Alumina-supported composite catalyst and its preparation method and application

By forming a three-dimensional hollow porous structure on the alumina support, combining proton-type heteropoly acids and active metal components, the problem of insufficient activity of alumina-supported heteropoly acid catalyst is solved, and the efficiency and stability of the catalyst are improved.

CN118616096BActive Publication Date: 2024-11-22ZHEJIANG UNIV +1

Patent Information

Application Number
CN202411095757.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The active sites of existing aluminum oxide-supported heteropolyacid catalysts are insufficiently exposed, the catalytic activity is insufficient, and the metal-heterolyacid synergistic effect is not significant, resulting in poor catalytic performance.

Method used

Alumina support with a three-dimensional hollow porous structure is adopted, and the proton-type heteropolyacid dispersed in a single molecule state and the active metal components dispersed in a single atom state are connected by covalent bonds and chemical bonds to form a stable composite catalyst structure.

Benefits of technology

The catalytic activity and stability of the catalyst are significantly improved, and the excellent performance of the catalytic reaction is achieved. The preparation method is simple, the cost is low, and the parameters are adjustable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118616096B_ABST
    Figure CN118616096B_ABST
Patent Text Reader

Abstract

The invention discloses an alumina-supported composite catalyst and a preparation method and application thereof. The composite catalyst comprises an alumina carrier, a heteropoly acid dispersed in a single molecule state and connected to the alumina carrier, and an active metal component dispersed in a single atom state and connected to one or both of the heteropoly acid and the alumina carrier. The heteropoly acid is a proton-type heteropoly acid capable of providing hydrogen ions, and the alumina carrier has a three-dimensional hollow porous structure. During the preparation, an alumina precursor and an active metal precursor are respectively used as raw materials, and they are subjected to conversion reaction with the proton-type heteropoly acid in the presence of water, calcined, and reduced to obtain the catalyst. The invention overcomes the problem in the prior art that the active sites of the metal and the heteropoly acid cannot be fully utilized, has the advantages of excellent catalytic activity, good stability, long service life, and the like, and is suitable for use in reactions such as alkylation, esterification, hydrogenation, and amination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to an alumina-supported composite catalyst and a preparation method and application thereof. Background Art

[0002] Heteropolyacids (POMs) are formed by heteroatoms (such as P, Si, Fe, Co, etc.) and polyatoms (such as Mo, W, V, Nb, Ta, etc.) coordinated and bridged by oxygen atoms. Heteropolyacids are not only acidic but also redox-sensitive, and are a new type of multifunctional catalyst. However, since heteropolyacids are non-porous solid substances (with a specific surface area of ​​less than 10 m 2 / g), when heteropolyacids are used directly as catalysts, due to their small specific surface area, the exposed acid active sites are limited, and non-polar reactants cannot enter their bulk phase, resulting in insufficient catalytic activity and difficulty in separating homogeneous reaction catalysts.

[0003] It is known that immobilizing heteropolyacids on a carrier helps to achieve homogeneous heterogeneity, making the catalyst easy to recover, reducing corrosion and significantly increasing the specific surface area, and enhancing the mechanical strength and thermal stability of the catalyst. Alumina is one of the commonly used catalyst carriers, and heteropolyacids have been reported in many papers. However, the catalytic activity of heteropolyacids supported on alumina reported is still unsatisfactory. For example, it still needs to be carried out at a higher temperature or under pressure. In addition, it is still a challenge to stabilize the heteropolyacid on alumina and minimize its loss.

[0004] Chinese patent document CN117138812A discloses a composite nano catalyst and a preparation method thereof, which can catalyze the hydrolysis of aluminum precursors and promote the generation of five-coordinated aluminum sites by in-situ introduction of polyoxometalates during the synthesis of porous nano alumina carriers, so that polyoxometalates can be in-situ anchored in the process of generating five-coordinated aluminum sites, thereby enabling polyoxometalates to stably exist on porous nano alumina carriers. However, the reaction catalyzed by the composite nano catalyst, such as the selective oxidation reaction of 2-methylbutyraldehyde, still needs to be carried out at 80°C and under pressure. In addition, it can be seen from the multiple schemes disclosed in the document that when the polyoxometalates used are in the form of salts such as ammonium phosphomolybdate and sodium phosphotungstate, the prepared catalyst has higher activity and selectivity than the acid form such as phosphomolybdic acid and phosphotungstic acid. Since the polyoxometalates in the form of salts usually have higher costs than the acid form, this also means that the pursuit of higher activity and selectivity will have to pay higher costs accordingly.

