A solid catalyst, its preparation method and application
The butyraldehyde condensation reaction was carried out in a fixed-bed reactor using Ce/BaMnO3-Al2O3 solid catalyst, which solved the problems of wastewater pollution from liquid alkaline catalysts and insufficient stability of solid alkaline catalysts. This method achieved efficient butyraldehyde conversion and octenal selectivity, making it suitable for industrial production.
Patent Information
- Application Number
- CN202310212752.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-03-07
AI Technical Summary
Existing liquid alkaline catalysts cause wastewater pollution in the butyraldehyde-hydroxyl condensation reaction, and solid alkaline catalysts have shortcomings in stability and reusability, which limit their industrial application.
Octenal was prepared by butyraldehyde condensation reaction using a Ce/BaMnO3-Al2O3 solid catalyst in a fixed-bed reactor. The catalyst consisted of BaMnO3 and Al2O3, with Ce as the active component supported on it, and was prepared by an equal-volume impregnation method.
It improves the conversion rate of butyraldehyde and the selectivity of octenal, and the catalyst has good stability, making it suitable for large-scale production.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] This application relates to a solid catalyst, its preparation method, and its application, and belongs to the field of chemical engineering. Background Technology
[0002] Currently, industrially, butyraldehyde is produced via aldol condensation catalyzed by liquid NaOH. While aldol condensation under specific temperature and pressure yields high butyraldehyde conversion and octenal selectivity, the resulting wastewater contains octenal, sodium butyrate, and trace amounts of various aldehydes and sodium organic acids. The generated sodium organic acids corrode equipment, and direct discharge of the wastewater causes severe environmental pollution. Domestic research on butyraldehyde and octenal alcohol technology focuses on catalyst development. However, under the advocacy of green chemistry, the research and development of an environmentally friendly solid alkali catalyst that achieves zero pollution during preparation and use is of unique significance.
[0003] Solid base catalysts have become a focus of research due to their high activity, high selectivity, and ease of separation. Literature reports that solid base catalysts used for the aldol condensation of n-butyraldehyde are mainly metal oxides and supported organic solid bases, achieving activity and selectivity similar to liquid bases. However, their poor stability and difficulty in reusing hinder their industrial application. Solid acids have been reported in some aldol condensation reactions, demonstrating not only high catalytic activity but also good stability, showing broad prospects for industrial application. However, research reports on the application of solid acids in the self-condensation of n-butyraldehyde are limited. Summary of the Invention
[0004] This application constructs a solid catalyst Ce / BaMnO3-Al2O3, which is of great significance for developing a solid catalyst in the reaction of butyraldehyde condensation to prepare octenal using a fixed-bed reactor. The catalyst has good activity, high butyraldehyde conversion rate and octenal selectivity, and good stability.
[0005] According to one aspect of this application, a solid catalyst is provided, the catalyst having the composition Ce / BaMnO3-Al2O3. Al2O3 has a hollow structure.
[0006] Optionally, the content of BaMnO3 accounts for 4.7~9 wt% of the BaMnO3-Al2O3. The content of Al2O3 accounts for 91~95.3 wt% of the BaMnO3-Al2O3; The Ce content is 1 to 5 wt% of the BaMnO3-Al2O3.
[0007] Optionally, the content of BaMnO3 is any value or a range between 4.7 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, and 9 wt% of the BaMnO3-Al2O3.
[0008] Optionally, the content of Al2O3 is any value or a range between 91 wt%, 92 wt%, 93 wt%, 94 wt%, 95 wt%, and 95.3 wt% of the BaMnO3-Al2O3.
[0009] Optionally, the Ce content is any value among 1 wt%, 2 wt%, 3 wt%, 4 wt%, and 5 wt% of the BaMnO3-Al2O3, or any value between both.
[0010] According to another aspect of this application, a method for preparing a solid catalyst is provided, comprising the following steps: Includes the following steps: (1) The BaMnO3 and hollow alumina are mixed and calcined to obtain BaMnO3-Al2O3; (2) Ce was loaded onto BaMnO3-Al2O3 by equal volume impregnation method to obtain the catalyst.
[0011] Optionally, in step (1), the BaMnO3 is prepared by a hot alkali method, specifically including the following steps: The mixture I containing barium source, manganese source and alkali is heated in stages, washed, filtered and dried to obtain BaMnO3; The segmented heating includes a first-stage heating and a second-stage heating performed sequentially.
