A NbTi superconducting wire and a method for preparing the same
By loading the NbTi superconductor powder into an aluminum tube and undergoing multiple aging heat treatments, combined with the tight arrangement and welding of the NbTi/Cu single core rod, the problem of the low critical current of the NbTi superconducting wire in a high field environment is solved, and the problem of the NbTi superconducting wire is improved. Current carrying capacity and thermal stability in high field environments.
Patent Information
- Application Number
- CN202411080268.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The critical current of NbTi superconducting wire is relatively low in high-field environments, which limits its performance and stability in high-magnetic field applications. In addition, traditional preparation methods have problems such as different deformation of core wires and long production cycles.
The superconductor rod is made by filling the NbTi superconductor powder into an aluminum tube, and the superconductor rod is tightly arranged and welded through multiple aging heat treatment and extrusion. The NbTi/Cu single mandrel is tightly arranged and welded to form an NbTi/Cu composite ingot, and finally NbTi is produced. Superconducting wire.
The critical current and thermal stability of NbTi superconducting wires in high-field environments are improved, and better current carrying capacity and consistency are achieved.
Smart Images

Figure CN118609905B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of superconducting wires and relates to a NbTi superconducting wire and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology, superconducting materials have shown great application potential in many fields such as electronics, biomedicine, science and engineering, transportation and electricity. Among them, NbTi (niobium titanium) superconducting wire, as an important low-temperature superconducting material, has become the mainstream product in the current superconducting material market due to its excellent superconducting properties, good mechanical properties and processing properties, and relatively low cost, and has occupied the vast majority of the market share. However, although NbTi superconducting wires have achieved remarkable application results in many fields, the problem of low critical current in high-field environments has become increasingly prominent, becoming a technical bottleneck restricting its further widespread application. The problem of low critical current in high-field environments is mainly due to the weakening of the magnetic flux pinning effect of NbTi superconducting wires in high magnetic fields, resulting in limited current carrying capacity. This not only limits the performance of NbTi superconducting wires in high magnetic field applications such as magnetic resonance imaging (MRI) and superconducting energy storage, but also poses severe challenges to its stability and reliability under extreme conditions. In addition, in traditional preparation methods, problems such as large differences in the deformation of the core wire inside the superconducting wire, long production cycle, and low yield rate have further aggravated the dilemma of low critical current in high-field environments. To solve the above problems, researchers are constantly exploring new preparation processes and technical means to improve the critical current and thermal stability of NbTi superconducting wires in high-field environments. Summary of the invention
[0003] The purpose of the present invention is to solve at least one of the above technical problems, and to use it to optimize the microstructure of NbTi superconducting wire in a simple and low-cost way, improve its current carrying capacity and thermal stability in a high-field environment, thereby promoting the application and development of NbTi superconducting wire in a wider range of fields. To this end, the present invention provides a NbTi superconducting wire and a preparation method thereof to solve this need in the art.
[0004] In one aspect, the present invention relates to a method for preparing a NbTi superconducting wire, comprising: filling NbTi superconductor powder into an aluminum tube to prepare a NbTi superconductor rod;
[0005] A plurality of NbTi / Cu single core rods are closely arranged in an oxygen-free copper tube, the gaps are filled with the NbTi superconductor rods, and the tubes are sealed and welded to obtain a NbTi / Cu composite ingot;
[0006] The NbTi / Cu composite ingot is subjected to extrusion, stretching and multiple aging heat treatments to obtain the NbTi superconducting wire.
[0007] Furthermore, in the preparation method of the NbTi superconducting wire provided by the present invention, the preparation method of the NbTi superconductor powder comprises: loading the NbTi rod into a Nb tube, and then loading it into an oxygen-free copper tube; performing multiple aging heat treatments to remove the copper on the surface, and finally pulverizing to obtain the NbTi superconductor powder.
[0008] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the particle size of the NbTi superconductor powder is 350-500 meshes.
[0009] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the diameter of the NbTi rod is 1-3 mm, and the thickness of the Nb tube or the oxygen-free copper tube is 0.2-0.4 mm.
