A semiconductor wafer aluminum stripping rework method

Through the segmented aluminum stripping method, combined with dry and wet etching, rinsing and running water wiping technology, the existing technology problems of low aluminum stripping rework efficiency and low product yield of semiconductor wafers have been solved, and efficient silicon wafers have been achieved. Slag removal and wafer surface quality improvement.

CN118610075BActive Publication Date: 2024-10-15BETONE TECH SHANGHAI INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411081297.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-15
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing semiconductor wafer aluminum stripping and reworking technology is inefficient, especially when there is no barrier layer. Wet aluminum corrosion leads to serious side corrosion. Dry silicon slag sweeping cannot completely remove silicon slag, affecting product yield.

Method used

Using the segmented aluminum stripping method, most of the aluminum and its residual silicon are first removed through dry aluminum etching and dry silicon slag sweeping, and then the remaining silicon slag is completely removed through wet etching, rinsing and running water wiping, which improves the removal efficiency.

Benefits of technology

Significantly improves the efficiency of aluminum stripping and rework of semiconductor wafers, reduces rework time, improves product yield, and avoids side corrosion caused by wet aluminum corrosion and damage to the front layer caused by dry sweeping silicon slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118610075B_ABST
    Figure CN118610075B_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor wafer aluminum stripping and rework method, comprising the following steps: providing a semiconductor wafer, wherein the semiconductor wafer comprises an aluminum layer and a silicon layer under the aluminum layer; performing dry aluminum etching on part of the aluminum layer by a dry method; performing dry silicon slag sweeping on the semiconductor wafer after the etching by a dry method, and simultaneously performing ultrasonic running water wiping; performing wet aluminum etching on the remaining aluminum layer; rinsing the semiconductor wafer after the wet aluminum etching and wiping it with a brush running water, and if it is qualified, performing aluminum sputtering, and if it is unqualified, rinsing it again and wiping it with a brush running water until it is qualified. The invention can improve the efficiency of aluminum stripping and reduce the rework time by stripping aluminum in sections, combining the dry silicon slag sweeping and the brush running water wiping, and can play a great role in improving production capacity and improving product yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor manufacturing, and in particular to a semiconductor wafer aluminum stripping rework method. Background Art

[0002] There are many structures of aluminum film processes used in current semiconductor wafers, such as the (TI-TIN-AL-TIN) sandwich structure commonly used in logic chips, the TI-AL-TIN structure commonly used on memory chips, and the TI-TIN-AL structure commonly used in six- and eight-inch power devices. In most of these structures, TI or TI+TIN is sputtered as a barrier layer before sputtering aluminum. If a microscope inspection finds abnormalities on the surface of the aluminum layer after sputtering aluminum (such as roughness, black spots on the surface caused by water and air leakage in the cavity, and silicon precipitation caused by staying in the high-temperature cavity for too long, etc.), the traditional aluminum stripping rework process will be chosen.

