High-entropy alloy coating with low thermal conductivity, high heat flux reflectivity and high corrosion resistance and preparation method and application thereof
Through the gradient structure of high-entropy alloy coating and supersonic spraying technology, the problem of insufficient stability of metal-based thermal barrier coatings in medium and high temperature applications is solved, and low thermal conductivity, high thermal flow reflectivity and high corrosion resistance are achieved, which is significantly Reduces heat loss of piston engines and improves thermal efficiency.
Patent Information
- Application Number
- CN202411075841.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing metal-based thermal barrier coatings are insufficient in stability and reliability during medium and high temperature applications, and it is difficult to achieve low thermal conductivity, high heat flow reflectivity and high corrosion resistance at the same time, and cannot effectively reduce the heat loss of piston engines.
The gradient structure of high-entropy alloy coating is prepared by supersonic flame spraying and glazing treatment. The chemical formula of the component is AlaCrbFecNidTieBf, which has a gradient structure of two upper and lower layers. The upper layer is submicron equiaxed crystal, and the lower layer is dendritic structure, combining inertia. Gas atomization and high-energy laser beam flow processing optimize process parameters to achieve low thermal conductivity, high thermal flow reflectivity and high corrosion resistance.
Low thermal conductivity and high thermal flow reflectivity below 1000°C are achieved, which significantly improves the thermal insulation and corrosion protection performance of the engine, reduces heat loss, and improves the thermal efficiency and reliability of the engine.
Smart Images

Figure CN118600358B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of surface thermal protection, and in particular to a high-entropy alloy coating with low thermal conductivity, high heat flux reflectivity and high corrosion resistance, and a preparation method and application thereof. Background Art
[0002] Piston engines have the advantages of high efficiency, durability and low cost and are widely used in various fields, such as high-power marine diesel engines, aviation kerosene piston engines, etc. According to statistics, nearly 40% of the thermal efficiency of piston engines is lost in the cooling system and combustion exhaust gas. Therefore, reducing heat loss is one of the effective ways to improve the thermal efficiency of piston engines.
[0003] Drawing on the successful application of ceramic-based thermal barrier coatings (TBCs) in aviation turbojet engines, a research team has proposed the design of metal-based thermal barrier coatings for automotive gasoline and diesel engines with relatively low temperatures but coupled thermal and mechanical loads. However, at present, metal-based thermal barrier coatings are still mainly Fe-based amorphous coatings, such as the series of invention patents on Fe-based amorphous alloys and their preparation methods as thermal insulation coatings published by Zhou Zheng's team, application numbers 201410128869.4, 201610025620.X and 201710811742.6, etc. However, Fe-based amorphous is a typical metastable material, which will crystallize at around 600°C. Crystallization and grain growth lead to the degradation of thermal insulation performance, resulting in insufficient stability and reliability when used as a thermal barrier coating in medium and high temperature applications. To this end, the team designed a new high entropy alloy as a metal-based thermal barrier coating material (see patent 201810317100.5), but the coating has a relatively high porosity ranging from 2.15 to 3.68%, and the thermal conductivity is about 3W / mK at room temperature.
[0004] For diesel engines or aviation kerosene piston engines used in marine vessels, the protective coating on the hot end surface must not only have a low thermal conductivity, but also require the coating surface to have a high heat flux reflectivity to reduce heat loss, and at the same time have good corrosion resistance. Therefore, the development of a new metal-based thermal barrier coating material and preparation method with better comprehensive performance is one of the problems that urgently need to be solved in the field of thermal insulation protection of piston engines. In view of this, the present invention is specially proposed. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a high-entropy alloy coating with low thermal conductivity, high heat flux reflectivity and high corrosion resistance, and a preparation method and application thereof.
[0006] Specifically, the technical solution of the present invention is as follows:
[0007] In a first aspect, the present invention provides a high entropy alloy coating, the chemical formula of which is marked as Al a Cr b Fe c Ni d Ti e B f , wherein a=0.30-0.60, b=0.80-0.95, c=0.90-1.25, d=0.80-1.10, e=0.10-0.30, f=0.01-0.1; the high entropy alloy coating is prepared by supersonic flame spraying and then glazing high entropy alloy powder of corresponding molar ratio, and has a gradient structure.