[0010] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the number of the NbTi / Cu single core rods in the oxygen-free copper tube is 7 to 346.
[0011] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the diameter of the NbTi / Cu single core rod is 10-30 mm, and the diameter of the NbTi superconductor rod is 1-3 mm.
[0012] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the number of the multiple aging heat treatments is 5 times, and the aging times are 40 h, 40 h, 80 h, 80 h, and 40 h, respectively.
[0013] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the temperature of each aging heat treatment is 550°C.
[0014] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the purity of aluminum in the aluminum tube is not less than 99.99%, and the thickness of the aluminum tube is 0.1-0.2 mm.
[0015] On the other hand, the present invention relates to a NbTi superconducting wire, which is prepared by the method for preparing the NbTi superconducting wire.
[0016] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages:
[0017] The present invention provides a method for preparing a NbTi superconducting wire, which adopts a method of filling NbTi superconducting powder into an aluminum tube to prepare a NbTi superconducting rod and inserting it into a NbTi / Cu assembly structure to prepare a NbTi superconducting wire. The NbTi superconducting wire provided by the present invention has good consistency and has a higher critical current and thermal stability value in a high field environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 This is the assembly structure when the number of NbTi / Cu single core rods is 7.
[0020] Among them, 100 is an oxygen-free copper tube, 210 is a first NbTi superconductor rod, 220 is a second NbTi superconductor rod, and 300 is a NbTi / Cu single core rod. DETAILED DESCRIPTION
[0021] The technical scheme of the present invention is described below in conjunction with the examples, but the present invention is not limited to the following examples. The experimental methods and detection methods described in each example are conventional methods unless otherwise specified; the reagents and materials are available on the market unless otherwise specified, and the % in the following examples are all mass percentages unless otherwise specified.
[0022] Example 1
[0023] This embodiment provides a method for preparing a NbTi superconducting wire.
[0024] Step 1: Place the NbTi rod into the Nb tube, and then into the oxygen-free copper tube; after multiple aging heat treatments, remove the copper on the surface and crush it, use 350 mesh and 500 mesh sieves to sieve the NbTi superconductor powder, and take the intermediate powder as the NbTi superconductor powder.
[0025] Step 2: If Figure 1 The assembly structure is designed as shown, the NbTi superconductor powder obtained in step 1 is loaded into an aluminum tube, the purity of aluminum in the aluminum tube is not less than 99.99%, and the thickness of the aluminum tube is 0.1-0.2 mm; according to the gap between the NbTi / Cu single core rod 300 and the oxygen-free copper tube 100, the NbTi superconductor powder is loaded into the aluminum tube in a glove box filled with high-purity argon (99.99%) to prepare a plurality of first NbTi superconductor rods 210; according to the gap between the NbTi / Cu single core rods 300, the NbTi superconductor powder is loaded into the aluminum tube in a glove box filled with high-purity argon (99.99%) to prepare a plurality of second NbTi superconductor rods 220.
[0026] Step 3: If Figure 1The designed assembly structure shown is used to mount a NbTi / Cu single core rod 300 with a diameter of 10-30 mm.
[0027] Step 4: Figure 1 The assembly structure shown in the design is to assemble the oxygen-free copper tube 100, the first NbTi superconductor rod 210, the second NbTi superconductor rod 220, and the NbTi / Cu single core rod 330 prepared in the previous steps, and then weld them after sealing to obtain a NbTi / Cu composite ingot.
[0028] Step 5: The NbTi / Cu composite ingot is subjected to extrusion, stretching and multiple aging heat treatments to obtain a NbTi superconducting wire.
[0029] Exemplarily, in step 1, the copper on the surface is removed by peeling or chemical etching, for example, a nitric acid solution with a concentration of 40-60% is used to remove the copper on the surface.
[0030] Exemplarily, in step 2, the diameter of the first NbTi superconductor rod 210 or the second NbTi superconductor rod 220 is 1-3 mm, which is adjusted according to the designed assembled structure, and the first NbTi superconductor rod 210 or the second NbTi superconductor rod 220 fills the gap between the NbTi / Cu single core rod 300 and the oxygen-free copper tube 100 as much as possible.