[0003] Take the case of no barrier layer in the previous layer as an example: some 6-8 inch line products have no barrier layer before sputtering the thick aluminum layer, and the front layer is Si. First of all, the ALSICU and ALSI targets used by the 6-8 inch PVD equipment contain 0.5%~1% Si (Si doping can prevent Al and Si from melting each other and causing damage to the pn junction). If the traditional aluminum stripping rework process is used, after the wet aluminum etching, the wet silicon slag is swept. Since the front layer is also silicon, it will directly damage the front layer. If you choose to skip the wet silicon slag sweeping, a small amount of silicon remaining after the aluminum is corroded will be embedded in the surface of the front silicon layer, which cannot be removed by running water wiping. The subsequent re-growth of aluminum will make the surface full of dense black spots. Therefore, in general, when there is no barrier layer in the front layer, once an abnormality occurs during the microscope inspection, it will be chosen to continue the tape-out or scrap it according to the severity, but this will greatly affect the yield of the product. Moreover, the traditional wet aluminum etching process will cause serious side corrosion when there is a pattern after photolithography; and the wet silicon slag sweeping cannot be completely removed when there is a lot of silicon slag; if dry aluminum etching with better etching directionality and dry silicon slag sweeping with better silicon slag removal effect are used, the front layer will be damaged; similarly, in the case of a barrier layer, the traditional process is first wet aluminum etching, and then wet silicon slag sweeping is used, at least 20 front water wipes are required, the efficiency of aluminum stripping rework is very low, and the wet aluminum etching process causes serious side corrosion. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a method for aluminum stripping and reworking of semiconductor wafers. In the process of the present invention, aluminum stripping is performed in sections. In the first step, most of the aluminum and its residual silicon are removed by highly efficient dry aluminum etching and dry silicon slag sweeping (since there are generally only 1-3 wafers that need aluminum stripping and reworking each time a problem occurs, the operation time of wet aluminum etching and silicon slag sweeping is only related to the thickness of the aluminum, and the time for one wafer is the same as that for a whole box of 25 wafers, so it is relatively time-consuming. However, dry aluminum etching and silicon slag sweeping are performed separately for each wafer, and the single-wafer time is fast, so the efficiency is high). In the second step, only a small part of the aluminum is left by wet etching, and the residual silicon slag is also less, which greatly improves the efficiency of sweeping silicon slag by rinsing and running water wiping. If segmented aluminum stripping is not used, the residual silicon in 4000nm AlSiCu must be rinsed and brushed with running water at least 20 times. The number of cycles of segmented aluminum stripping, rinsing and running water wiping can be up to about 5 times, and it can be completely removed.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A semiconductor wafer aluminum stripping rework method comprises the following steps:

[0007] S1: Providing a semiconductor wafer, wherein the semiconductor wafer comprises an aluminum layer;

[0008] S2: dry aluminum etching of part of the aluminum layer by dry method;

[0009] S3: Dry-cleaning the etched semiconductor wafer for silicon slag by dry method, and then performing ultrasonic water wiping on the wafer;

[0010] S4: performing wet aluminum etching on the remaining aluminum layer;

[0011] S5: If there is a silicon layer under the aluminum layer, the semiconductor wafer after wet aluminum etching is rinsed and wiped with running water by a brush. If it is qualified, aluminum sputtering is performed; if it is unqualified, it is rinsed again and wiped with running water by a brush until it is qualified. If there is a barrier layer under the aluminum layer, after wet aluminum etching, wet silicon slag is swept and then wiped with running water. If it is qualified, aluminum sputtering is performed; if it is unqualified, it is wiped with running water again until it is qualified.

[0012] As a further solution of the present invention, the barrier layer is located between the aluminum layer and the silicon layer.

[0013] As a further solution of the present invention, the barrier layer includes a TI layer or a TI layer + a TIN layer.

[0014] As a further solution of the present invention, the partial aluminum layer accounts for 1%-99% of the entire aluminum layer.

[0015] As a further solution of the present invention, the partial aluminum layer accounts for 5 / 6 of the entire aluminum layer.

[0016] As a further solution of the present invention, step S1 also includes testing the provided semiconductor wafer. If the aluminum layer is qualified, the next step of wafer taping is carried out. If it is unqualified, aluminum stripping and rework are carried out.

[0017] As a further solution of the present invention, in step S2, the direction of aluminum corrosion is controlled by a dry method.

[0018] As a further solution of the present invention, by segmented aluminum stripping, most of the aluminum and its residual silicon are first removed by dry aluminum etching and dry silicon slag sweeping, and then the remaining aluminum is wet-etched, thereby improving the efficiency of silicon slag sweeping by rinsing and running water wiping.

