Oil-based drilling fluid and preparation method thereof

By using amino acids to modify polyurethane and silicon to modify carbon nanotubes in oil-based drilling fluid, organic-inorganic composite particles are formed, which solves the problems of instability of the well wall and high filtration loss under high temperature and high pressure conditions, and achieves better Blocking performance and thermal stability.

CN118599504BActive Publication Date: 2024-12-03SHANDONG DESHUNYUAN PETROLEUM SCI&TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077115.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-03
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing oil-based drilling fluid cannot effectively seal the cracks in the well wall under high temperature and high pressure conditions, resulting in unstable well walls and high filtration loss, affecting the drilling effect.

Method used

Oil-based drilling fluids using amino acids to modify polyurethane and silicon-modified carbon nanotubes are prepared by calcium carbonate modification and esterification reactions to form organic-inorganic composite particles, enhancing the well wall sealing ability and filtration loss reduction effect.

Benefits of technology

The well wall stability and sealing performance are significantly improved at high temperatures, the filtration loss is reduced, the rheology and thermal stability of the drilling fluid are maintained, and the service life of the drilling fluid is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of petrochemical industry, and discloses an oil-based drilling fluid and a preparation method thereof. The invention provides an oil-based drilling fluid by adding amino acid modified polyurethane, silicon modified carbon nanotubes, white oil, calcium chloride solution, Tween 20 emulsifier, phosphate wetting agent, and oxidized asphalt into a stirrer and stirring. In the drilling process, calcium carbonate in amino acid modified polyurethane can enter the fractured stratum, effectively plug the fractures, maintain the stability of the well wall, and calcium carbonate can reduce the filtration loss of the drilling fluid; the polyurethane absorbs water and expands underground to form a high-strength elastic body, which enters the fractures in the well wall, thereby achieving the effect of plugging. The carbon nanotubes also have good plugging and filtration loss reduction effects, and the synergistic effect enables the drilling fluid to maintain good stability at high temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of petrochemical engineering, in particular to an oil-based drilling fluid and a preparation method thereof. Background Art

[0002] With the development of deep-layer oil and gas exploration, the probability of encountering high-temperature and high-pressure formations is gradually increasing, which puts higher requirements on drilling fluids. Oil-based drilling fluids have the advantages of good salt resistance, lubricity, and high temperature resistance, but they are expensive, and leakage will damage the formation, making it impossible to continue drilling. How to avoid this phenomenon is the key to solving the problem. For example, CN10419750A discloses a nano-plugging agent for oil-based drilling fluids and a preparation method thereof. The nano-plugging agent for oil-based drilling fluids provided by the invention can effectively plug nano-scale micro-cracks and solve the problem of easy collapse of the well wall of shale gas wells, but it is only applicable within 150°C, and it is not known whether it can be applied at temperatures above 150°C. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides an oil-based drilling fluid and a preparation method thereof, which improves the stability of the well wall, has good plugging properties, and reduces filtration loss.

[0005] (II) Technical solution

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: an oil-based drilling fluid, comprising the following components by weight: 5-8 parts by weight of amino acid-modified polyurethane, 6-10 parts by weight of silicon-modified carbon nanotubes, 3-6 parts by weight of hydroxylated boron nitride, 60-80 parts by weight of white oil, 2-4 parts by weight of calcium chloride solution, 1-3 parts by weight of Tween 20 emulsifier, 2-3 parts by weight of phosphate wetting agent, and 2-3 parts by weight of oxidized asphalt.

[0007] Preferably, the preparation method of the amino acid modified polyurethane is:

[0008] (1) adding 2-4 parts by weight of calcium carbonate to deionized water, stirring to dissolve, and then adding 0.3-0.4 parts by weight of L-histidine, reacting at 65-70° C. for 50-70 min, filtering after reaction, and drying the filter cake in an oven at 75-90° C. for 5-7 h, to obtain L-histidine-modified calcium carbonate nanoparticles;

[0009] (2) 8-12 parts by weight of hexamethylene diisocyanate and 5-7 parts by weight of 1,4-butanediol are added to anhydrous tetrahydrofuran solvent, stirred at a constant speed for 20-35 minutes, and then 3-4 parts by weight of L-histidine-modified calcium carbonate nanospheres and 0.2-0.3 parts by weight of dibutyltin dilaurate catalyst are added, and heated and stirred at 45-70° C. for 2-4 hours. After the reaction is completed, the mixture is cooled to room temperature, washed with methanol for 2-4 times, and vacuum dried at 50-60° C. for 22-25 hours to obtain amino acid-modified polyurethane.

