous solution to obtain a concentrated sodium silicate aqueous solution as a reaction raw material in step 4);

[0025] The operating pressure of the concentration treatment is 0.8~1.4MPa, and the operating temperature is 30~40℃.

[0026] The method for preparing the regenerable defluorinating agent as described above, wherein, in the aqueous solution comprising aluminum ions and iron ions, the concentration of aluminum ions is 0.3-1 mol / L, the concentration of iron ions is 0.1-0.2 mol / L, and the concentration of hydrochloric acid is 0.08-0.15 mol / L; and / or,

[0027] Step 7) further comprises: drying the renewable defluorinating agent matrix at 400-450° C. for 1-3 hours, mixing it with the aqueous solution comprising aluminum ions and iron ions, adding hydrochloric acid to the obtained mixed system to adjust the pH value of the mixed system to 2-3, and then subjecting the mixed system to ultrasonic oscillation treatment for 1-4 hours to obtain an ultrasonic oscillation treatment system; subjecting the ultrasonic oscillation treatment system to solid-liquid separation treatment, washing the obtained solid phase product with distilled water until the pH value of the washing liquid obtained by washing is 7, and then vacuum drying the solid phase product at 80-150° C. for 2-5 hours to obtain the renewable defluorinating agent; and / or,

[0028] In step 5), the ratio of the amount of the sodium bicarbonate substance to the sum of the amounts of the aluminum hydroxide and the zinc hydroxide substance is (0.05-0.08): 1; and / or,

[0029] The ratio of the amount of the template substance to the sum of the amounts of the aluminum hydroxide and the zinc hydroxide substances is 0.8-1.5:1.

[0030] The method for preparing the regenerable defluorinating agent as described above, wherein step 6) further comprises extracting the liquid phase product with an organic solvent to obtain a mixture including a template and an aqueous phase mixture;

[0031] Flash evaporating the mixture including the template to obtain the template as the reaction raw material in step 4);

[0032] The aqueous phase mixture is mixed with the sodium hydroxide aqueous solution in step 3) as a reaction raw material.

[0033] The present invention also provides a renewable defluorinating agent, wherein the renewable defluorinating agent is prepared using any of the above-mentioned methods for preparing the renewable defluorinating agent.

[0034] The present invention also provides a defluorination method, wherein the defluorination method uses any of the above-mentioned regenerable defluorination agents to contact a to-be-treated object containing fluoride ions to obtain a treated product and a fluorine-containing defluorination agent.

[0035] The defluorination method as described above, wherein the method further comprises subjecting the fluorine-containing defluorination agent to acid treatment, alkali treatment, rinsing treatment and drying treatment in sequence to obtain a regenerated defluorination agent;

[0036] The acid treatment comprises contacting the fluorine-containing defluorinating agent with a hydrochloric acid solution, wherein the concentration of the hydrochloric acid solution is 0.02-0.06 mol / L, and the contact time is 1-3 hours, to obtain an acid-treated product;

[0037] The alkali treatment comprises contacting the acid-treated product with an aqueous sodium hydroxide solution, wherein the concentration of the aqueous sodium hydroxide solution is 0.04 to 0.08 mol / L, and the contact time is 2 to 6 hours, to obtain an alkali-treated product;

[0038] The rinsing treatment includes rinsing the alkali-treated product with distilled water until the pH value of the washing solution obtained by rinsing is 7, thereby obtaining a rinsed product;

[0039] The drying treatment includes vacuum drying the flushing product at 100-180° C. for 2-5 hours to obtain the regenerated defluorination agent.

[0040] The present invention also provides a production system of a renewable defluorinating agent, which is used to perform any of the above-mentioned methods for preparing a renewable defluorinating agent, wherein the system comprises a desulfurization reactor, an acidification reactor, a leaching reactor, a membrane concentration device, and a reactor for steps 4) to 6) of the above-mentioned method for preparing a renewable defluorinating agent, which are connected in sequence;

[0041] The reactor comprises a stirrer, a microwave waveguide, a microwave heating cavity and a heating device.

[0042] The production system of the regenerable defluorinating agent as described above, wherein the system further comprises a first regenerator and a second regenerator which are interconnected, wherein the first regenerator comprises a first circulation pump, and the second regenerator comprises a second circulation pump.

[0043] The preparation method of the renewable defluorinating agent provided by the invention utilizes wastewater sludge as a main raw material, has the characteristics of simple preparation process, and can produce a renewable defluorinating agent with good defluorination effect and high regeneration efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced one by one below. Obviously, the drawings in the following description are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0045] Figure 1 A structural diagram of the first renewable defluorination agent production system provided by the present invention;

[0046] Figure 2 A structural diagram of a reactor in the first regenerative defluorination agent production system provided by the present invention;

[0047] Figure 3 A structural diagram of a second renewable defluorination agent production system provided by the present invention;

[0048] Figure 4 This is a structural diagram of the regeneration device in the regenerable defluorination agent production system provided by the present invention.