[0031] Exemplarily, in step 4, vacuum electron beam welding is adopted.
[0032] Exemplarily, the present embodiment does not particularly limit the specifications of the NbTi / Cu single core rod 330 , and the copper excess ratio of the NbTi / Cu single core rod is 0.2-5.
[0033] Exemplarily, in step 1, the present embodiment does not specifically limit the time, temperature and number of multiple aging heat treatments in step 1. The temperature of the multiple aging heat treatments is 500° C. to 800° C., the time is 50 h to 100 h, and the number is 3 to 6 times.
[0034] Exemplarily, in step 5, this embodiment does not specifically limit the time, temperature and number of multiple aging heat treatments in step 5. The temperature of the multiple aging heat treatments is 500° C. to 800° C., the time is 50 h to 100 h, and the number is 3 to 6 times.
[0035] Preferably, in step 5, the temperature of the multiple aging heat treatments is 550° C., the number of times is 5 times, and the aging times are 40 h, 40 h, 80 h, 80 h, and 40 h, respectively.
[0036] Example 2
[0037] This embodiment provides a method for preparing a NbTi superconducting wire.
[0038] Refer to Figure 1 According to the designed assembly structure and the preparation steps provided in Example 1, the experimental design shown in Table 1 was carried out.
[0039] Table 1: Experimental design
[0040]
[0041] As shown in Table 1, NbTi superconducting wire samples of test groups 1#~8# were prepared, and their critical currents and RRR values under 10T high field conditions were measured. The test results are shown in Table 2.
[0042] Table 2: Properties of NbTi superconducting wire
[0043]
[0044] As shown in Table 2, the present invention provides a method for preparing a NbTi superconducting wire, which adopts a method of loading NbTi superconductor powder into an aluminum tube to prepare a NbTi superconductor rod and inserting it into a NbTi / Cu assembly structure. While having good consistency, it has a higher critical current and thermal stability value in a high field environment.
[0045] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.
Claims
1. A method for preparing a NbTi superconducting wire, characterized in that: include: The NbTi superconductor powder is placed in an aluminum tube to prepare a NbTi superconductor rod; A plurality of NbTi / Cu single core rods are closely arranged in an oxygen-free copper tube, the gaps are filled with the NbTi superconductor rods, and the tubes are sealed and welded to obtain a NbTi / Cu composite ingot; The NbTi / Cu composite ingot is subjected to extrusion, stretching and multiple aging heat treatments to obtain the NbTi superconducting wire.
2. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The preparation method of the NbTi superconductor powder comprises: placing a NbTi rod into a Nb tube, and then placing the rod into an oxygen-free copper tube; performing multiple aging heat treatments, removing copper on the surface, and finally pulverizing the rod to obtain the NbTi superconductor powder.
3. The method for preparing the NbTi superconducting wire according to claim 2, characterized in that: The particle size of the NbTi superconductor powder is 350-500 meshes.
4. The method for preparing the NbTi superconducting wire according to claim 2, characterized in that: The diameter of the NbTi rod is 1-3 mm, and the thickness of the Nb tube or the oxygen-free copper tube is 0.2-0.4 mm.
5. The method for preparing the NbTi superconducting wire according to claim 1, characterized in that: The number of NbTi / Cu single core rods in the oxygen-free copper tube is 7 to 346.
6. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The diameter of the NbTi / Cu single core rod is 10-30 mm, and the diameter of the NbTi superconductor rod is 1-3 mm.
7. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The number of the multiple aging heat treatments is 5 times, and the aging times are 40h, 40h, 80h, 80h, and 40h, respectively.
8. The method for preparing the NbTi superconducting wire according to claim 7, characterized in that: The aging heat treatment temperature is 550°C each time.
9. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The purity of aluminum in the aluminum tube is not less than 99.99%, and the thickness of the aluminum tube is 0.1-0.2 mm.
10. A NbTi superconducting wire, characterized in that: The superconducting wire is prepared by the method for preparing the NbTi superconducting wire according to any one of claims 1 to 9.