[0010] Preferably, the preparation method of the silicon-modified carbon nanotubes is:

[0011] S1. Add di(dimethylamino)methylvinylsilane and chloroacetic acid to N,N-dimethylformamide solvent, stir to dissolve, react at 90-110°C for 8-12h, remove the solvent by distillation under reduced pressure, filter and dry to obtain intermediate 1;

[0012] S2. Add intermediate 1 and glycidol to acetone solvent, stir evenly, then continue to add p-toluenesulfonic acid catalyst to carry out esterification reaction, react at 95-120° C. for 8-14 hours, cool to room temperature after completion, wash, filter, and dry to obtain intermediate 2;

[0013] S3. Add 1-2 parts by weight of sodium dodecyl sulfate emulsifier and 4-6 parts by weight of vinyl carbon nanotubes into deionized water, disperse them evenly, add 5-10 parts by weight of intermediate 2, 4-7 parts by weight of methyl acrylate and 8-12 parts by weight of allyltrimethylammonium chloride, introduce nitrogen protection, and then continue to add 0.8-1 parts by weight of azobisisobutyronitrile initiator, react at 90-110°C, wash with deionized water and ethanol in turn, and dry to obtain silicon-modified carbon nanotubes.

[0014] Preferably, the mass ratio of di(dimethylamino)methylvinylsilane to chloroacetic acid in S1 is 1:1.2-1.6.

[0015] Preferably, the mass ratio of the intermediate 1, glycidol and p-toluenesulfonic acid catalyst in S2 is 1:1.4-1.8:0.01-0.03.

[0016] Preferably, the reaction time in S3 is 4-10 h.

[0017] Preferably, the preparation method of the oil-based drilling fluid is: adding amino acid-modified polyurethane, silicon-modified carbon nanotubes, hydroxylated boron nitride, white oil, calcium chloride solution, Tween 20 emulsifier, phosphate wetting agent, and oxidized asphalt into a stirrer, stirring for 10-15 minutes, and obtaining the oil-based drilling fluid.

[0018] 3. Beneficial technical effects

[0019] The invention prepares oil-based drilling fluid by adding amino acid-modified polyurethane, silicon-modified carbon nanotubes, white oil, calcium chloride solution, Tween 20 emulsifier, phosphate wetting agent and oxidized asphalt into a stirrer and stirring.

[0020] Calcium carbonate and L-histidine are reacted to obtain L-histidine modified calcium carbonate nanospheres; the isocyanate group in hexamethylene diisocyanate and the hydroxyl group in 1,4-butanediol are reacted, stirred at a uniform speed, and then L-histidine modified calcium carbonate nanosphere chain extender and dibutyltin dilaurate catalyst are added to react to obtain amino acid modified polyurethane; the tertiary amine group in di(dimethylamino)methylvinylsilane and the chlorine group in chloroacetic acid are reacted to generate a quaternary ammonium salt group, and an olefin group and a carboxyl group are introduced to obtain intermediate 1, the carboxyl group in intermediate 1 and the hydroxyl group in glycidol are esterified to obtain intermediate 2, and sodium dodecyl sulfate emulsifier and vinyl carbon nanotubes, intermediate 2, methyl acrylate, and allyltrimethylammonium chloride are reacted under the action of azobisisobutyronitrile initiator to obtain silicon modified carbon nanotubes.

[0021] During the drilling process, the calcium carbonate in the amino acid modified polyurethane can enter the fractured formation, effectively seal the fractures and maintain the stability of the well wall. At the same time, the calcium carbonate can reduce the filtration loss of the drilling fluid. The polyurethane therein absorbs water and expands underground to form a high-strength elastic body, which enters the cracks in the well wall, thereby achieving a sealing effect. At the same time, the polyurethane will form an organic-inorganic composite particle filtration reducer with the carbon nanotubes in the silicon-modified carbon nanotubes. The flexibility of the polyurethane is conducive to entering the pores in the filter cake under a pressure difference, thereby maintaining the stability of the drilling fluid. The carbon nanotubes also have good sealing and filtration loss reduction effects, and the synergistic effect enables the drilling fluid to maintain good stability at high temperatures. DETAILED DESCRIPTION