[0049] Description of reference numerals:

[0050] A-desulfurization reactor;

[0051] B-acidification reactor;

[0052] C-leaching reactor;

[0053] D-membrane concentration device;

[0054] E-reactor;

[0055] E1-liquid feed port;

[0056] E2-feeding port;

[0057] E3-Microwave waveguide;

[0058] E4-microwave heating cavity;

[0059] E5-Agitator;

[0060] E6-Heating device;

[0061] E7-solenoid valve;

[0062] F-solid-liquid separator;

[0063] G-extractor;

[0064] H-Flash evaporator;

[0065] I-modification reactor;

[0066] J-first regenerator;

[0067] K- Second regenerator. DETAILED DESCRIPTION

[0068] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0069] The first aspect of the present invention protects a method for preparing a regenerable defluorinating agent, the method comprising the following steps:

[0070] 1) After the photovoltaic wastewater sludge is contacted with the sodium carbonate aqueous solution, the obtained mixed system is subjected to solid-liquid separation treatment to obtain solid A;

[0071] 2) After solid A is contacted with a hydrochloric acid solution, the obtained mixed system is subjected to a solid-liquid separation treatment to obtain solid B;

[0072] 3) contacting solid B with an aqueous sodium hydroxide solution, and performing solid-liquid separation treatment on the obtained mixed system to obtain high-purity calcium fluoride sludge and a sodium silicate aqueous solution;

[0073] 4) mixing the sodium silicate aqueous solution with aluminum hydroxide, zinc hydroxide and sodium hydroxide and stirring the mixture, mixing the obtained mixture with a template and heating the mixture to a first temperature to obtain a first temperature system;

[0074] 5) mixing the first temperature system with sodium bicarbonate and subjecting the mixture to a first microwave treatment, while simultaneously heating the mixture to a second temperature to obtain a second temperature system;

[0075] 6) performing a second microwave treatment on the second temperature system, and performing a solid-liquid separation treatment on the obtained second microwave system to obtain a regenerable defluorination agent matrix;

[0076] 7) contacting the regenerable defluorinating agent matrix with an aqueous solution including aluminum ions and iron ions to obtain a regenerated regenerable defluorinating agent;

[0077] Template agents include morpholine and isopropylamine;

[0078] The first temperature is 70~80℃, and the second temperature is 160~200℃;

[0079] In step 4), the molar ratio of sodium silicate, aluminum hydroxide, zinc hydroxide and sodium hydroxide is 1: (0.1-0.4): (0.01-0.05): (0.5-1.5).

[0080] The main components of photovoltaic wastewater calcium fluoride sludge are CaF2, SiO2, CaSO4, precipitant and flocculant. Contacting photovoltaic wastewater sludge with sodium carbonate aqueous solution can convert calcium sulfate in the sludge into calcium carbonate that is less soluble in water, thereby achieving the effect of removing sulfur in the sludge. The mixed system obtained after contacting photovoltaic wastewater sludge with sodium carbonate aqueous solution is subjected to solid-liquid separation treatment to obtain solid A.

[0081] Furthermore, solid A can be contacted with hydrochloric acid to dissolve calcium carbonate and calcium hydroxide in the solid, and the mixed system obtained by contacting solid A with hydrochloric acid is subjected to solid-liquid separation to obtain solid B without calcium carbonate.

[0082] Furthermore, contacting solid B with an aqueous sodium hydroxide solution can cause SiO2 contained in solid B to react with sodium hydroxide to generate water-soluble sodium silicate. At this time, in the mixed system formed by contacting solid B with an aqueous sodium hydroxide solution, the solid phase is calcium fluoride with a relatively high purity, and the liquid phase is a sodium silicate solution. The mixed system is subjected to a solid-liquid separation process to obtain a sodium silicate solution.

[0083] The present invention does not limit the concentrations of the sodium carbonate aqueous solution, hydrochloric acid, and sodium hydroxide aqueous solution, nor does it limit the contact time and contact temperature of the above-mentioned contact process, as long as the above-mentioned technical effects can be obtained.

[0084] Furthermore, the sodium silicate aqueous solution is mixed with aluminum hydroxide, zinc hydroxide and sodium hydroxide and stirred, the obtained mixed system is mixed with a template and heated to a first temperature to obtain a first temperature system; the first temperature system is mixed with sodium bicarbonate and subjected to a first microwave treatment, and the temperature is simultaneously raised to a second temperature to obtain a second temperature system; the second temperature system is subjected to a second microwave treatment, and the obtained second microwave system is subjected to a solid-liquid separation treatment to obtain a renewable defluorination agent matrix.

[0085] Among them, morpholine and isopropylamine as templates help the defluorination agent matrix to form a specific structure, so that the defluorination agent prepared has stronger F - The present invention does not limit the molar ratio of morpholine to isopropylamine. In one embodiment, the molar ratio of morpholine to isopropylamine is 1:4. The above molar ratio can make the defluorination agent have stronger F - Adsorption capacity.

[0086] The defluorination agent matrix has a structure similar to that of a molecular sieve. The use of microwave-assisted heating helps to improve the crystallinity and surface area of ​​the defluorination agent, accelerate the crystallization rate, and reduce energy consumption. The multi-step microwave heating method can further shorten the synthesis time to 1-3 hours by combining low-temperature activation and high-temperature crystallization, and rapidly grow into the target crystal, which is significantly improved compared to the time of traditional hydrothermal synthesis of molecular sieves. The use of aluminum hydroxide and zinc hydroxide can maintain the alkalinity of the reaction solution; zinc is introduced into the raw material so that zinc enters the molecular sieve framework under the action of microwaves and is confined in the framework cage, thereby increasing the ion exchange capacity of the molecular sieve and increasing its potential adsorption capacity; the addition of sodium bicarbonate can decompose to a certain extent in the formula of the present invention during microwave heating, release CO2 gas, increase the number of product structure channels and holes, and expand the specific surface area of ​​the molecular sieve.

[0087] In one embodiment, a certain amount of Al(OH)3 and Zn(OH)2, NaOH and Na2SiO3 solution can be mixed, stirred at 200~250rpm for 20min~90min at room temperature, and then a template is added. After stirring, the mixed system is heated to a first temperature, and then NaHCO3 is quickly added. The stirring speed is slowed down to 20~100rpm, and then a first microwave treatment and a second microwave treatment are sequentially performed. The obtained second microwave system is subjected to solid-liquid separation treatment to obtain a renewable defluorination agent matrix.