[0019] As a further solution of the present invention, in step S5, the silicon slag is loosened by rinsing, and the loose silicon slag is removed by running water and brushes on the front of the wiper. The time interval between rinsing and running water wiping is limited to no more than one hour. Rinsing is to remove the oxide layer produced by natural oxidation in the air, loosen the silicon slag and the front layer of silicon, and facilitate the brush to sweep away the silicon slag. The limit is one hour to prevent re-oxidation. The front layer mentioned in the present invention is the layer after the aluminum layer is removed. In the present invention, the front layer includes a barrier layer or a silicon layer.

[0020] The present invention has the following beneficial effects:

[0021] The process of the present invention solves the problem of aluminum stripping rework under the premise that there is no barrier layer in the front layer. The silicon slag and the front layer of silicon are both silicon, and there is no reactant that only corrodes the silicon slag but does not corrode the silicon substrate. Therefore, it is impossible to directly remove the silicon slag by wet method without damaging the front layer of silicon. However, when the front layer is completely exposed after aluminum corrosion, the silicon slag on the surface of the front layer of silicon is loosened by rinsing, and the front water flow and brush of the wiper are used to remove the loosened silicon slag, and the surface silicon slag can be removed until the standard is met by circulating rinsing and running water wiping. In addition, the present invention also solves how to achieve rapid aluminum stripping rework in the presence of a barrier layer.

[0022] The present invention solves the problem of serious side corrosion of wet aluminum corrosion by improving the process. Wet corrosion has the characteristic of isotropy, so the present invention makes the film etched by wet aluminum corrosion as thin as possible, thereby reducing the time of side corrosion. Dry etching has anisotropy and can control the etching direction. By allowing most of the aluminum to be etched by dry aluminum corrosion, the desired etching effect can be achieved.

[0023] The present invention solves the problem of damage to the front layer by dry etching and dry silicon slag sweeping by improving the process. In the current technology, the aluminum etching process does not use dry etching, because whether the front layer has a barrier layer or not, the front layer will be damaged by dry plasma etching. The present invention does not completely remove the aluminum film by dry etching, leaving about one-sixth of the aluminum film, so that neither dry aluminum etching nor dry silicon slag sweeping will affect the front layer, and there is a residual aluminum film barrier, and there is no need to worry about the surface quality of the aluminum film, and the wet method will be used to continue aluminum stripping later.

[0024] The present invention solves the problem that wet silicon slag sweeping cannot be cleaned up when there is a lot of silicon slag by improving the process. The dry silicon slag sweeping has a stronger etching ability, which makes up for the disadvantage that the wet silicon slag sweeping has a mild reaction and is difficult to remove a large amount of silicon slag.

[0025] The present invention solves the problem of low efficiency of removing a large amount of silicon slag by running water wipes without a barrier layer by improving the process. The present invention removes most of the aluminum and its residual silicon by highly efficient dry aluminum etching and dry silicon slag sweeping in the first step through segmented aluminum stripping. Only a small part of the aluminum remains in the second step of wet etching, and the residual silicon slag is also less, which greatly improves the efficiency of rinsing and running water wipes. If segmented aluminum stripping is not used, the residual silicon in 4000nm AlSiCu must be rinsed and wiped with a brush at least 20 times. However, the number of cycles of segmented aluminum stripping, rinsing and running water wipes can be up to about 5 times, and it can be completely removed.

[0026] When there is no barrier layer in the front layer, that is, when the front layer is a silicon layer, the present invention can improve the efficiency of aluminum stripping and reduce rework time by segmented aluminum stripping, combining dry sweeping of silicon slag and wiping with a rinsing brush and running water, which can greatly play a role in increasing production capacity and improving product yield.

[0027] In order to more clearly illustrate the structural features and effects of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the barrier-free aluminum stripping rework process in the prior art.

[0029] Figure 2 The present invention is a schematic diagram of the aluminum stripping rework process with a barrier layer in the prior art.

[0030] Figure 3 for Figure 2 Schematic diagram of the specific process of the mid-stripping aluminum rework method.