[0022] Preparation of calcium carbonate: refer to the literature "High-temperature resistant calcium carbonate-polyurethane core-shell microsphere well wall strengthener for oil-based drilling fluid" ("Oilfield Chemistry" Vol. 41, No. 2). Take 1.11 g of calcium chloride and dissolve it in 100 mL of deionized water. Stir ultrasonically, add 2.4732 g of boric acid to the calcium chloride solution, and stir and mix in a three-necked flask; then take 5 mL of sodium carbonate solution (0.2 mol / L) and slowly add it dropwise to the above mixed solution, and react at 50°C for 1 hour; the solution after the reaction is aged at room temperature for 1 hour, filtered, and the filter cake is dried in an oven at 105°C for 5 hours. The dry white powder is calcium carbonate.

[0023] The preparation process of vinyl carbon nanotubes refers to the journal "Materials Science and Engineering Plastics", Volume 23, Issue 4, "Surface Vinyl Functionalization of Multi-walled Carbon Nanotubes": 0.3g of multi-walled carbon nanotubes were added to 30mL of 98% concentrated sulfuric acid and 10mL of 70% concentrated nitric acid, refluxed at 140°C for 1h, filtered, and washed. 0.1g of the acidified carbon nanotubes obtained were weighed and dispersed in 15mL of acetone and 15mL of chloroform, 2mL of triethylamine and 5mL of acryloyl chloride were added, and the reaction was carried out at 40°C for 24h. Then 10mL of ethanol was added and stirred for 2h, filtered, and washed to obtain vinyl carbon nanotubes. Example 1

[0024] (1) 2 parts by weight of calcium carbonate was added to deionized water, stirred to dissolve, and 0.3 parts by weight of L-histidine was added thereto, and the reaction was carried out at 65° C. for 50 min. After the reaction was completed, the mixture was filtered and the filter cake was dried in an oven at 75° C. for 5 h. After the reaction was completed, L-histidine-modified calcium carbonate nanoparticles were obtained.

[0025] (2) 8 parts by weight of hexamethylene diisocyanate and 5 parts by weight of 1,4-butanediol were added to anhydrous tetrahydrofuran solvent, stirred at a constant speed for 20 minutes, and then 3 parts by weight of L-histidine-modified calcium carbonate nanospheres and 0.2 parts by weight of dibutyltin dilaurate catalyst were added, heated and stirred at 45°C for 2 hours. After the reaction was completed, the mixture was cooled to room temperature, washed twice with methanol, and vacuum dried at 50°C for 22 hours to obtain amino acid-modified polyurethane;

[0026] (3) Add di(dimethylamino)methylvinylsilane and chloroacetic acid to N,N-dimethylformamide solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to chloroacetic acid is 1:1.2, stir to dissolve, react at 90°C for 8h, and then remove the solvent by distillation under reduced pressure, filter and dry to obtain intermediate 1;

[0027] (4) adding intermediate 1 and glycidol to an acetone solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of intermediate 1, glycidol, and p-toluenesulfonic acid catalyst is 1:1.4:0.01, and carrying out esterification reaction at 95°C for 8h. After completion, cooling to room temperature, washing, filtering, and drying to obtain intermediate 2;

[0028] (5) 1 part by weight of sodium dodecyl sulfate emulsifier and 4 parts by weight of vinyl carbon nanotubes were added to deionized water, and after being evenly dispersed, 5 parts by weight of intermediate 2, 4 parts by weight of methyl acrylate, and 8 parts by weight of allyltrimethylammonium chloride were added, and nitrogen was introduced for protection. Then, 0.8 parts by weight of azobisisobutyronitrile initiator was added, and the mixture was reacted at 90° C. for 4 hours. The mixture was washed with deionized water and ethanol in turn, and dried to obtain silicon-modified carbon nanotubes;

[0029] (6) Add 5 parts by weight of amino acid-modified polyurethane, 6 parts by weight of silicon-modified carbon nanotubes, 3 parts by weight of hydroxylated boron nitride, 60 parts by weight of white oil, 2 parts by weight of calcium chloride solution, 1 part by weight of Tween 20 emulsifier, 2 parts by weight of phosphate wetting agent, and 2 parts by weight of oxidized asphalt into a stirrer and stir for 10 minutes to obtain an oil-based drilling fluid. Example 2