[0005] It is also known that metal-heteropolyacid composite bifunctional catalysts can theoretically achieve the synergistic catalytic effect of acidic active centers and metal active centers by introducing metal active species into the acidic catalyst system, so that such catalysts have broad application prospects in oxidation reactions, dehydrogenation reactions and hydrogenation reactions. However, the realization of the synergistic effect of metal-heteropolyacids in specific catalysts, especially the realization of significant synergistic effects, is quite difficult. The literature (Angew. Chem. Int. Ed. 2016, 55, 8319-8323) reported that metal Pt was loaded on the surface of phosphomolybdic acid heteropolyacid in the form of a single atom, and the literature (Angew. Chem. Int. Ed. 2023, e202218265) reported that metal Pd was loaded on the surface of silicomolybdic acid heteropolyacid in the form of a single atom, but the two still failed to achieve a satisfactory and significant synergistic effect. Some literature also reports the further compounding of metals on the basis of heteropolyacids supported on carriers. However, in such a more complex catalyst system, the realization of the synergistic effect of metals and heteropolyacids faces greater uncertainty.

[0006] In summary, it is still necessary to conduct in-depth research on issues related to heteropolyacid catalysts in order to develop catalysts with better performance. Summary of the invention

[0007] The problem to be solved by the present invention is to provide a novel alumina-supported composite catalyst with excellent performance and a simple and controllable preparation method for the catalyst.

[0008] The present invention also provides the use of the novel alumina-supported composite catalyst in an acid catalytic system or a selective catalytic reaction, especially in oxidation reactions, dehydrogenation reactions, hydrogenation reactions and the like, which has a significantly better catalytic effect.

[0009] In order to solve the above technical problems, a technical solution adopted by the present invention is:

[0010] An alumina-supported composite catalyst comprises an alumina carrier, a heteropolyacid dispersed in a single molecule state and connected to the alumina carrier, and an active metal component dispersed in a single atom state and connected to one or both of the heteropolyacid and the alumina carrier, wherein the heteropolyacid is a proton-type heteropolyacid capable of providing hydrogen ions, and the alumina carrier has a three-dimensional hollow porous structure.

[0011] According to the present invention, in the proton-type heteropolyacid, heteroatoms and polyatoms are coordinated and bridged by oxygen atoms, the heteroatoms include at least one selected from P, Si, Fe, and Co, and the polyatoms include at least one selected from Mo, W, V, Nb, and Ta.

[0012] In some preferred embodiments of the present invention, in the composite catalyst, the proton-type heteropoly acid is connected to the alumina carrier at least through a covalent bond.

[0013] Furthermore, a covalent bond is formed between the polyatoms in the proton-type heteropolyacid, the terminal oxygen in the proton-type heteropolyacid and the aluminum atom in the alumina carrier.

[0014] In some preferred embodiments of the present invention, the proton-type heteropoly acid is uniformly dispersed in the skeleton, inside the pores and on the surface of the alumina carrier.

[0015] In some preferred embodiments of the present invention, the active metal component is connected to the proton-type heteropolyacid via a chemical bond, wherein the chemical bond comprises a coordination bond, and the active metal component is also selectively adsorbed on the alumina carrier.

[0016] In some preferred embodiments of the present invention, the pores in the three-dimensional hollow porous structure are discretely distributed in the three-dimensional direction.

[0017] In the present invention, the three-dimensional hollow porous structure has a single hollow chamber or a cavity combination formed by a plurality of hollow chambers gathered in a connected state or a partially connected state.

[0018] In some preferred embodiments of the present invention, the diameter of the hollow chamber or the cavity combination is 1-90 nm; or, the ratio of the diameter of the hollow chamber or the cavity combination to the particle size of the alumina-supported composite catalyst is 0.3-0.9:1.

[0019] In some preferred embodiments of the present invention, the average pore diameter of the alumina-supported composite catalyst is 2-30 nm, and the average pore volume is 0.4-1.5 cc / g.

[0020] In some preferred embodiments of the present invention, the average density of the alumina-supported composite catalyst is 0.5-4.0 g / cm 3 .

[0021] According to the present invention, the particle size of the composite catalyst of the present invention can be made relatively smaller, and a shorter mass transfer path can be achieved. In some preferred embodiments of the present invention, the average particle size of the alumina-supported composite catalyst is 10-350 nm.

[0022] Furthermore, the average particle size of the alumina-supported composite catalyst is 80-250 nm.

[0023] According to the present invention, the alumina-supported composite catalyst is a spherical structure. The "spherical structure" in the present invention refers to a standard spherical structure or a structure close to a spherical structure, that is, including a substantially spherical structure.

[0024] In some preferred embodiments of the present invention, the active metal component is a combination of one or more selected from transition metals.

[0025] Furthermore, the active metal component is a combination of one or more selected from Group IB-IIB and Group VB-VIIIB.

[0026] Furthermore, the active metal component is a combination of one or more selected from Pd, Pt, Ru, Au, Ag, Rh, Ni, Cu, Fe and Co.

[0027] In some preferred embodiments of the present invention, the mass content of the active metal component in the alumina-supported composite catalyst is 0.01%-15% by mass percentage.

[0028] Furthermore, in terms of mass percentage, the mass content of the active metal component in the alumina-supported composite catalyst is 0.04%-15%.