[0012] Optionally, the barium source is selected from at least one of barium nitrate and barium sulfate; The manganese source is selected from manganese dioxide; The alkali is selected from at least one of sodium hydroxide and potassium hydroxide.
[0013] Optionally, the molar ratio of the barium source to the manganese source is 1:0.9~1, based on the molar ratio of barium in the barium source to manganese in the manganese source.
[0014] Optionally, the molar ratio of the barium source to the manganese source is selected from any value among 1:0.9, 1:0.95, and 1:1, or a range between the two values.
[0015] Optionally, the molar ratio of the barium source to the alkali is 1:300-400, wherein the barium element in the barium source and the OH group in the alkali are... - The molar timer.
[0016] Optionally, the molar ratio of the barium source to the alkali is selected from any value among 1:300, 1:350, and 1:400, or a range between two values.
[0017] Optionally, the temperature of the first heating stage is 160~240℃, and the heating time is 0.2~0.5h; The temperature of the two-stage heating is 160~240℃, and the heating time is 12~48h.
[0018] Optionally, the temperature of the heating segment is selected from any value or a range between 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, and 240℃.
[0019] Optionally, the heating time is selected from any value of 0.2h, 0.3h, 0.4h, 0.5h or a range between any two.
[0020] Optionally, the temperature of the two-stage heating is any value or a range between 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, and 240℃.
[0021] Optionally, the heating time for the two stages is any value among 12h, 18h, 24h, 30h, 36h, 42h, and 48h, or a range between any two.
[0022] Optionally, the solvent used for washing is water.
[0023] Optionally, the drying temperature is 60~120℃, and the drying time is 12~18h.
[0024] Optionally, the drying temperature is any value among 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, and 120℃, or a range between any two.
[0025] Optionally, the drying temperature is any value among 12h, 13h, 14h, 15h, 16h, and 17h, or a range between any two.
[0026] Optionally, in step (1), the hollow alumina is prepared using carbon spheres as a template agent, and the specific steps are as follows: The mixture II containing Al(NO3)3, ethanol and carbon spheres was ultrasonically dispersed, allowed to stand, filtered, dried (I), and calcined (II) to obtain hollow alumina.
[0027] Optionally, the solid-liquid ratio of the carbon spheres, Al(NO3)3, and ethanol is 1:30~50:200~300 g / ml.
[0028] Optionally, the solid-liquid ratio of the carbon spheres, Al(NO3)3, and ethanol is selected from any value or a range between two values from 1:30:200 g / ml, 1:35:220 g / ml, 1:40:250 g / ml, 1:45:270 g / ml, and 1:50:300 g / ml.
[0029] Optionally, the ultrasonic dispersion time is 10~60 min.
[0030] Optionally, the ultrasonic dispersion time is selected from any value or a range between 10 min, 20 min, 30 min, 40 min, 50 min, and 60 min.
[0031] Optionally, the settling time is 4 to 10 hours.
[0032] Optionally, the settling time is any value among 4h, 5h, 6h, 7h, 8h, 9h, and 10h, or a range between any two.
[0033] Optionally, the temperature of the drying process I is 100~120℃, and the drying time is 6~12h.
[0034] Optionally, the temperature of the drying process I is any value among 100°C, 110°C, and 120°C, or a range between any two.
[0035] Optionally, the drying time I is any value among 6h, 7h, 8h, 9h, 10h, 11h, and 12h, or a range between any two.
[0036] Optionally, the temperature of calcination II is 500~600℃, and the time of calcination I is 4~8h.
[0037] Optionally, the calcination temperature II is any value among 500°C, 550°C, and 600°C, or a range between any two.
[0038] Optionally, the calcination time II is any value among 4h, 5h, 6h, 7h, and 8h, or a range between any two.
[0039] Optionally, in step (1), the mixing method is selected from mechanical mixing or wet mixing.
[0040] Optionally, the mass ratio of BaMnO3 to hollow alumina is 1:10~20.
[0041] Optionally, the mass ratio of BaMnO3 to hollow alumina is any value among 1:10, 1:15, and 1:20, or any range between the two.
[0042] Optionally, the calcination temperature I is 500~600℃, and the calcination time I is 4~8h.
[0043] Optionally, the calcination temperature I is any value among 500°C, 550°C, and 600°C, or a range between any two.
[0044] Optionally, the calcination time I is any value among 4h, 5h, 6h, 7h, and 8h, or a range between any two.