[0088] Furthermore, in one embodiment, in step 4), the molar ratio of sodium silicate, aluminum hydroxide, zinc hydroxide, and sodium hydroxide is 1: (0.1-0.4): (0.01-0.05): (0.5-1.5). A suitable raw material ratio can increase the ion exchange capacity of the molecular sieve, so that the regenerable defluorination agent obtained has a higher F - Adsorption capacity.

[0089] Furthermore, the regenerable defluorinating agent matrix is ​​contacted with an aqueous solution including aluminum ions and iron ions to obtain a regenerable defluorinating agent. The molecular sieve structure of the invention can adsorb F to a large extent. - , and can adsorb more modified metal ions, Al 3 + and Fe 3+ It is adsorbed in its holes and fixed on the skeleton, making it difficult to fall off.

[0090] The present invention does not limit the specific composition and concentration of the aqueous solution including aluminum ions and iron ions, and it only needs to include the above two metal ions. In one embodiment, the aqueous solution is an aqueous solution of Al2(SO4)3 and Fe2(SO4)3. The present invention also does not limit the contact time and contact temperature of the above contact process, and it is sufficient to 3+ and Fe 3+It only needs to be fixed on the defluorination agent matrix skeleton.

[0091] Furthermore, when the regenerable defluorination agent substrate is in contact with the aqueous solution including aluminum ions and iron ions, ultrasonic immersion and oscillation treatment can be performed simultaneously. 3+ and Fe 3+ Enters into and adsorbs into the pores of the defluorination agent matrix through ion exchange; Al 3+ and Fe 3+ The composite use of Al 3+ and Fe 3+ The complex formed during fluorine removal has a large specific surface area and is more effective for F - The coordination ability is stronger and the adsorption is greater, which can further improve the defluorination effect on the basis of the defluorination agent matrix. In one embodiment, the defluorination agent matrix is ​​put into Al2(SO4)3 and Fe2(SO4)3 solution, hydrochloric acid is added to adjust the pH to 2-3, ultrasonic oscillation is performed for 1-4 hours, and the product after oscillation is rinsed with distilled water until neutral, and vacuum dried at 80-150°C for 2-5 hours to obtain the target defluorination agent.

[0092] In one embodiment, the step 1 is further performed after the photovoltaic wastewater calcium fluoride sludge is finely dispersed by a ball mill). Dispersing the sludge can increase the sludge surface area, making subsequent treatment more efficient.

[0093] The preparation method of the renewable defluorinating agent provided by the present invention utilizes Na2CO3, hydrochloric acid and NaOH to purify photovoltaic wastewater sludge, which can avoid the entry of impurities when alkali solution leaches silicon element, and can obtain a sodium silicate solution with high purity, further prepare a defluorinating agent matrix, and can also improve the resource utilization rate of calcium fluoride sludge in the later stage. The method has the characteristics of simple preparation process, good defluorination effect and high regeneration efficiency.

[0094] In one embodiment, in step 1), the concentration of the sodium carbonate aqueous solution is 2.5-5 mol / L, the contact temperature of the photovoltaic wastewater sludge and the sodium carbonate aqueous solution is 50-80°C, and the contact time is 2-5 hours; and / or, in step 2), the concentration of the hydrochloric acid solution is 1.5-3.5 mol / L, the contact temperature of the solid A and the hydrochloric acid solution is 20-30°C, and the contact time is 0.5-1 hour; and / or, in step 3), the concentration of the sodium hydroxide aqueous solution is 10-25 mol / L, the contact temperature of the solid B and the sodium hydroxide aqueous solution is 80-150°C, and the contact time is 3-10 hours. The above solution concentration, contact temperature and contact time can improve the reaction rate and the purity of sodium silicate for silicon leaching of sludge in photovoltaic wastewater, so that the preparation method of the renewable defluorination agent provided by the present invention has higher efficiency.

[0095] The first microwave treatment has a processing power of 300W and a processing time of 10-40min; and / or the second microwave treatment has a processing power of 400W and a processing time of 30-120min. The above microwave treatment conditions are helpful to further improve the crystallinity and surface area of ​​the defluorinating agent, accelerate the crystallization speed, and make the prepared molecular sieve have better defluorination effect.

[0096] Furthermore, in one embodiment, step 3) further comprises concentrating the sodium silicate aqueous solution using a nanofiltration membrane to obtain a concentrated sodium silicate aqueous solution for use in step 4); the operating pressure of the concentration treatment is 0.8-1.4 MPa, and the operating temperature is 30-40°C.

[0097] In the prior art, conventional evaporation and concentration treatment is often used to concentrate the sodium silicate aqueous solution. During the evaporation and concentration process, Na2SiO3 is very easy to form a precipitate at high temperature, and the solution is turbid. Nanofiltration membrane concentration and water removal can not destroy the structure of Na2SiO3 in the solution, has a protective effect on the solution, and can avoid the denaturation and precipitation of Na2SiO3 in conventional evaporation and water removal. The present invention does not limit the mass fraction of sodium silicate in the concentrated sodium silicate aqueous solution. In one embodiment, the mass fraction of sodium silicate in the concentrated sodium silicate aqueous solution is 30~50wt%, and more preferably 30~35wt%. The concentrated sodium silicate aqueous solution with the above mass fraction can provide sufficient H2O amount during molecular sieve microwave crystallization, thereby improving the reaction efficiency.

[0098] In one embodiment, in an aqueous solution including aluminum ions and iron ions, the aluminum ion concentration is 0.3-1 mol / L, the iron ion concentration is 0.1-0.2 mol / L, and the hydrochloric acid concentration is 0.08-0.15 mol / L. The above solution has a suitable pH while including suitable aluminum ions and iron ions, which can increase the amount of metal loaded on the defluorinating agent matrix. Further, in one embodiment, in an aqueous solution including aluminum ions and iron ions, the Al2(SO4)3 solution concentration is 0.15-0.5 mol / L, the Fe2(SO4)3 solution concentration is 0.05-0.1 mol / L, the hydrochloric acid concentration is 0.08-0.15 mol / L, and the pH of the solution is 2-3.