[0031] Figure 4 This is the aluminum stripping rework flow chart mentioned in the present invention when there is no barrier layer in the front layer.

[0032] Figure 5 The present invention provides a flow chart of aluminum stripping rework with a barrier layer.

[0033] Figure 6 It is a specific flow chart of a semiconductor wafer aluminum stripping rework method mentioned in the present invention. DETAILED DESCRIPTION

[0034] The present invention will be further explained below in conjunction with the accompanying drawings and related knowledge, and described clearly and completely. Obviously, the described application is only a part of the embodiments of the present invention, rather than all the embodiments.

[0035] The terms mentioned in the present invention are explained as follows:

[0036] Wet aluminum etching: Use corrosive liquid to corrode the aluminum layer on the surface of the immersed wafer.

[0037] Dry aluminum etching: The aluminum layer is etched by plasma.

[0038] Rinsing: It is commonly used to clean the natural oxide layer formed on the surface of single crystal silicon. In the present invention, the silicon slag on the surface of the silicon layer is loosened, so that the silicon slag can be removed by brushing and wiping. 16:1 BHF solution is commonly used.

[0039] Wet silicon slag sweeping: remove the silicon slag remaining after the aluminum layer is corroded. Commonly used wet silicon slag sweeping methods on the market include HAC 10%(W): HN03 2%(W): H3P04 71%(W): HBF4 3%(W), and dry silicon slag sweeping methods are also available.

[0040] Dry sweeping of silicon slag: CF4&O2 is commonly used to produce plamsa to etch silicon slag.

[0041] Visual inspection: Use a microscope to check for defects on the wafer surface.

[0042] Aluminum sputtering: Aluminum film is deposited on the wafer surface by physical deposition sputtering.

[0043] Flowing water wiping: Remove particles from the wafer surface through a wafer cleaning machine with forward and reverse ultrasonic flowing water cleaning, brush cleaning and other functions.

[0044] Reference Figure 1As shown, taking the process of some six- to eight-inch line products where there is no barrier layer before the sputtering of the thick aluminum layer 1, and the direct front layer is the silicon layer 2 as an example, in the prior art, wet aluminum etching is first performed, and then wet silicon slag 3 is swept. Since the front layer is also silicon, the front layer will be directly damaged, and the wet silicon slag sweeping cannot be removed cleanly when there is a lot of silicon slag. If the dry method is used to remove the silicon slag 3, the silicon layer 2 will also be damaged. If you choose to skip the wet silicon slag sweeping or dry silicon slag sweeping, a small amount of silicon remaining after the aluminum is corroded will be embedded in the surface of the front silicon layer, which cannot be removed by running water wiping. The subsequent growth of aluminum will make the surface full of dense black spots. Therefore, generally, when there is no barrier layer in the front layer, if there is an abnormality in the microscope inspection, it will be chosen to continue the wafer or scrap it according to the severity, but this will greatly affect the yield of the product;

[0045] Similarly, refer to Figure 2 , Figure 3 As shown, if there is a barrier layer, the barrier layer is TI layer 4 + TIN layer 5 as the barrier layer. The traditional process is firstly carried out by wet aluminum etching, and then wet silicon slag is swept. At least 20 front water wipes are required, and the wet aluminum etching process causes serious side corrosion.

[0046] Based on the above problems, the present invention is proposed. Figure 4 , Figure 6 As shown, a semiconductor wafer aluminum stripping rework method comprises the following steps:

[0047] S1: Provide a semiconductor wafer, the semiconductor wafer includes an aluminum layer 1 and a silicon layer 2 located under the aluminum layer. The structure is that the front layer (silicon layer 2) has no barrier layer and cannot be stripped for aluminum rework. After aluminum sputtering, microscopic inspection finds that the surface of the aluminum layer is abnormal (such as roughness, black spots on the surface caused by water and air leakage in the cavity, and silicon precipitation caused by staying in the high-temperature cavity for too long, etc.), and the traditional aluminum stripping rework process will be chosen;