[0045] Optionally, in step (2), the specific steps for loading Ce onto the BaMnO3-Al2O3 using the equal-volume impregnation method are as follows: The Ce source aqueous solution was added to BaMnO3-Al2O3, aged, dried (II), and calcined (III) to obtain the Ce / BaMnO3-Al2O3 catalyst.
[0046] Optionally, the Ce source aqueous solution is an aqueous solution of cerium nitrate.
[0047] Optionally, the aging temperature is 25~30℃, and the aging time is 18~24h.
[0048] Optionally, the aging temperature is any value among 25°C, 26°C, 27°C, 28°C, 29°C, and 30°C, or a range between any two.
[0049] Optionally, the aging time is any value among 18h, 19h, 20h, 21h, 22h, 23h, and 24h, or a range between any two.
[0050] Optionally, the temperature of the second drying step is 100~120℃, and the drying time is 6~12h.
[0051] Optionally, the temperature of the drying II is any value among 100°C, 110°C, and 120°C, or a range between any two.
[0052] Optionally, the drying time II is any value among 6h, 7h, 8h, 9h, 10h, 11h, and 12h, or a range between any two.
[0053] Optionally, the temperature of calcination III is 500~600℃, and the calcination time of calcination III is 4~8h.
[0054] Optionally, the calcination temperature III is any value among 500°C, 550°C, and 600°C, or a range between any two.
[0055] Optionally, the calcination time III is any value among 4h, 5h, 6h, 7h, and 8h, or a range between any two.
[0056] According to another aspect of this application, A method for preparing octenal by butyraldehyde condensation reaction is provided, wherein butyraldehyde is contacted with a catalyst and reacted to obtain the octenal; The catalyst is selected from the above-described catalysts or the catalysts obtained according to the above preparation method.
[0057] Optionally, the reaction conditions are: temperature 100~200℃, pressure 1~5MPa, and time 3~5h.
[0058] Optionally, the temperature of the reaction is any value or a range between 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C.
[0059] Optionally, the reaction time is any value among 3h, 4h, and 5h, or a range between any two.
[0060] Optionally, the pressure of the reaction is any value of 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, or a range between any two.
[0061] Optionally, the space time of the butyraldehyde is 0.1 ~ 10 g·min / ml.
[0062] Optionally, the space time of the butyraldehyde is any value or a range between 0.1 g·min / ml, 0.5 g·min / ml, 1 g·min / ml, 2 g·min / ml, 3 g·min / ml, 4 g·min / ml, 5 g·min / ml, 6 g·min / ml, 7 g·min / ml, 8 g·min / ml, 9 g·min / ml, and 10 g·min / ml.
[0063] The reaction described in this application is carried out in a fixed-bed reactor, and the catalyst is packed in the fixed-bed reactor.
[0064] The beneficial effects that this application can produce include: 1) The catalyst provided in this application can be applied to the butyraldehyde condensation reaction to prepare octenal, and improves the conversion rate of butyraldehyde and the selectivity of the generated octenal.
[0065] 2) The preparation method of the catalyst provided in this application is stable, controllable and reproducible.
[0066] 3) The method for preparing octenal by butyraldehyde condensation provided in this application uses the catalyst provided in this application, which has a fast reaction rate and high yield, and can be applied to large-scale production. Attached Figure Description
[0067] Figure 1 Catalyst 1 # X-ray powder diffraction pattern of BaMnO3. Detailed Implementation
[0068] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.
[0069] Unless otherwise specified, the raw materials and catalysts used in the embodiments of this application were all purchased commercially. The gas chromatograph used was an Agilent 7890B gas chromatograph.
[0070] The conversion rate and selectivity calculation formulas in the embodiments of this application are as follows (with butyraldehyde conversion rate as the evaluation index): Butyraldehyde conversion rate = (initial carbon number of butyraldehyde - carbon number of butyraldehyde in the product) 100 / initial molar number of butyraldehyde Octenal selectivity = number of carbon atoms in octenal 100 / ∑ (number of carbon atoms in octenal + number of carbon atoms in other products).
[0071] Example 1 Preparation of catalysts Taking item 1 in Table 1 as an example, barium nitrate and manganese dioxide with a barium to manganese molar ratio of 1:1 are mixed with alkali (NaOH and KOH) (the barium element in the barium source and the OH- in the alkali) - The mixture (with a molar ratio of 1:350) was placed in a polytetrafluoroethylene container and heated in a 200 ℃ oven for 0.5 h; then removed and stirred, and heated in a 200 ℃ oven for 24 h. After cooling, it was washed with deionized water, filtered, and dried in a 60 ℃ oven for 12 h to obtain the BaMnO3 mixture.