[0099] Furthermore, in one embodiment, step 7) further comprises: drying the renewable defluorinating agent matrix at 400-450° C. for 1-3 hours and then mixing it with an aqueous solution comprising aluminum ions and iron ions, adding hydrochloric acid to the obtained mixed system to adjust the pH value of the mixed system to 2-3, and then subjecting the mixed system to ultrasonic oscillation treatment for 1-4 hours to obtain an ultrasonic oscillation treatment system; subjecting the ultrasonic oscillation treatment system to solid-liquid separation treatment, rinsing the obtained solid phase product with distilled water until the pH value of the washing solution obtained by rinsing is 7, and then vacuum drying the solid phase product at 80-150° C. for 2-5 hours to obtain a renewable defluorinating agent.

[0100] The template agent remaining in the renewable defluorinating agent matrix can be removed by drying the renewable defluorinating agent matrix at 400-450°C, and then the mixed system is subjected to ultrasonic oscillation treatment to enable aluminum ions and iron ions to have a better binding effect with the renewable defluorinating agent matrix, so that the renewable defluorinating agent prepared has a good defluorination effect.

[0101] Furthermore, in one embodiment, in step 5), the ratio of the amount of sodium bicarbonate to the sum of the amounts of aluminum hydroxide and zinc hydroxide is 0.05-0.08:1. A suitable raw material ratio can increase the ion exchange capacity of the molecular sieve, so that the regenerable defluorination agent obtained has a higher F - Furthermore, in one embodiment, controlling the ratio of the amount of the template substance to the sum of the amounts of the aluminum hydroxide and zinc hydroxide substances to 0.8 to 1.5:1 can make the obtained renewable defluorination agent have a higher F - Adsorption capacity.

[0102] In one embodiment, step 6) further includes using an organic solvent to perform solid-liquid separation on the obtained second microwave system to obtain a liquid product, extracting the liquid product to obtain a mixture including a template and an aqueous mixture; flashing the mixture including the template to obtain a template as a reaction raw material in step 4); mixing the aqueous mixture with the sodium hydroxide aqueous solution in step 3) as a reaction raw material. The liquid product contains a template. Extracting the template with an organic solvent can obtain an organic solvent solution of the template, that is, a mixture including the template. Flashing the mixture can separate the template from the organic solvent, and reusing the template as the reaction raw material in step 4) can improve the economy of the preparation method of the regenerable defluorination agent provided by the present invention.

[0103] The present invention does not limit the type of organic solvent, as long as it can play the role of separating the template agent. In one embodiment, the organic solvent is selected from at least one of dichloroethane, ethylene glycol dimethyl ether, ethyl acetate, and cyclohexane. The aqueous phase mixture contains sodium hydroxide, which is reused in step 3) to improve the economic efficiency of the preparation method of the regenerable defluorinating agent provided by the present invention.

[0104] The second aspect of the present invention provides a renewable defluorinating agent, which is prepared using any one of the preparation methods of the renewable defluorinating agent provided in the first aspect of the present invention. The renewable defluorinating agent provided by the present invention has the characteristics of good defluorination effect and high regeneration efficiency.

[0105] The third aspect of the present invention provides a defluorination method, which uses the renewable defluorinating agent provided by the second aspect of the present invention to contact the object to be treated containing fluoride ions to obtain a treated product and a fluorine-containing defluorinating agent. The present invention does not limit the specific composition of the object to be treated containing fluoride ions, as long as it meets the requirement of containing fluoride ions. The present invention also does not limit the contact time between the renewable defluorinating agent and the object to be treated containing fluoride ions, which can be determined according to actual needs. In one embodiment, the contact time between the renewable defluorinating agent and the object to be treated containing fluoride ions is not less than 2 hours.

[0106] Further, in one embodiment, the defluorination method provided by the present invention also includes sequentially subjecting the fluorine-containing defluorinating agent to acid treatment, alkali treatment, rinsing treatment and drying treatment to obtain a regenerated defluorinating agent. Wherein, the acid treatment includes contacting the fluorine-containing defluorinating agent with a hydrochloric acid solution, the concentration of the hydrochloric acid solution is 0.02~0.06mol / L, and the contact time is 1~3h to obtain an acid-treated product; the alkali treatment includes contacting the acid-treated product with a sodium hydroxide aqueous solution, the concentration of the sodium hydroxide aqueous solution is 0.04~0.08mol / L, and the contact time is 2~6h to obtain an alkali-treated product; the rinsing treatment includes rinsing the alkali-treated product with distilled water until the pH value of the washing solution obtained by rinsing is 7 to obtain a rinse product; the drying treatment includes vacuum drying the rinse product at 100~180℃ for 2~5h to obtain a regenerated defluorinating agent. The sequential acid treatment and alkali treatment of the fluorine-containing defluorinating agent can separate the fluorine ions adsorbed in the fluorine-containing defluorinating agent, so that the obtained regenerated defluorinating agent has the function of adsorbing fluorine ions again.

[0107] The fourth aspect of the present invention provides a regenerative defluorinating agent production system, which is used to implement the preparation method of the regenerative defluorinating agent provided in the first aspect of the present invention. Figure 1 The structural diagram of the first regeneration defluorination agent production system provided by the present invention is as follows: Figure 1As shown, the system includes A-desulfurization reactor, acidification reactor, C-leaching reactor, D-membrane concentrating device, and E-reactor, wherein the logistics outlet of A-desulfurization reactor is connected with the logistics inlet of B-acidification reactor, the logistics outlet of B-acidification reactor is connected with the logistics inlet of C-leaching reactor, the logistics outlet of C-leaching reactor is connected with the logistics inlet of D-membrane concentrating device, and the logistics outlet of D-membrane concentrating device is connected with E1-liquid feed port of E-reactor.