[0048] S2: Dry aluminum etching is performed on a part of the aluminum layer by a dry method. The present invention to be explained firstly performs two functions by etching a part of the aluminum layer and performing dry aluminum etching. Firstly, most of the aluminum layer 1 can be quickly removed by dry aluminum etching, and dry aluminum etching can also avoid the situation where serious side corrosion caused by wet aluminum etching process occurs;

[0049] S3: Dry-sweep the etched semiconductor wafer for silicon slag 3, and then wipe the etched semiconductor wafer with ultrasonic water flow. In this step, the etched semiconductor wafer is dry-sweep the silicon slag to achieve rapid removal of the front part of the silicon slag 3, and wipe the etched semiconductor wafer with ultrasonic water flow. The present invention uses dry etching to not completely remove the aluminum film, leaving about one-sixth of the aluminum film, so that neither dry aluminum etching nor dry sweeping of silicon slag will affect the front layer, and there is a residual aluminum film blocking it, and there is no need to worry about the surface quality of the aluminum film, and the wet method will be used to continue aluminum stripping later; and the dry sweeping of silicon slag has a strong etching ability, which makes up for the shortcomings of wet sweeping of silicon slag, which has a mild reaction and is difficult to remove a large amount of silicon slag;

[0050] S4: wet aluminum etching is performed on the remaining aluminum layer 1. In this step, wet etching has the characteristic of isotropy. In the present invention, the film etched by wet aluminum etching is made as thin as possible to reduce the time of side corrosion. Therefore, most of the aluminum is etched by dry aluminum etching. Dry etching is anisotropic and can control the etching direction. In the present invention, it is not necessary to completely remove the aluminum film by dry etching, and about one-sixth of the aluminum film is left. In this way, neither dry aluminum etching nor dry silicon slag sweeping will affect the previous layer, and there is a residual aluminum film blocking it, and there is no need to worry about the surface quality of the aluminum film. The wet method will be used to continue aluminum stripping later;

[0051] S5: Rinse the semiconductor wafer after wet aluminum etching and wipe it with running water with a brush. If it is qualified, aluminum sputtering is performed. If it is unqualified, rinse it again and wipe it with running water with a brush until it is qualified. The present invention uses segmented aluminum stripping. In the first step, most of the aluminum and its residual silicon are removed by highly efficient dry aluminum etching and dry silicon slag sweeping. Only a small part of the aluminum remains in the second step of wet etching, and the residual silicon slag is also less, which greatly improves the efficiency of rinsing and running water wiping to sweep silicon slag. If segmented aluminum stripping is not used, the residual silicon in 4000nm AlSiCu must be rinsed and wiped with running water for at least 20 times. However, the number of cycles of segmented aluminum stripping, rinsing and running water wiping can be achieved within about 5 times, and it can be removed completely.

[0052] The present invention first uses the process of segmented aluminum stripping, combined with dry sweeping of silicon slag (which can quickly remove silicon slag), and then uses rinsing and brush water wiping. Through the combination of the above three processes, the efficiency of aluminum stripping can be improved, rework time can be reduced, and it can play a great role in increasing production capacity and improving product yield. It should be noted that in the present invention, the brush water wiping method is not limited to the front water flow and brush of the wiping machine to remove the loose silicon slag, but also includes other forms of water wiping equipment that can loosen the silicon slag, and the silicon slag on the surface of the silicon layer is loosened by rinsing; and the rinsing process is not used in the prior art.