[0072] Weigh Al(NO3)39H2O and add anhydrous ethanol solution (the solid-liquid ratio of carbon spheres, Al(NO3)39H2O, and anhydrous ethanol is 1:40:250 g / ml) to prepare an aluminum nitrate ethanol solution. Add carbon spheres, sonicate for 30 min, and let stand for 8 h. Filter and dry at 100 ℃ for 10 h, then calcine at 550 ℃ for 4 h to obtain hollow alumina.
[0073] A mixture of BaMnO3 and hollow alumina was wet-mixed at a mass ratio of 1:15 and calcined at 550℃ for 4 h to obtain BaMnO3-Al2O3. A 3 wt% cerium nitrate aqueous solution was then added to the BaMnO3-Al2O3 mixture, and the mixture was aged at 25℃ for 24 h, dried at 100℃ for 10 h, and calcined at 550℃ for 4 h to obtain Ce / BaMnO3-Al2O3, denoted as catalyst 1. # .
[0074] Following the steps below, adjust the type and amount of each raw material and the reaction parameters to obtain a series of catalysts numbered 2 to 28, denoted as catalyst 2. # ~Catalyst 28 # As shown in Table 1 below: Table 1
[0075] Table 2
[0076] Table 3
[0077] The explanations for each column in Table 1-3 above are as follows: Barium sources: barium nitrate (Ba1), barium sulfate (Ba2).
[0078] Manganese source: manganese dioxide (Mn).
[0079] Bases: NaOH (Na), KOH (K), NaOH and KOH (NaK).
[0080] Ce source: cerium nitrate (Ce).
[0081] First heating stage: The first heating stage in the preparation of BaMnO3.
[0082] Second-stage heating: The second heating process in the preparation of BaMnO3.
[0083] Drying I: Drying during the preparation of hollow alumina.
[0084] Drying II: Drying during the preparation of Ce / BaMnO3-Al2O3 catalyst.
[0085] Calcination I: Calcination during the preparation of BaMnO3-Al2O3 catalyst.
[0086] Calcination II: Calcination during the preparation of hollow alumina.
[0087] Calcination III: Calcination during the preparation of Ce / BaMnO3-Al2O3 catalyst.
[0088] Mixing methods: mechanical mixing (method 1), wet mixing (method 2).
[0089] XRD characterization Catalyst 1 was analyzed using a Miniflex 600 X-ray diffractometer with a Cu target. # Powder diffraction yielded catalyst 1. # The diffraction peaks of BaMnO3 conform to the characteristic peaks of BaMnO3 (e.g., Figure 1 (As shown).
[0090] Gas chromatography characterization The composition of the butyraldehyde condensation reaction products was analyzed using an Agilent 7890B gas chromatograph (FID detector, HP-5 capillary column).
[0091] Example 2 The catalyst is used in the butyraldehyde condensation reaction to prepare octenal.
[0092] Catalysts 1-28 prepared in Example 1 # ~Catalyst 28 # The catalyst is used to prepare octenal by butyraldehyde condensation. The reaction is carried out at a temperature of 180°C, a reaction time of 4 hours, a reaction pressure of 2 MPa, and a raw material space time of 1 g·min / ml. The raw material is fed into a fixed-bed reactor carrying 3 g of the catalyst to produce octenal by condensation reaction.
[0093] After the reaction stabilized, both the reactants and products were analyzed using online gas chromatography. The results are shown in Table 4.
[0094] Table 4
[0095] Example 3 Catalyst 1 prepared in Table 1-3 # The reaction to prepare octenal by butyraldehyde condensation was carried out. After the reaction parameters were changed and the reaction stabilized, the reactants and products were analyzed by online gas chromatography. The reaction results are shown in Table 5.
[0096] Table 5
[0097] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A solid catalyst, characterized in that, The solid catalyst is composed of Ce / BaMnO3-Al2O3, wherein Al2O3 has a hollow structure, and the content of BaMnO3 accounts for 4.7~9 wt% of the BaMnO3-Al2O3. The content of Al2O3 accounts for 91~95.3 wt% of the BaMnO3-Al2O3; The Ce content is 1 to 5 wt% of the BaMnO3-Al2O3.