[0030] (1) 4 parts by weight of calcium carbonate were added to deionized water, stirred to dissolve, and 0.4 parts by weight of L-histidine were added thereto, reacted at 70° C. for 70 min, filtered after reaction, and the filter cake was dried in an oven at 90° C. for 7 h, to obtain L-histidine-modified calcium carbonate nanoparticles;

[0031] (2) 12 parts by weight of hexamethylene diisocyanate and 7 parts by weight of 1,4-butanediol were added to anhydrous tetrahydrofuran solvent, stirred at a constant speed for 35 minutes, and then 4 parts by weight of L-histidine-modified calcium carbonate nanospheres and 0.3 parts by weight of dibutyltin dilaurate catalyst were added, heated and stirred at 70°C for 4 hours. After the reaction was completed, the mixture was cooled to room temperature, washed with methanol 4 times, and vacuum dried at 60°C for 25 hours to obtain amino acid-modified polyurethane;

[0032] (3) Add di(dimethylamino)methylvinylsilane and chloroacetic acid to N,N-dimethylformamide solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to chloroacetic acid is 1:1.6, stir to dissolve, and react at 110°C for 12 hours. After the reaction, remove the solvent by distillation under reduced pressure, filter and dry to obtain intermediate 1;

[0033] (4) adding intermediate 1 and glycidol to acetone solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of intermediate 1, glycidol, and p-toluenesulfonic acid catalyst is 1:1.8:0.03, and carrying out esterification reaction at 120°C for 14h. After completion, cooling to room temperature, washing, filtering, and drying to obtain intermediate 2;

[0034] (5) Add 2 parts by weight of sodium dodecyl sulfate emulsifier and 6 parts by weight of vinyl carbon nanotubes into deionized water, and after uniform dispersion, add 10 parts by weight of intermediate 2, 7 parts by weight of methyl acrylate, and 12 parts by weight of allyltrimethylammonium chloride, introduce nitrogen protection, and then continue to add 1 part by weight of azobisisobutyronitrile initiator, react at 110° C. for 10 hours, wash with deionized water and ethanol in turn, and dry to obtain silicon-modified carbon nanotubes;

[0035] (6) Add 8 parts by weight of amino acid-modified polyurethane, 10 parts by weight of silicon-modified carbon nanotubes, 6 parts by weight of hydroxylated boron nitride, 80 parts by weight of white oil, 4 parts by weight of calcium chloride solution, 3 parts by weight of Tween 20 emulsifier, 3 parts by weight of phosphate wetting agent, and 3 parts by weight of oxidized asphalt into a stirrer and stir for 15 minutes to obtain an oil-based drilling fluid. Example 3

[0036] (1) 3 parts by weight of calcium carbonate was added to deionized water, stirred to dissolve, and 0.35 parts by weight of L-histidine was added thereto, and the mixture was reacted at 68° C. for 60 min. After the reaction, the mixture was filtered, and the filter cake was dried in an oven at 82° C. for 6 h. After the reaction, L-histidine-modified calcium carbonate nanoparticles were obtained.

[0037] (2) 10 parts by weight of hexamethylene diisocyanate and 6 parts by weight of 1,4-butanediol were added to anhydrous tetrahydrofuran solvent, stirred at a constant speed for 27.5 minutes, and then 3.5 parts by weight of L-histidine-modified calcium carbonate nanospheres and 0.25 parts by weight of dibutyltin dilaurate catalyst were added, heated and stirred at 57.5°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, washed with methanol 3 times, and vacuum dried at 55°C for 23.5 hours to obtain amino acid-modified polyurethane;

[0038] (3) Add di(dimethylamino)methylvinylsilane and chloroacetic acid to N,N-dimethylformamide solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to chloroacetic acid is 1:1.4, stir to dissolve, react at 100°C for 10 hours, and then remove the solvent by distillation under reduced pressure, filter and dry to obtain intermediate 1;

[0039] (4) Add intermediate 1 and glycidol to acetone solvent, stir evenly, and then continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, glycidol, and p-toluenesulfonic acid catalyst is 1:1.6:0.02, and carry out esterification reaction at 107.5°C for 11 hours. After completion, cool to room temperature, wash, filter, and dry to obtain intermediate 2;