[0053] In the present invention, reference is made to Figure 5 As shown, the semiconductor wafer also includes a barrier layer, and the barrier layer is located between the aluminum layer 1 and the silicon layer 2. In some embodiments, the barrier layer includes a TI layer or a TI layer 4+TIN layer 5, that is, the present invention is also suitable for aluminum stripping rework in the presence of a barrier layer. Moreover, the current aluminum etching process rarely uses dry etching, because whether the front layer has a barrier layer or not, the front layer will be lost by dry plasma etching, but the present solution distributes the aluminum stripping method so that the dry etching does not damage the aluminum front layer, so the process of the present invention is also applicable to the presence of a barrier layer; it should be further explained that in the presence of a barrier layer, firstly, dry aluminum etching is performed on part of the aluminum layer 1 by dry method, and dry silicon slag is swept on the etched semiconductor wafer by dry method, and ultrasonic water wiping is performed after sweeping the silicon slag 3, and wet aluminum etching is performed on the remaining part of the aluminum layer 1, and wet aluminum etching is performed after wet aluminum etching, and then wet silicon slag 3 is swept, and then water wiping is performed, and aluminum sputtering is performed if it is qualified, and water wiping is performed again if it is unqualified until it is qualified. Because there is a barrier layer, wet sweeping of silicon slag will not damage the barrier layer. In this solution, rinsing and brushing with running water are not used. In this implementation, generally 1-5 times of running water wiping can pass. If segmented aluminum stripping is not used, at least 20 times of rinsing and brushing with running water are required to remove the residual silicon in 4000nm AlSiCu. However, segmented aluminum stripping is used, and finally the silicon slag is swept by wet method, and the running water wiping is 1-5 times to remove it completely, which greatly improves the efficiency.

[0054] In the present invention, dry aluminum etching is performed on a portion of the aluminum layer by a dry method, and the portion of the aluminum layer accounts for 1%-99% of the entire aluminum layer. That is to say, the present invention adopts a segmented aluminum stripping method, and the first step is dry aluminum etching, which can avoid side corrosion, and the removal speed is faster than the wet method. The second time, the wet method is used to remove the remaining aluminum layer. Since the remaining aluminum layer accounts for a very low proportion, the corrosion speed is also efficient, and the underlying silicon does not need to be damaged.

[0055] In the present invention, dry aluminum etching is performed on a portion of the aluminum layer by a dry method, and the portion of the aluminum layer preferably occupies 5 / 6 of the entire aluminum layer. By using dry etching, the aluminum film is not completely removed, and about one-sixth of the aluminum film is left. In this way, neither dry aluminum etching nor dry silicon slag sweeping will affect the previous layer, and there is a residual aluminum film to block it, and there is no need to worry about the surface quality of the aluminum film, and the wet method will be used to continue stripping the aluminum later.

[0056] In the present invention, step S1 also includes testing the provided semiconductor wafer. If the aluminum layer is qualified, the next step of wafer taping is carried out. If it is unqualified, aluminum stripping and rework are carried out.

[0057] The following provides specific embodiments of the present invention. Example 1

[0058] Reference Figure 4 , Figure 6 As shown, a semiconductor wafer aluminum stripping rework method comprises the following steps:

[0059] S1: providing a semiconductor wafer, the semiconductor wafer comprising an aluminum layer 1 and a silicon layer 2 located under the aluminum layer. This embodiment is described by taking a non-barrier layer as an example. By testing the provided semiconductor wafer, if the aluminum layer is qualified, the next step of wafer taping is performed, and if it is unqualified, aluminum stripping rework is performed;

[0060] S2: Dry aluminum etching is performed on part of the aluminum layer by dry method. In the prior art, current aluminum etching processes rarely use dry etching, because no matter whether the front layer has a barrier layer or not, the front layer will be lost by dry plasma etching, and the dry silicon slag selection is relatively low. The present invention uses dry etching to not completely remove the aluminum film, leaving about one-sixth of the aluminum film, so that neither dry aluminum etching nor dry silicon slag sweeping will affect the front layer, there is residual aluminum film blocking, and there is no need to worry about the surface quality of the aluminum film. The wet method will be used to continue aluminum stripping later, which solves the damage to the front layer caused by dry etching and dry silicon slag sweeping;