2. The method for preparing the solid catalyst according to claim 1, characterized in that, Includes the following steps: (1) The BaMnO3 and hollow alumina are mixed and calcined to obtain BaMnO3-Al2O3; (2) Ce was loaded onto BaMnO3-Al2O3 by equal volume impregnation method to obtain the catalyst.
3. The preparation method according to claim 2, characterized in that, In step (1), the BaMnO3 is prepared by a hot alkali method, the specific steps of which include: The mixture I containing barium source, manganese source and alkali is heated in stages, washed, filtered and dried to obtain BaMnO3; The segmented heating includes a first-stage heating and a second-stage heating performed sequentially.
4. The preparation method according to claim 3, characterized in that, The barium source is selected from at least one of barium nitrate and barium sulfate; The manganese source is manganese dioxide; The alkali is at least one of sodium hydroxide and potassium hydroxide.
5. The preparation method according to claim 4, characterized in that, The molar ratio of the barium source to the manganese source is 1:0.9~1, and the molar ratio of the barium element in the barium source to the manganese element in the manganese source is 1:300~400, based on the molar ratio of the barium element in the barium source to the OH element in the manganese source. - The molar timer.
6. The preparation method according to claim 4, characterized in that, The temperature of the first heating stage is 160~240℃, and the heating time is 0.2~0.5h; The temperature of the two-stage heating is 160~240℃, and the heating time is 12~48h.
7. The preparation method according to claim 4, characterized in that, In the washing step, the washing solvent is water.
8. The preparation method according to claim 4, characterized in that, The drying temperature is 60~120℃, and the drying time is 12~18 h.
9. The preparation method according to claim 2, characterized in that, In step (1), the hollow alumina is prepared using carbon spheres as a template agent. The specific steps are as follows: The mixture II containing Al(NO3)3, ethanol and carbon spheres was ultrasonically dispersed, allowed to stand, filtered, dried (I), and calcined (II) to obtain hollow alumina.
10. The preparation method according to claim 9, characterized in that, The solid-liquid ratio of the carbon spheres, Al(NO3)3, and ethanol is 1:30~50:200~300 g / ml.
11. The preparation method according to claim 9, characterized in that, The ultrasonic dispersion time is 10~60 min; The settling time is 4 to 10 hours.
12. The preparation method according to claim 9, characterized in that, The temperature of drying I is 100~120℃, and the drying time is 6~12 h; The calcination temperature II is 500~600℃, and the calcination time II is 4~8h.
13. The preparation method according to claim 2, characterized in that, In step (1), the mixing method is selected from mechanical mixing or wet mixing.
14. The preparation method according to claim 13, characterized in that, The mass ratio of BaMnO3 to hollow alumina is 1:10~20.
15. The preparation method according to claim 13, characterized in that, The calcination temperature I is 500~600℃, and the calcination time I is 4~8h.
16. The preparation method according to claim 2, characterized in that, In step (2), the specific steps for loading Ce onto BaMnO3-Al2O3 using the equal-volume impregnation method are as follows: The Ce source aqueous solution was added to BaMnO3-Al2O3, aged, dried (II), and calcined (III) to obtain the Ce / BaMnO3-Al2O3 catalyst; the Ce source aqueous solution was a cerium nitrate aqueous solution.
17. The preparation method according to claim 16, characterized in that, The aging temperature is 25~30℃, and the aging time is 18~24h.
18. The preparation method according to claim 16, characterized in that, The temperature of the second drying process is 100~120℃, and the drying time is 6~12h.
19. The preparation method according to claim 16, characterized in that, The calcination temperature III is 500~600℃, and the calcination time III is 4~8h.
20. A method for preparing octenal by butyraldehyde condensation reaction, characterized in that, Butyraldehyde is reacted with a catalyst to obtain octenal; The catalyst is selected from the solid catalyst of claim 1 or the solid catalyst obtained by the preparation method according to any one of claims 2 to 19.
21. The method according to claim 20, characterized in that, The reaction conditions are: temperature 100~200℃, pressure 1~5Mpa, time 3~5h; the space time of butyraldehyde is 0.1~10 g·min / ml.
Citation Information
Patent Citations
Catalyst, preparation method of catalyst and preparation method of 2-ethyl hexanal
CN107930647A
Method for one-step synthesis of isooctanal by catalyzing n-butyraldehyde with solid catalyst