[0008] Preferably, the gradient structure comprises two layers, the upper layer is submicron equiaxed crystal, and the phase structure is composed of ordered B2 phase and disordered A2 phase; the lower layer is dendrite structure, and the phase structure is mainly A2 phase.
[0009] Preferably, the gradient structure comprises two layers, the upper layer being a heat flow reflection layer and / or a corrosion resistant layer; and the lower layer being a heat insulation layer.
[0010] Preferably, the thickness of the upper layer is 5-100 μm, and the thickness of the lower layer is 200-350 μm.
[0011] Preferably, in the component chemical formula, a=0.35-0.55, b=0.83-0.95, c=0.90-1.15, d=0.85-1.05, e=0.10-0.25, and f=0.01-0.09.
[0012] In a second aspect, the present invention provides a method for preparing the high entropy alloy coating, comprising the following steps: supersonic flame spraying the high entropy alloy powder, and then glazing it.
[0013] Preferably, in the high entropy alloy powder: the powder particle size is 15-45 μm.
[0014] Preferably, the high entropy alloy powder is prepared by an inert gas atomization method.
[0015] Preferably, the process parameters of the supersonic flame spraying include: oxygen flow rate 1950-2100 SCFH, kerosene flow rate 6.0-6.2 GPH, nitrogen flow rate 26±2 SCFH, powder feeding rate 5.0-5.5 r / min, and spraying distance 380-400 mm.
[0016] Preferably, the process parameters of the glazing treatment include: laser power 400-450W, scanning speed 10-12mm / s, overlap rate 45-50%, spot diameter less than 4mm, 1-2 cycles, and argon protection.
[0017] In a third aspect, the present invention also provides an application of the high entropy alloy coating or the high entropy alloy coating prepared by the preparation method in the thermal insulation and corrosion resistance protection of the hot end surface of a marine diesel engine or a piston aircraft engine.
[0018] Preferably, the thermal insulation and corrosion resistance protection means: the thermal conductivity can be maintained at no more than 6.96W / mK within 1000°C; the corrosion potential in a neutral salt solution (3.5wt.% NaCl) is higher than -275mV SCE , corrosion current is less than 0.5μA / cm 2 .
[0019] Beneficial effects:
[0020] The present invention provides a high entropy alloy coating with low thermal conductivity, high heat flux reflectivity and high corrosion resistance, and a preparation method and application thereof. The chemical formula of the high entropy alloy coating is marked as Al a Cr b Fe c Ni d Ti e B f , wherein a=0.30-0.60, b=0.80-0.95, c=0.90-1.25, d=0.80-1.10, e=0.10-0.30, f=0.01-0.1; the high entropy alloy coating is made of high entropy alloy powder of corresponding molar ratio by supersonic flame spraying and then glazing treatment, and has a gradient structure. The high entropy alloy coating provided by the present invention not only realizes the heat insulation protection function, but also exhibits high heat flow reflectivity and corrosion resistance, can effectively protect the hot end components of the piston engine, improve the thermal efficiency of the engine, reduce heat loss, promote energy conservation and emission reduction, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be described below.
[0022] Figure 1 XRD analysis patterns of high entropy alloy coatings prepared in Example 3 and Comparative Example 4;
[0023] Figure 2 This is the TEM morphology of the high entropy alloy coating prepared in Example 3. DETAILED DESCRIPTION
[0024] The invention provides a high-entropy alloy coating with low thermal conductivity, high heat flux reflectivity and high corrosion resistance, as well as a preparation method and application thereof. The high-entropy alloy coating is composed of AlCrFeNiTiB, and its preparation method first adopts supersonic flame spraying technology to prepare the coating, and then glazes the surface of the coating. The high-entropy alloy coating provided by the present invention has a gradient structure of upper and lower layers. The upper layer is fine submicron equiaxed crystals, which function to improve the heat flux reflectivity of the coating and simultaneously improve the corrosion resistance; the lower layer is mainly a coarse dendrite structure, which functions to ensure the thermal insulation effect of the coating, and can be used for thermal insulation and corrosion protection of the hot end face of a piston engine to improve combustion efficiency.
[0025] In a more specific embodiment, the present invention adopts the following technical solution:
[0026] A high entropy alloy coating with low thermal conductivity, high heat flux reflectivity and high corrosion resistance, wherein the high entropy alloy coating has a gradient structure, and the chemical formula of the high entropy alloy coating component is marked as Al a Cr b Fe c Ni d Ti e B f , where a=0.30-0.60, b=0.80-0.95, c=0.90-1.25, d=0.80-1.10, e=0.10-0.30, f=0.01-0.1.