[0061] S3: Dry-sweeping the etched semiconductor wafer with silicon slag, and then performing ultrasonic water wiping. The dry-sweeping of silicon slag has a strong etching ability, which makes up for the disadvantage of the wet-sweeping of silicon slag, which has a mild reaction and is difficult to remove a large amount of silicon slag;

[0062] S4: Wet aluminum etching is performed on the remaining aluminum layer, and the film etched by wet aluminum etching is made as thin as possible, so as to reduce the time of side corrosion. Therefore, most of the aluminum is etched by dry aluminum etching. Dry etching is anisotropic and the etching direction can be controlled.

[0063] S5: After wet aluminum etching, the semiconductor wafer is rinsed and wiped with running water by a brush. If it is qualified, aluminum sputtering is performed. If it is unqualified, it is rinsed again and wiped with running water by a brush until it is qualified. Through segmented aluminum stripping, the first step is to remove most of the aluminum and its residual silicon through extremely efficient dry aluminum etching and dry silicon slag sweeping. In the second step, only a small part of the aluminum is wet-etched, and the residual silicon slag is also less, which greatly improves the efficiency of rinsing and running water wiping. If segmented aluminum stripping is not used, the residual silicon in 4000nm AlSiCu must be rinsed and wiped with running water at least 20 times. However, the number of cycles of segmented aluminum stripping, rinsing and running water wiping can be achieved within about 5 times, which can be completely removed, greatly improving efficiency.

[0064] In this embodiment, taking the reworked 4000nm AlSiCu as an example, if wet etching is used for aluminum, both silicon slag and the front silicon layer are silicon, and there is no reactant that only corrodes silicon slag but does not corrode the silicon substrate. Therefore, it is impossible to directly remove silicon slag by wet method without damaging the front silicon layer. However, in the present invention, when the front layer is completely exposed after aluminum etching, the silicon slag on the surface of the front silicon layer is loosened by rinsing, and the front water and brush of the wiper are used to remove the loose silicon slag, and the surface silicon slag can be removed until the standard is met by circulating rinsing and wiping with running water. The number of cleaning times is generally 1-5 times;

[0065] If the first step is to remove aluminum by wet method, firstly, since there are generally only 1-3 wafers that need to be stripped and reworked each time a problem occurs, the operation time of wet aluminum etching and silicon slag sweeping is only related to the thickness of the aluminum. The time for one wafer is the same as that for a whole box of 25 wafers, so it is a waste of time. And then, the loose silicon slag is removed by adding the front water flow and brush of the wafer wiper, which requires 20 cycles, and the time required is 40 minutes for wet aluminum removal and 30 minutes for wet silicon slag sweeping. In addition, in the absence of a barrier layer, the silicon layer will be damaged. Each of the 20 cleanings takes about 10 minutes, and the total cleaning time is about 200 minutes, which is more than 4 hours, and the efficiency is too low.

[0066] In the case of no barrier layer, the first step of the present embodiment is to perform dry aluminum etching on part of the aluminum layer by the dry method, and the time for each wafer is about 6 minutes. The semiconductor wafer after etching is dry-sweeped for silicon slag by the dry method, and the maximum time required for ultrasonic running water plus brush running water wiping after silicon slag sweeping is 20 minutes; the time for wet aluminum etching of the remaining aluminum layer is 10 minutes, and the time for rinsing the semiconductor wafer after wet aluminum etching and wiping it with a brush running water is 5 minutes, and the total time is about 45 minutes. If a batch of wafers that need to be stripped and reworked is greater than 1 wafer, the total time for each additional wafer will be increased by 10 minutes on the basis of 45 minutes. In addition, since there are generally only 1-3 wafers that need to be stripped and reworked each time a problem occurs, there are generally only 1-3 wafers that need to be stripped and reworked. In the case where there is no barrier layer in the front layer, the present invention can improve the efficiency of aluminum stripping and reduce rework time by stripping aluminum in sections, combining dry sweeping of silicon slag and wiping with a rinsing brush and running water, which can greatly play a role in increasing production capacity and improving product yield; the present invention overcomes the shortcomings of dry etching, improves wafer yield, reduces the number of scrapped wafers in the TF department, improves process stability, and increases production capacity; and directly solves the problem of scrapping caused by heavy sputtering of wafers without a barrier layer in the front layer that cannot be stripped of aluminum, and this solution has wider versatility.