[0108] Among them, A-desulfurization reactor is used to contact photovoltaic wastewater sludge with sodium carbonate aqueous solution and then perform solid-liquid separation treatment to obtain solid A; B-acidification reactor is used to contact solid A with hydrochloric acid solution and then perform solid-liquid separation treatment to obtain solid B; C-leaching reactor is used to contact solid B with sodium hydroxide aqueous solution and then perform solid-liquid separation treatment to obtain high-purity calcium fluoride sludge and sodium silicate aqueous solution; E-reactor is used to perform steps 4) to 6) of the method for preparing a renewable defluoridating agent provided in the first aspect of the present invention.

[0109] Further, Figure 2 The structural diagram of the E-reactor in the first regenerative defluorination agent production system provided by the present invention is as follows: Figure 2 As shown, the reactor includes E1-liquid feed port, E2-feeding port, E3-microwave waveguide device, E4-microwave heating cavity, E5-agitator, E6-heating device, and E7-solenoid valve. Among them, E1-liquid feed port is used for Na2SiO3 solution feeding, and E2-feeding port is used for solid material E2-feeding port; the bottom of the E-reactor is conical and a discharge port is provided, and the discharge port is controlled by E7-solenoid valve, and the conical structure is conducive to the outflow of materials after the reaction. E3-microwave waveguide device is provided in the cylinder of the E-reactor, and E3-microwave waveguide device is provided with a power regulator; E6-heating device is provided in the cone at the bottom of the E-reactor; E3-microwave waveguide heating and E6-heating device are combined, and microwave power and material heating temperature can be adjusted. E5-agitator is fixed above the E-reactor and extends to the bottom conical area to ensure that the material can be evenly stirred. Furthermore, E7-solenoid valve control facilitates discharge, and can realize the continuous preparation of the defluorination agent matrix.

[0110] Further, Figure 3 The system diagram of the second renewable defluorination agent production system provided by the present invention is as follows: Figure 3As shown, the system also includes F-solid-liquid separator, G-extractor, H-flash evaporator, and I-modification reactor. Among them, the F-solid-liquid separator is connected to the logistics outlet (i.e., bottom solenoid valve) of the E-reactor, the solid phase outlet of the F-solid-liquid separator is connected to the I-modification reactor, the liquid phase outlet of the F-solid-liquid separator is connected to the G-extractor, the water phase mixture outlet of the G-extractor is connected to the logistics inlet of the C-leaching reactor, the mixture outlet including the template agent of the G-extractor is connected to the H-flash evaporator, and the template agent outlet of the H-flash evaporator is connected to the E2-feeding port of the E5-agitator.

[0111] I-modified reactor is used to perform step 7 of the method for preparing a regenerable defluorinating agent provided in the first aspect of the present invention, G-extractor uses an organic solvent to extract the template in the mixture including the template, and H-flash evaporator evaporates the template by flash evaporation and returns it to E-reactor.

[0112] Figure 4 The structure diagram of the regeneration device in the regenerable defluorination agent production system provided by the present invention is shown in FIG. Figure 4 As shown, the regenerable defluorinating agent production system provided by the present invention also includes a regeneration device for regenerating the fluorine-containing defluorinating agent. The regeneration device includes a J-first regenerator and a K-second regenerator that are interconnected, the J-first regenerator includes a first circulation pump, and the K-second regenerator includes a second circulation pump.

[0113] The J-first regenerator and the K-second regenerator are cylindrical and are used to regenerate the fluorine-containing defluorinating agent. Specifically, the fluorine-containing defluorinating agent enters the J-first regenerator, which includes a hydrochloric acid solution with a concentration of 0.02-0.06 mol / L, and also includes a first circulation pump, which is used to circulate and rinse the hydrochloric acid solution in the J-first regenerator, so that it can fully contact with the fluorine-containing defluorinating agent, shorten the regeneration time, and obtain an acid-treated product.

[0114] Furthermore, the acid-treated product enters the K-second regenerator. The K-second regenerator contains a sodium hydroxide aqueous solution with a concentration of 0.04-0.08 mol / L, and also includes a second circulation pump, which is used to circulate and rinse the sodium hydroxide aqueous solution in the K-second regenerator so that it can fully contact with the acid-treated product, shorten the regeneration time, and obtain an alkali-treated product.

[0115] Furthermore, the alkali-treated product is rinsed and dried in sequence to obtain a regenerated defluorinating agent, which can be used again as a raw material in the defluorinating method provided by the present invention.

[0116] The present invention does not limit Figure 4 The regeneration device and Figure 3The connection relationship of other equipment in the renewable defluorination agent production system shown in the figure, in one embodiment, Figure 4 The regeneration device shown can be independent of Figure 3 The other equipment of the regenerable defluorination agent production system shown is set separately. Figure 3 The renewable defluoridation agent produced by the equipment shown in the figure can be used to absorb fluoride ions to become a fluorine-containing defluoridation agent. Figure 4 The regeneration device shown is used for regeneration to obtain a regenerated defluorinating agent.