[0027] Furthermore, the preferred values of a, b, c, d, and e are: a=0.35-0.55, b=0.83-0.95, c=0.90-1.15, d=0.85-1.05, e=0.10-0.25, f=0.01-0.09.
[0028] The high entropy alloy coating provided by the present invention presents a gradient structure with upper and lower layers of different tissues: the upper structure is a fine submicron equiaxed crystal structure, the phase structure is composed of an ordered B2 phase and a disordered A2 phase, the thickness is 5-100μm, and the function is to improve the heat flow reflectivity of the coating and simultaneously improve the corrosion resistance; the tissue of the lower structure is mainly a coarse dendrite tissue, the phase structure is mainly composed of an A2 phase, the thickness is 200-350μm, and the main function is to provide a heat insulation effect to protect the substrate and improve the combustion efficiency of the combustion chamber.
[0029] The method for preparing the high entropy alloy coating of the present invention preferably comprises the following steps:
[0030] Step 1: preparing the powder of the high entropy alloy coating component by an inert gas atomization method, wherein the powder particle size is 15-45 μm after screening;
[0031] Step 2: The high entropy alloy powder is sprayed by supersonic flame to prepare the high entropy alloy coating, and the process parameters are: oxygen flow rate 1950-2100 SCFH, kerosene flow rate 6.0-6.2 GPH, nitrogen flow rate 26 SCFH, powder feeding rate 5.0-5.5 r / min, spraying distance 380-400 mm;
[0032] Step 3: The high entropy alloy coating is glazed with the following process parameters: laser power 400-450W, scanning speed 10-12mm / s, overlap rate 45-50%, spot diameter less than 4mm, 1-2 cycles, and argon protection.
[0033] The present invention provides the high entropy alloy coating and the preparation method thereof, which can be used in the thermal insulation and corrosion resistance protection of the hot end surface of a marine diesel engine or a piston aircraft engine. Compared with known conventional coatings, it has significant advantages in heat flow reflectivity and corrosion resistance.
[0034] In the present invention, the high entropy alloy coating has excellent comprehensive performance mainly due to the reasonable coordination between the components and the optimization of the preparation method. The coating material described in the present invention is a multi-principal alloy comprising Al, Cr, Fe, Ni, Ti, and B, and the phase structure is mainly a BCC composed of an ordered B2 phase and a disordered A2 phase. Among them, the atomic radii of the three transition metals are relatively close, which can achieve good mutual dissolution, which is conducive to ensuring that the coating obtains a single-phase solid solution structure, so that the material can have better process adaptability, that is, the particles have good deformation ability during deposition to promote the coating to increase density; the nearly equimolar ratio of Cr and Fe content helps to ensure the generation of disordered BCC phase, thereby increasing the scattering effect of the lattice on electrons and phonons, and sufficient Cr element content helps to improve corrosion resistance. The atomic radius of the Al element is relatively large, which can increase the degree of lattice distortion of the alloy. At the same time, the large-sized Ti element is an element that promotes the formation of BCC. The present invention uses specific process conditions to make the Al and Ti elements or Ni and Ti elements in the alloy diffuse and react to form an ordered B2 phase. The interface between the ordered and disordered phases helps to increase the scattering of electrons and phonons and reduce the overall thermal conductivity of the coating. Al and Ni, Ti and Fe and Cr are easy to form coarse brittle intermetallic compound phases, which are not conducive to the overall mechanical properties of the coating, and thus affect the service reliability. In view of this problem, the present invention controls the spraying process on the basis of reasonable component design, reduces the overall thermal enthalpy of the metal melt, inhibits the formation of intermetallic compound phases, and increases the formation of ordered B2 phases. The addition of a small amount of B element in the present invention helps to deoxidize during the spraying process, reduces the oxidation loss of BCC phase-forming elements, increases the bonding strength of the coating, and ensures the reliability of the coating. Similarly, Cr and Fe elements in the alloy system are more sensitive to B. On the one hand, the solid solubility of B element is low in most metal elements. On the other hand, B element and Cr or Fe element are easy to react to form boride precipitation phases. The formation of brittle boride phases significantly reduces the corrosion resistance of the coating, and is not conducive to the glazing treatment of the coating, so that the coating is prone to cracking or peeling during the