[0040] (5) 1.5 parts by weight of sodium dodecyl sulfate emulsifier and 5 parts by weight of vinyl carbon nanotubes were added to deionized water, and after uniform dispersion, 7.5 parts by weight of intermediate 2, 5.5 parts by weight of methyl acrylate, and 10 parts by weight of allyltrimethylammonium chloride were added, and nitrogen was introduced for protection. Then, 0.9 parts by weight of azobisisobutyronitrile initiator was added, and the mixture was reacted at 100° C. for 7 hours. The mixture was washed with deionized water and ethanol in turn, and dried to obtain silicon-modified carbon nanotubes;

[0041] (6) 6.5 parts by weight of amino acid-modified polyurethane, 8 parts by weight of silicon-modified carbon nanotubes, 4.5 parts by weight of hydroxylated boron nitride, 70 parts by weight of white oil, 3 parts by weight of calcium chloride solution, 2 parts by weight of Tween 20 emulsifier, 2.5 parts by weight of phosphate wetting agent, and 2.5 parts by weight of oxidized asphalt were added into a stirrer and stirred for 12.5 minutes to obtain an oil-based drilling fluid. Example 4

[0042] (1) 2 parts by weight of calcium carbonate was added to deionized water, stirred to dissolve, and 0.3 parts by weight of L-histidine was added thereto, and the reaction was carried out at 65° C. for 50 min. After the reaction was completed, the mixture was filtered and the filter cake was dried in an oven at 75° C. for 5 h. After the reaction was completed, L-histidine-modified calcium carbonate nanoparticles were obtained.

[0043] (2) 8 parts by weight of hexamethylene diisocyanate and 5 parts by weight of 1,4-butanediol were added to anhydrous tetrahydrofuran solvent, stirred at a constant speed for 20 minutes, and then 3 parts by weight of L-histidine-modified calcium carbonate nanospheres and 0.2 parts by weight of dibutyltin dilaurate catalyst were added, heated and stirred at 45°C for 2 hours. After the reaction was completed, the mixture was cooled to room temperature, washed twice with methanol, and vacuum dried at 50°C for 22 hours to obtain amino acid-modified polyurethane;

[0044] (3) Add di(dimethylamino)methylvinylsilane and chloroacetic acid to N,N-dimethylformamide solvent, wherein the mass ratio of di(dimethylamino)methylvinylsilane to chloroacetic acid is 1:1.6, stir to dissolve, and react at 110°C for 12 hours. After the reaction, remove the solvent by distillation under reduced pressure, filter and dry to obtain intermediate 1;

[0045] (4) adding intermediate 1 and glycidol to acetone solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of intermediate 1, glycidol, and p-toluenesulfonic acid catalyst is 1:1.8:0.03, and carrying out esterification reaction at 120°C for 14h. After completion, cooling to room temperature, washing, filtering, and drying to obtain intermediate 2;

[0046] (5) 1.5 parts by weight of sodium dodecyl sulfate emulsifier and 5 parts by weight of vinyl carbon nanotubes were added to deionized water, and after uniform dispersion, 7.5 parts by weight of intermediate 2, 5.5 parts by weight of methyl acrylate, and 10 parts by weight of allyltrimethylammonium chloride were added, and nitrogen was introduced for protection. Then, 0.9 parts by weight of azobisisobutyronitrile initiator was added, and the mixture was reacted at 100° C. for 7 hours. The mixture was washed with deionized water and ethanol in turn, and dried to obtain silicon-modified carbon nanotubes;

[0047] (6) 6.5 parts by weight of amino acid-modified polyurethane, 8 parts by weight of silicon-modified carbon nanotubes, 4.5 parts by weight of hydroxylated boron nitride, 70 parts by weight of white oil, 3 parts by weight of calcium chloride solution, 2 parts by weight of Tween 20 emulsifier, 2.5 parts by weight of phosphate wetting agent, and 2.5 parts by weight of oxidized asphalt were added into a stirrer and stirred for 12.5 minutes to obtain an oil-based drilling fluid.

[0048] Comparative Example 1

[0049] Compared with Example 4, this comparative example is characterized in that no amino acid-modified polyurethane is added.

[0050] Comparative Example 2

[0051] The difference between this comparative example and Example 4 is that no silicon-modified carbon nanotubes are added.

[0052] The oil-based drilling fluid prepared in the above examples and comparative examples was hot rolled at 210°C for 16 hours, and its rheological properties (including apparent viscosity AV, plastic viscosity PV and dynamic shear force YP) and demulsification voltage Es before and after rolling were measured. The hot rolled oil-based drilling fluid was added to a high-temperature and high-pressure permeability plugging instrument equipped with a core sand tray, sealed, and pressurized with liquid oil to record the sand tray leakage (FL) at 210°C and 1000 psi for 30 minutes. HTHP The sand disc model is 170-53-3, the average pore size is 20 μm, and the test results are shown in Table 1.