[0117] The preparation method of the regenerable defluorination agent provided by the present invention is described below in conjunction with the embodiments: Example 1

[0118] This embodiment adopts the following steps to prepare the regenerable defluorination agent:

[0119] 1) After the photovoltaic wastewater calcium fluoride sludge is finely dispersed by a ball mill, 50 kg is added to the A-desulfurization reactor, and 80 L of 3.0 mol / L Na2CO3 solution is added to mix and stir, heated to 60 ° C, reacted for 2 hours, and solid A is separated;

[0120] 2) Solid A is transported to a B-acidification reactor containing 80 L of hydrochloric acid with a concentration of 2 mol / L, heated to 25°C, and reacted for 0.5 h to obtain solid B by solid-liquid separation;

[0121] 3) Solid B is transported to the C-leaching reactor without washing and drying. The C-leaching reactor includes 80L of NaOH aqueous solution, the concentration of NaOH aqueous solution is 15mol / L, the leaching temperature is 120℃, the leaching time is 6h, the reacted materials are separated into solid and liquid, and the Na2SiO3 filtrate is filtered; the Na2SiO3 solution filtrate is concentrated to a concentration of 35% through a nanofiltration membrane and transferred to a microwave heating reactor. The nanofiltration membrane concentration operating pressure is 0.9MPa and the operating temperature is 30℃.

[0122] 4) According to the amount of 35% Na2SiO3 solution added, Al(OH)3, Zn(OH)2 and additional NaOH are added at a molar ratio of Na2SiO3:Al(OH)3:Zn(OH)2:NaOH of 1:0.2:0.04:1.1, and the stirring speed is 200 rpm at room temperature. After stirring for 30 minutes, the template agents morpholine and isopropylamine are added, and the molar ratio of morpholine and isopropylamine is 1:4, and the molar ratio of template agent: (Al(OH)3+Zn(OH)2) is 0.9:1; after stirring and dispersing, the temperature is raised to 70°C to obtain the first temperature system;

[0123] 5) The stirring speed was slowed down to 30 rpm, and NaHCO3 was quickly added, and the molar ratio of NaHCO3 to the sum of the amounts of Al(OH)3 and Zn(OH)2 was 0.06:1. The microwave reactor was turned on for the first microwave treatment, and the microwave reaction was carried out at a power of 300 W for 20 min, and the temperature was raised to 180°C to obtain the second temperature system;

[0124] 6) performing a second microwave treatment on the second temperature system, specifically, performing a microwave reaction at a power of 400 W for 80 min, opening the E7-solenoid valve at the lower end of the reactor, and using a solid-liquid separation device to perform solid-liquid separation on the reactants, and the obtained solid is the regenerable defluorination agent matrix;

[0125] 7) Dry the defluorinating agent matrix in a resistance furnace drying system at 400°C for 2 h, put the defluorinating agent matrix into 0.2 mol / L Al2(SO4)3 and 0.07 mol / L Fe2(SO4)3 solutions, add 0.08 mol / L hydrochloric acid to adjust the pH to 2, and soak the product after ultrasonic oscillation for 2 h, rinse it with distilled water until it is neutral, and vacuum dry it at 100°C for 3 h to obtain regenerable defluorinating agent A1. Example 2

[0126] This embodiment is basically the same as embodiment 1, except that in step 1), the contact time between the sludge and the sodium carbonate solution is 4 hours, and a regenerable defluorinating agent A2 is obtained. Example 3

[0127] This embodiment is basically the same as embodiment 1, except that in step 3), the leaching temperature is 80° C., the leaching time is 8 h, and a regenerable defluorinating agent A3 is obtained. Example 4

[0128] This embodiment is basically the same as embodiment 1, except that in step 4), Al(OH)3, Zn(OH)2 and additional NaOH are added in a molar ratio of Na2SiO3:Al(OH)3:Zn(OH)2:NaOH of 1:0.3:0.02:0.8 to obtain a regenerable defluorinating agent A4. Example 5

[0129] This embodiment is basically the same as embodiment 1, except that in step 5), the treatment time of the first microwave treatment is 30 minutes to obtain a regenerable defluorinating agent A5. Example 6

[0130] This embodiment is basically the same as Embodiment 1, except that, in step 6), the treatment time of the second microwave treatment is 120 min, and a regenerable defluorinating agent A6 is obtained. Example 7

[0131] This embodiment is basically the same as embodiment 1, except that in step 2), the Na2SiO3 solution is concentrated to the same concentration using conventional evaporation concentration treatment to obtain a regenerable defluorinating agent A7. Example 8

[0132] This embodiment is basically the same as embodiment 1, except that in step 2), Al(OH)3, Zn(OH)2 and additional NaOH are added in a molar ratio of Na2SiO3:Al(OH)3:Zn(OH)2:NaOH of 1:0.05:0.1:0.8 to obtain a regenerable defluorinating agent A8. Example 9

[0133] This embodiment is basically the same as embodiment 1, except that in step 5), the treatment time of the first microwave treatment is 5 minutes to obtain a regenerable defluorinating agent A9. Example 10

[0134] This embodiment is basically the same as Embodiment 1, except that, in step 5), the treatment time of the second microwave treatment is 10 min, and a regenerable defluorinating agent A10 is obtained.

[0135] Comparative Example 1

[0136] This comparative example is basically the same as Example 1, except that the first microwave treatment and the second microwave treatment are not performed in step 5) and step 6), to obtain a regenerable defluorination agent B1.

[0137] Comparative Example 2

[0138] This comparative example is basically the same as Example 1, except that no Al(OH)3 is added in step 4), and a regenerable defluorinating agent B2 is obtained.

[0139] Comparative Example 3

[0140] This comparative example is basically the same as Example 1, except that no Zn(OH)2 is added in step 4), and a regenerable defluorinating agent B3 is obtained.

[0141] Comparative Example 4

[0142] This comparative example is basically the same as Example 1, except that the solution in step 7) does not contain Al2(SO4)3, and a regenerable defluorinating agent B4 is obtained.