preparation process. The present invention overcomes this technical problem by coordinating the B content and the preparation process.The present invention adopts an asynchronous preparation method. First, the high entropy alloy coating is prepared by a supersonic flame spraying method. The ultra-high flight speed helps the particles to fully deform, so that the coating presents a denser particle overlap structure. The overlap interface helps to increase the barrier effect on heat transfer carriers. The present invention also controls the melting degree of the particles by adjusting the flame temperature of the spraying process parameter, regulates the size of the dendrite structure, avoids the formation of coarse pores or coating defects, and ensures the ultra-high bonding strength of the coating. In addition, based on the preparation of high entropy alloy by HVOF, the present invention performs glazing treatment on the surface of the coating by a high-energy laser beam with a small spot diameter, and regulates the body energy density by controlling the process parameters to achieve inducing the phase change of the above-mentioned alloy components while causing micro-healing of the micropores and the interface of the deformed particles, thereby reconstructing the organization and phase structure of the coating within a thickness of tens of microns from the upper surface, reducing the surface roughness of the coating, increasing the reflectivity of the upper surface of the coating to the heat flow, reducing heat loss, and simultaneously improving the corrosion resistance of the coating. The present invention provides a coating with a multi-scale synergistic organizational structure of micron interlayer pores, disordered BCC phase of dendrite organization, disordered BCC phase of equiaxed crystal organization and nanometer ordered BCC phase through the coordination of components and asynchronous processes, thereby achieving the simultaneous reduction of thermal conductivity and improvement of heat flow reflectivity and corrosion resistance.
[0035] The overall improvement of the comprehensive performance of the coating is mainly achieved through the rational configuration of the alloy's own components and the combined effect of the preparation method. It is not determined by any single element, but it is also indispensable. Of course, it cannot be achieved through just a limited number of tests.
[0036] The beneficial effects of the present invention are at least: 1) The high entropy alloy coating has good thermal insulation performance, and the room temperature thermal conductivity is lower than 2.13W / mK; 2) The coating surface does not require additional machining treatment, and the roughness Ra is lower than 5.5μm; 3) The bonding strength between the coating and the substrate is greater than 55MPa, and the microhardness is greater than 1050HV; 4) The corrosion potential of the coating in a neutral salt solution is higher than -275mV SCE , corrosion current is less than 0.5μA / cm 2 ; 5) The thermal efficiency of the piston engine combustion chamber is significantly improved.
[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0039] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "specific implementations", or "some specific implementations" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0040] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0041] In the following embodiments, the coating is prepared by the following steps:
[0042] Step 1: Prepare the powder of the high entropy alloy coating component by an inert gas atomization method, and the powder particle size is 15-45 μm after screening.
[0043] Step 2: The high entropy alloy powder is prepared by a supersonic flame spraying method, and the process parameters are: oxygen flow rate 1950-2100 SCFH, kerosene flow rate 6.0-6.2 GPH, nitrogen flow rate 26 SCFH, powder feeding rate 5.0-5.5 r / min, and spraying distance 380-400 mm.
[0044] Step 3: The high entropy alloy coating is glazed with the following process parameters: laser power 400-450W, scanning speed 10-12mm / s, overlap rate 45-50%, spot diameter less than 4mm, 1-2 cycles, and argon protection.
[0045] Example 1
[0046] High entropy alloy coating Al a Cr b Fe cNi d Ti e B f In the chemical formula: a=0.30, b=0.80, c=1.20, d=1.10, e=0.10, f=0.01. Spraying process parameters are: oxygen flow rate 1950SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 380mm. Glazing treatment process parameters are: laser power 400W, scanning speed 12mm / s, overlap rate 48%, spot diameter 2.5mm, circulation times 2 times, argon protection.
[0047] Example 2
[0048] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.40, b=0.85, c=1.25, d=1.00, e=0.15, f=0.05. The spraying process parameters are: oxygen flow rate 2000SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 390mm. The glazing treatment process parameters are: laser power 430W, scanning speed 11mm / s, overlap rate 48%, spot diameter 3mm, circulation pass 2 times, argon protection.