[0053] Table 1: Oil-based drilling fluid was hot rolled at 210°C for 16 hours to test rheological properties and sand plate leakage.

[0054]

[0055] As can be seen from Table 1, for Examples 1-4 and Comparative Examples 1-2, the apparent viscosity AV, plastic viscosity PV, dynamic shear force YP and demulsification voltage Es before and after hot rolling do not change much, indicating that the drilling fluid of the present invention has good stability and high temperature resistance. From the rate loss, it can be concluded that the present invention has good plugging performance, rheology, and thermal stability, and improves the high temperature plugging performance of the oil-based drilling fluid.

[0056] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. An oil-based drilling fluid, characterized in that: The invention comprises the following components by weight: 5-8 parts by weight of amino acid modified polyurethane, 6-10 parts by weight of silicon modified carbon nanotubes, 3-6 parts by weight of hydroxylated boron nitride, 60-80 parts by weight of white oil, 2-4 parts by weight of calcium chloride solution, 1-3 parts by weight of Tween 20 emulsifier, 2-3 parts by weight of phosphate wetting agent, and 2-3 parts by weight of oxidized asphalt; The preparation method of the amino acid modified polyurethane is: (1) adding 2-4 parts by weight of calcium carbonate to deionized water, stirring to dissolve, and then adding 0.3-0.4 parts by weight of L-histidine, reacting at 65-70° C. for 50-70 min, filtering after reaction, and drying the filter cake in an oven at 75-90° C. for 5-7 h, to obtain L-histidine-modified calcium carbonate nanoparticles; (2) adding 8-12 parts by weight of hexamethylene diisocyanate and 5-7 parts by weight of 1,4-butanediol to anhydrous tetrahydrofuran solvent, stirring at a constant speed for 20-35 minutes, then adding 3-4 parts by weight of L-histidine-modified calcium carbonate nanospheres and 0.2-0.3 parts by weight of dibutyltin dilaurate catalyst, heating and stirring at 45-70° C. for 2-4 hours, cooling to room temperature after the reaction is completed, washing with methanol for 2-4 times, and vacuum drying at 50-60° C. for 22-25 hours to obtain amino acid modified polyurethane; The preparation method of the silicon-modified carbon nanotubes is as follows: S1. Add di(dimethylamino)methylvinylsilane and chloroacetic acid to N,N-dimethylformamide solvent, stir to dissolve, react at 90-110°C for 8-12h, remove the solvent by distillation under reduced pressure, filter and dry to obtain intermediate 1; S2. Add intermediate 1 and glycidol to acetone solvent, stir evenly, then continue to add p-toluenesulfonic acid catalyst to carry out esterification reaction, react at 95-120° C. for 8-14 hours, cool to room temperature after completion, wash, filter, and dry to obtain intermediate 2; S3. 1-2 parts by weight of sodium dodecyl sulfate emulsifier and 4-6 parts by weight of vinyl carbon nanotubes are added to deionized water, and after uniform dispersion, 5-10 parts by weight of intermediate 2, 4-7 parts by weight of methyl acrylate, 8-12 parts by weight of allyltrimethylammonium chloride are added, nitrogen is introduced for protection, and then 0.8-1 parts by weight of azobisisobutyronitrile initiator is added, and the reaction is carried out at 90-110°C, and the reaction is carried out successively with deionized water and ethanol, and dried to obtain silicon-modified carbon nanotubes; The mass ratio of di(dimethylamino)methylvinylsilane to chloroacetic acid in S1 is 1:1.2-1.6; The mass ratio of intermediate 1, glycidol, and p-toluenesulfonic acid catalyst in S2 is 1:1.4-1.8:0.01-0.03; The reaction time in S3 is 4-10h.

2. A method for preparing an oil-based drilling fluid as claimed in claim 1, characterized in that: The preparation method of the oil-based drilling fluid is as follows: amino acid-modified polyurethane, silicon-modified carbon nanotubes, hydroxylated boron nitride, white oil, calcium chloride solution, Tween 20 emulsifier, phosphate wetting agent, and oxidized asphalt are added into a stirrer and stirred for 10-15 minutes to obtain the oil-based drilling fluid.