[0143] Comparative Example 5

[0144] This comparative example is basically the same as Example 1, except that the solution in step 7) does not contain Fe2(SO4)3, and a regenerable defluorinating agent B5 is obtained.

[0145] Comparative Example 6

[0146] This comparative example is basically the same as Example 1, except that in step 5), the temperature is raised to 120° C. to obtain a regenerable defluorinating agent B6.

[0147] Comparative Example 7

[0148] This comparative example is basically the same as Example 1, except that in step 4), the temperature is raised to 50° C. to obtain a regenerable defluorinating agent B7.

[0149] Comparative Example 8

[0150] This comparative example is basically the same as Example 1, except that the template agent is replaced with polyethylene glycol of the same amount of substance to obtain a regenerable defluorinating agent B8.

[0151] Test example

[0152] 1. The fluorine removal rate, primary regeneration efficiency and secondary regeneration efficiency of each regenerable defluorinating agent sample were tested. The test results are shown in Table 1.

[0153] Among them, the test method for fluorine removal rate is as follows:

[0154] Take 50mL of a solution with a fluoride ion concentration of 10.00mg / L (for example, sodium fluoride aqueous solution can be used), adjust the pH value of the solution to 6.0 with hydrochloric acid and sodium hydroxide aqueous solution, weigh 0.5g of the regenerable defluoridation agent sample, add it to the fluoride solution and shake for two hours. Use a fluoride ion concentration meter to measure the residual fluoride ion concentration of the solution.

[0155] For example, in one embodiment, the residual fluoride ion concentration is 0.82 mg / L, and the fluoride removal rate of the regenerable defluorinating agent is 91.8%, corresponding to a fluoride adsorption amount of 0.918 mg / g.

[0156] The regeneration method is as follows: the defluorinating agent after defluorination is treated in the J-first regenerator and the K-second regenerator in turn, the hydrochloric acid concentration in the J-first regenerator is 0.03 mol / L, and the treatment time is 2 hours; the sodium hydroxide aqueous solution concentration in the K-second regenerator is 0.06 mol / L, and the treatment time is 4 hours; after reaching the regeneration time, the defluorinating agent is rinsed with distilled water until it is neutral, and vacuum dried at 100°C for 3 hours to obtain a once-regenerated defluorinating agent.

[0157] The test method for primary regeneration efficiency is as follows:

[0158] Take 50mL of a solution with a fluoride ion concentration of 10mg / L (for example, sodium fluoride aqueous solution can be used), adjust the pH value of the solution to 6.0 with hydrochloric acid and sodium hydroxide aqueous solution, weigh 0.5g of the primary regeneration defluoridation agent sample and add it to the fluoride solution for two hours of shaking. Use a fluoride ion concentration meter to measure the residual fluoride ion concentration of the solution and calculate the primary regeneration efficiency.

[0159] For example, in one embodiment, the residual fluoride ion concentration is 1.73 mg / L, and the fluoride adsorption capacity of the defluoridation agent in one regeneration is 0.827 mg / g. The fluoride adsorption capacity of the defluoridation agent before the first regeneration is 0.918 mg / g, and the regeneration efficiency is 90.1%.

[0160] The test method for secondary regeneration efficiency is as follows:

[0161] The fluorine-containing primary regenerated defluorinating agent having a fluorine adsorption capacity of 0.827 mg / g is subjected to a second regeneration treatment according to the above method to obtain a secondary regenerated defluorinating agent;

[0162] Take 50mL of a solution with a fluoride ion concentration of 10mg / L (for example, sodium fluoride aqueous solution can be used), adjust the pH value of the solution to 6.0 with hydrochloric acid and sodium hydroxide aqueous solution, weigh 0.5g of secondary regeneration defluoridation agent sample, add it to the fluoride solution and shake for two hours. Use a fluoride ion concentration meter to measure the residual fluoride ion concentration of the solution and calculate the secondary regeneration efficiency.

[0163] In one embodiment, the residual fluoride ion concentration is 3.54 mg / L, and the fluoride adsorption capacity of the secondary regenerated defluorinating agent obtained after the secondary regeneration is 0.646 mg / g. The fluoride adsorption capacity before the first regeneration is 0.918 mg / g, and the secondary regeneration efficiency is 70.4%.

[0164] Table 1- Fluoride removal agent test data

[0165] It can be seen from Table 1 that compared with the defluorinating agents B1-B8 prepared in each comparative example, the defluorinating agents A1-A10 have higher defluorinating rates, primary regeneration efficiencies, and secondary regeneration efficiencies.

[0166] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some or all of the technical features can be replaced by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a renewable defluorination agent, It is characterized in that The steps include: 1) contacting photovoltaic wastewater sludge with a sodium carbonate aqueous solution, and performing solid-liquid separation treatment on the obtained mixed system to obtain solid A; 2) contacting the solid A with a hydrochloric acid solution, and performing solid-liquid separation on the obtained mixed system to obtain a solid B; 3) contacting the solid B with a sodium hydroxide aqueous solution, and performing solid-liquid separation treatment on the obtained mixed system to obtain calcium fluoride sludge and a sodium silicate aqueous solution; 4) mixing the sodium silicate aqueous solution with aluminum hydroxide, zinc hydroxide and sodium hydroxide and stirring the mixture, mixing the obtained mixed system with a template and heating the mixture to a first temperature to obtain a first temperature system; 5) mixing the first temperature system with sodium bicarbonate and subjecting the mixture to a first microwave treatment, while simultaneously heating the mixture to a second temperature to obtain a second temperature system; 6) performing a second microwave treatment on the second temperature system, and performing a solid-liquid separation treatment on the obtained second microwave system to obtain a liquid phase product and a regenerable defluorination agent matrix; 7) contacting the regenerable defluorinating agent matrix with an aqueous solution comprising aluminum ions and iron ions to obtain the regenerated regenerable defluorinating agent; The template agent includes morpholine and isopropylamine; The first temperature is 70-80°C, and the second temperature is 160-200°C; In step 4), the molar ratio of the sodium silicate, the aluminum hydroxide, the zinc hydroxide and the sodium hydroxide is 1: (0.1-0.4): (0.01-0.05): (0.5-1.5).