[0049] Example 3
[0050] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.50, b=0.90, c=1.00, d=0.90, e=0.20, f=0.05. The spraying process parameters are: oxygen flow rate 2000SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 390mm. The glazing treatment process parameters are: laser power 430W, scanning speed 12mm / s, overlap rate 50%, spot diameter 3mm, cycle pass 1 time, argon protection.
[0051] Example 4
[0052] High entropy alloy coating Al a Cr b Fe c Ni d Ti e Bf In the chemical formula: a=0.30, b=0.80, c=1.20, d=1.10, e=0.10, f=0.06. The spraying process parameters are: oxygen flow rate 2000SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 380mm. The glazing treatment process parameters are: laser power 410W, scanning speed 11mm / s, overlap rate 48%, spot diameter 2.5mm, cycle 1 time, argon protection.
[0053] Example 5
[0054] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.50, b=0.90, c=1.00, d=0.90, e=0.20, f=0.05. The spraying process parameters are: oxygen flow rate 2000SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 390mm. The glazing treatment process parameters are: laser power 450W, scanning speed 11mm / s, overlap rate 45%, spot diameter 3mm, cycle pass 1 time, argon protection.
[0055] Example 6
[0056] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.40, b=0.85, c=1.25, d=1.00, e=0.15, f=0.07. The spraying process parameters are: oxygen flow rate 2000SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 390mm. The glazing treatment process parameters are: laser power 450W, scanning speed 12mm / s, overlap rate 48%, spot diameter 2.5mm, cycle 1 time, argon protection.
[0057] Example 7
[0058] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B fIn the chemical formula: a=0.60, b=0.95, c=0.90, d=0.80, e=0.25, f=0.07. Spraying process parameters are: oxygen flow 2050SCFH, kerosene flow 6.1GPH, nitrogen flow 26SCFH, powder feeding rate 5.0r / min, spraying distance 395mm. Glazing treatment process parameters are: laser power 420W, scanning speed 11mm / s, overlap rate 48%, spot diameter 3mm, circulation pass 2 times, argon protection.
[0059] Example 8
[0060] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.50, b=0.90, c=1.00, d=0.90, e=0.20, f=0.08. Spraying process parameters are: oxygen flow rate 2100SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 400mm. Glazing treatment process parameters are: laser power 450W, scanning speed 12mm / s, overlap rate 48%, spot diameter 3mm, cycle 1 time, argon protection.
[0061] Example 9
[0062] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.60, b=0.95, c=0.90, d=0.80, e=0.25, f=0.07. Spraying process parameters are: oxygen flow rate 1950SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 380mm. Glazing treatment process parameters are: laser power 420W, scanning speed 11mm / s, overlap rate 48%, spot diameter 3mm, circulation pass 2 times, argon protection.
[0063] Example 10
[0064] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B fIn the chemical formula: a=0.60, b=0.95, c=1.10, d=1.00, e=0.30, f=0.09. Spraying process parameters are: oxygen flow rate 2100SCFH, kerosene flow rate 6.1GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.0r / min, spraying distance 400mm. Glazing treatment process parameters are: laser power 450W, scanning speed 11mm / s, overlap rate 48%, spot diameter 2.5mm, circulation times 2 times, argon protection.
[0065] Comparative Example 1
[0066] The molar percentages of elemental components in the high entropy alloy coating in the existing patent (ZL201810317100.5) are as follows: Al: 12.7%; Co: 15%; Cr: 17.5%; Fe: 18.6%; Ni: 17%; Ti: 19.2%; and unavoidable impurities: <0.5%.
[0067] Comparative Example 2
[0068] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=1.00, b=1.00, c=1.00, d=1.00, e=1.00, f=0.01. Spraying process parameters are: oxygen flow rate 2050SCFH, kerosene flow rate 6.0GPH, nitrogen flow rate 26SCFH, powder feeding rate 5.5r / min, spraying distance 400mm. Glazing treatment process parameters are: laser power 450W, scanning speed 9mm / s, overlap rate 40%, spot diameter 3mm, circulation pass 2 times, argon protection.
[0069] Comparative Example 3
[0070] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.50, b=1.00, c=1.10, d=0.90, e=0.50, f=0.06. The spraying process parameters are: oxygen flow rate 1800SCFH, kerosene flow rate 6.2GPH, nitrogen flow rate 22SCFH, powder feeding rate 5.0r / min, spraying distance 380mm. The glazing treatment process parameters are: laser power 400W, scanning speed 11mm / s, overlap rate 45%, spot diameter 3mm, circulation pass 2 times, argon protection.