[0067] The technical principle of the present invention is described above in combination with the specific embodiments, which are only preferred implementations of the present invention. The protection scope of the present invention is not limited to the above embodiments, and all technical solutions under the idea of ​​the present invention belong to the protection scope of the present invention. Those skilled in the art can think of other specific implementations of the present invention without creative work, and these methods will fall within the protection scope of the present invention.

Claims

1. A semiconductor wafer aluminum stripping rework method, characterized in that: The following steps are involved: S1: Providing a semiconductor wafer, wherein the semiconductor wafer comprises an aluminum layer; S2: dry aluminum etching of part of the aluminum layer by dry method; S3: Dry-cleaning the etched semiconductor wafer for silicon slag by dry method, and then performing ultrasonic water wiping on the wafer; S4: performing wet aluminum etching on the remaining aluminum layer; S5: If there is a silicon layer under the aluminum layer, the semiconductor wafer after wet aluminum etching is rinsed and wiped with running water by a brush. If it is qualified, aluminum sputtering is performed; if it is unqualified, it is rinsed again and wiped with running water by a brush until it is qualified. If there is a barrier layer under the aluminum layer, after wet aluminum etching, wet silicon slag is swept and then wiped with running water. If it is qualified, aluminum sputtering is performed; if it is unqualified, it is wiped with running water again until it is qualified.

2. A semiconductor wafer aluminum stripping rework method as claimed in claim 1, characterized in that: The barrier layer is located between the aluminum layer and the silicon layer.

3. A semiconductor wafer aluminum stripping rework method as claimed in claim 2, characterized in that: The barrier layer includes a TI layer or a TI layer + a TIN layer.

4. A semiconductor wafer aluminum stripping rework method as claimed in claim 3, characterized in that: The partial aluminum layer accounts for 1%-99% of the entire aluminum layer.

5. A semiconductor wafer aluminum stripping rework method as claimed in claim 4, characterized in that: The partial aluminum layer accounts for 5 / 6 of the entire aluminum layer.

6. A semiconductor wafer aluminum stripping rework method as claimed in claim 5, characterized in that: Step S1 also includes testing the provided semiconductor wafer. If the aluminum layer is qualified, the next step of wafer taping is carried out. If it is unqualified, aluminum stripping and rework are carried out.

7. A semiconductor wafer aluminum stripping rework method as claimed in claim 6, characterized in that: In step S2, the direction of aluminum corrosion is controlled by a dry method.

8. A semiconductor wafer aluminum stripping rework method as claimed in claim 7, characterized in that: By stripping aluminum in sections, most of the aluminum and its residual silicon are first removed by dry aluminum etching and dry silicon slag sweeping, and then the remaining aluminum is etched by wet etching.

9. A semiconductor wafer aluminum stripping rework method as claimed in claim 8, characterized in that: In step S5, the silicon slag is loosened by rinsing, and the loose silicon slag is removed by the front water flow and brush of the wafer cleaning machine.

Citation Information

Patent Citations

  • Method of aluminum film technology

    CN106847669A

  • Semiconductor device manufacturing method

    JP2013219102A

  • Recycling of a wafer comprising a multi-layer structure after taking-off a thin layer

    SG113895A1

  • Eliminating residual polymer in the cleaning process of post pad etching

    US20030196681A1

  • Process for fabricating a wiring layer of aluminum or aluminum alloy on semiconductor devices

    US4547260A