2. The method for preparing the renewable defluorination agent according to claim 1, It is characterized in that In step 1), the concentration of the sodium carbonate aqueous solution is 2.5-5 mol / L, the contact temperature of the photovoltaic wastewater sludge and the sodium carbonate aqueous solution is 50-80° C., and the contact time is 2-5 h; and / or, In step 2), the concentration of the hydrochloric acid solution is 1.5-3.5 mol / L, the contact temperature of the solid A and the hydrochloric acid solution is 20-30° C., and the contact time is 0.5-1 h; and / or, In step 3), the concentration of the sodium hydroxide aqueous solution is 10-25 mol / L, the contact temperature of the solid B and the sodium hydroxide aqueous solution is 80-150° C., and the contact time is 3-10 h.

3. The method for preparing the renewable defluorination agent according to claim 2, It is characterized in that The first microwave treatment has a processing power of 300W and a processing time of 10 to 40 minutes; and / or; The second microwave treatment has a processing power of 400W and a processing time of 30 to 120min; and / or, Step 3) further comprises using a nanofiltration membrane to concentrate the sodium silicate aqueous solution to obtain a concentrated sodium silicate aqueous solution as a reaction raw material in step 4); The operating pressure of the concentration treatment is 0.8~1.4MPa, and the operating temperature is 30~40℃.

4. The method for preparing the renewable defluorination agent according to claim 3, It is characterized in that In the aqueous solution comprising aluminum ions and iron ions, the concentration of aluminum ions is 0.3-1 mol / L, and the concentration of iron ions is 0.1-0.2 mol / L; and / or, Step 7) further comprises: drying the renewable defluorinating agent matrix at 400-450° C. for 1-3 hours, mixing it with the aqueous solution comprising aluminum ions and iron ions, adding hydrochloric acid to the obtained mixed system to adjust the pH value of the mixed system to 2-3, and then subjecting the mixed system to ultrasonic oscillation treatment for 1-4 hours to obtain an ultrasonic oscillation treatment system; subjecting the ultrasonic oscillation treatment system to solid-liquid separation treatment, washing the obtained solid phase product with distilled water until the pH value of the washing liquid obtained by washing is 7, and then vacuum drying the solid phase product at 80-150° C. for 2-5 hours to obtain the renewable defluorinating agent; and / or, In step 5), the ratio of the amount of the sodium bicarbonate substance to the sum of the amounts of the aluminum hydroxide and the zinc hydroxide substance is (0.05-0.08): 1; and / or, The ratio of the amount of the template substance to the sum of the amounts of the aluminum hydroxide and the zinc hydroxide substances is 0.8-1.5:

1.

5. The method for preparing the renewable defluorination agent according to claim 4, It is characterized in that Step 6) further comprises extracting the liquid phase product with an organic solvent to obtain a mixture including a template and an aqueous phase mixture; Flash evaporating the mixture including the template to obtain the template as a reaction raw material in step 4); The aqueous phase mixture is mixed with the sodium hydroxide aqueous solution in step 3) as a reaction raw material.

6. A renewable defluorination agent, It is characterized in that The invention is prepared by the preparation method of the regenerable defluorination agent according to any one of claims 1 to 5.

7. A method for removing fluorine, It is characterized in that The regenerable defluorinating agent according to claim 6 is used to contact the object to be treated containing fluoride ions to obtain a treated product and a fluorine-containing defluorinating agent.

8. The defluorination method according to claim 7, It is characterized in that The method further comprises sequentially subjecting the fluorine-containing defluorinating agent to an acid treatment, an alkali treatment, a rinsing treatment and a drying treatment to obtain a regenerated defluorinating agent; The acid treatment comprises contacting the fluorine-containing defluorinating agent with a hydrochloric acid solution, wherein the concentration of the hydrochloric acid solution is 0.02-0.06 mol / L, and the contact time is 1-3 hours, to obtain an acid-treated product; The alkali treatment comprises contacting the acid-treated product with an aqueous sodium hydroxide solution, wherein the concentration of the aqueous sodium hydroxide solution is 0.04 to 0.08 mol / L, and the contact time is 2 to 6 hours, to obtain an alkali-treated product; The rinsing treatment includes rinsing the alkali-treated product with distilled water until the pH value of the washing solution obtained by rinsing is 7, thereby obtaining a rinsed product; The drying treatment includes vacuum drying the flushing product at 100-180° C. for 2-5 hours to obtain the regenerated defluorination agent.

9. A production system for a renewable defluorinating agent for carrying out the preparation method of the renewable defluorinating agent according to any one of claims 1 to 5, It is characterized in that The production system of the renewable defluorinating agent comprises a desulfurization reactor, an acidification reactor, a leaching reactor, a membrane concentration device, and a reactor for performing steps 4) to 6) of the method for preparing the renewable defluorinating agent provided in any one of claims 1 to 5, which are connected in sequence; The reactor used to perform steps 4) to 6) of the method for preparing a regenerable defluorinating agent provided in any one of claims 1 to 5 comprises a stirrer, a microwave waveguide, a microwave heating cavity, and a heating device.

10. The production system of the renewable defluorination agent according to claim 9, It is characterized in that The invention also includes a first regenerator and a second regenerator which are interconnected. The first regenerator includes a first circulation pump, and the second regenerator includes a second circulation pump.