[0071] Comparative Example 4
[0072] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.50, b=0.90, c=1.00, d=0.90, e=0.20, f=0.05. Spraying process parameters: oxygen flow 2000SCFH, kerosene flow 6.1GPH, nitrogen flow 26SCFH, powder feeding rate 5.0r / min, spraying distance 390mm. Unglazed treatment.
[0073] Comparative Example 5
[0074] High entropy alloy coating Al a Cr b Fe c Ni d Ti e B f In the chemical formula: a=0.30, b=0.90, c=0.90, d=1.10, e=0.30, f=0.09. Spraying process parameters are: oxygen flow 2100SCFH, kerosene flow 6.1GPH, nitrogen flow 26SCFH, powder feeding rate 5.0r / min, spraying distance 400mm. Glazing treatment process parameters are: laser power 500W, scanning speed 12mm / s, overlap rate 55%, spot diameter 3mm, cycle 1 time, argon protection.
[0075] The coatings prepared in each embodiment and comparative example were subjected to XRD, TEM and microhardness tests; the thermal conductivity of the coatings prepared in each embodiment and comparative example was analyzed using a laser thermal conductivity analyzer; the coatings prepared in each embodiment and comparative example were subjected to a potentiodynamic polarization test using a three-electrode electrochemical workstation, and the etching solution was a 3.5wt.% NaCl solution.
[0076] The XRD test results of high entropy alloy coating are as follows: Figure 1 As shown, the TEM morphology is Figure 2 The results of coating microhardness, thermal conductivity, self-corrosion current and self-corrosion potential are shown in Table 1.
[0077] Table 1 Test results of microhardness, thermal conductivity, self-corrosion current and self-corrosion potential of high entropy alloy coatings in the embodiments and comparative examples
[0078]
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high entropy alloy coating, characterized in that: Its chemical formula is Al a Cr b Fe c Ni d Ti e B f , wherein a=0.30-0.60, b=0.80-0.95, c=0.90-1.25, d=0.80-1.10, e=0.10-0.30, f=0.01-0.1; the high entropy alloy coating is prepared by supersonic flame spraying and glazing of high entropy alloy powder of corresponding molar ratio, and has a gradient structure; the gradient structure includes two layers, the upper layer is submicron equiaxed crystal, and the phase structure is composed of ordered B2 phase and disordered A2 phase; the lower layer is dendrite structure, and the phase structure is mainly A2 phase.
2. The high entropy alloy coating according to claim 1, characterized in that: The upper layer of the gradient structure is a heat flow reflection layer and / or a corrosion resistant layer; the lower layer is a heat insulation layer.
3. The high entropy alloy coating according to claim 1 or 2, characterized in that: The thickness of the upper layer is 5-100 μm, and the thickness of the lower layer is 200-350 μm.
4. The high entropy alloy coating according to claim 1, characterized in that: In its component chemical formula, a=0.35-0.55, b=0.83-0.95, c=0.90-1.15, d=0.85-1.05, e=0.10-0.25, f=0.01-0.
09.
5. The method for preparing the high entropy alloy coating according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: supersonic flame spraying the high entropy alloy powder and then glazing the high entropy alloy powder.
6. The preparation method according to claim 5, characterized in that: In the high entropy alloy powder: the powder particle size is 15-45 μm; and / or the high entropy alloy powder is prepared by an inert gas atomization method.
7. The preparation method according to claim 5, characterized in that: The process parameters of the supersonic flame spraying include: oxygen flow rate 1950-2100 SCFH, kerosene flow rate 6.0-6.2 GPH, nitrogen flow rate 26±2 SCFH, powder feeding rate 5.0-5.5r / min, and spraying distance 380-400 mm.
8. The preparation method according to claim 5, characterized in that: The process parameters of the glazing treatment include: laser power 400-450 W, scanning speed 10-12 mm / s, overlap rate 45-50%, spot diameter less than 4 mm, 1-2 cycles, and argon protection.
9. Application of the high entropy alloy coating according to any one of claims 1 to 4 or the high entropy alloy coating prepared by the preparation method according to any one of claims 5 to 8 in thermal insulation and corrosion protection of the hot end surface of a marine diesel engine or a piston aircraft engine.