[0029] In some preferred embodiments of the present invention, the proton-type heteropolyacid includes a combination of one or more selected from phosphomolybdic acid, phosphotungstic acid, silicotungstic acid, silicomolybdic acid, phosphovanadium heteropolyacid, phosphoniobial heteropolyacid, phosphotantalum heteropolyacid, ferromolybdic heteropolyacid, ferrotungsten heteropolyacid, ferrovanadium heteropolyacid, cobaltmolybdic heteropolyacid, cobalttungsten heteropolyacid, and cobaltvanadium heteropolyacid.

[0030] In some preferred embodiments of the present invention, the mass content of the proton-type heteropoly acid in the alumina-supported composite catalyst is 1%-68% by mass percentage.

[0031] Furthermore, in terms of mass percentage, the mass content of the proton-type heteropoly acid in the alumina-supported composite catalyst is 7%-45%.

[0032] Furthermore, in terms of mass percentage, the mass content of the proton-type heteropoly acid in the alumina-supported composite catalyst is 7%-25%.

[0033] According to the present invention, the specific surface area of ​​the alumina-supported composite catalyst can be made relatively larger. In some preferred embodiments of the present invention, the specific surface area of ​​the alumina-supported composite catalyst is greater than or equal to 200 m 2 / g.

[0034] Furthermore, the specific surface area of ​​the alumina-supported composite catalyst is greater than or equal to 300 m 2 / g.

[0035] In some embodiments, the specific surface area of ​​the alumina-supported composite catalyst is less than or equal to 1000 m 2 / g.

[0036] According to some preferred and specific aspects of the present invention, the specific surface area of ​​the alumina-supported composite catalyst is 200-800 m 2 / g.

[0037] In some preferred embodiments of the present invention, the alumina-supported composite catalyst is prepared by a preparation method that meets the following conditions:

[0038] (a) using an aluminum oxide precursor and an active metal precursor as raw materials, respectively, wherein the aluminum oxide precursor and the active metal precursor refer to substances that can be converted into aluminum oxide or active metal components through one or more conversion treatments, and the conversion treatment at least includes a treatment for producing a chemical reaction;

[0039] (b) carrying out the one or more conversion treatments in the presence of the protic heteropolyacid and water.

[0040] In the present invention, the presence of proton-type heteropolyacid can participate in the transformation process of alumina precursor. The two work together to promote the transformation and formation of a three-dimensional porous structure alumina carrier, and can also facilitate the dispersion of proton-type heteropolyacid in a single molecule state. At the same time, it can also promote a more stable connection between the proton-type heteropolyacid and the alumina carrier, for example, it is conducive to the formation of covalent bonds between the polyatoms in the proton-type heteropolyacid, the terminal oxygen in the proton-type heteropolyacid and the aluminum atoms in the alumina carrier. In addition, there may also be hydrogen bonding forces.

[0041] Furthermore, in the present invention, water is used for the first time to participate in the formation of the alumina carrier with a three-dimensional porous structure. In this process, in an organic solvent, in the presence of a proton-type heteropoly acid, the addition of water can induce the Kirkendall effect, thereby forming more mesoporous structures, and is also conducive to the formation of hollow structures and spherical morphologies. Specifically, Figure 1As shown, during the gelation process, the precursor of aluminum oxide (A: for example, Al(OR)3) will first form a spherical micelle structure, and then under the action of the Kirkendall effect induced by water (B: H2O), the surface of the sphere changes, and the surface is presented as a nano-sized sheet structure. A large number of mesoporous structures appear between the many sheet structures on the surface of the sphere, and the sheet structure itself can also appear porous. As the water-induced Kirkendall effect continues, the interior of the spherical structure gradually transforms into a hollow structure (AB: AlOOH). The existence of the hollow structure is conducive to promoting the dispersion of heteropolyacids in a true single-molecule state and further promoting the monodispersity of metal active components. On the other hand, this structure also gives the material a high specific surface area, low density, high loading capacity and hollow chamber, which is conducive to the catalytic reaction and mass transfer, thus becoming an ideal carrier.

[0042] According to some preferred aspects of the present invention, the aluminum oxide precursor is a compound containing aluminum and an organic group selected from acidic, basic or neutral compounds.

[0043] Furthermore, in some preferred embodiments of the present invention, the precursor of aluminum oxide is a substance that can be converted into aluminum oxide by sequentially performing gelation treatment and calcination treatment.

[0044] Furthermore, the precursor of aluminum oxide is a combination of one or more selected from aluminum alcohol compounds, hydrocarbon aluminum compounds, and organic aluminates.

[0045] According to some specific and preferred aspects of the present invention, the precursor of aluminum oxide is a combination of one or more selected from trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum chloride, aluminum isopropoxide, aluminum n-butoxide, aluminum acetate, and aluminum propionate.

[0046] In some preferred embodiments of the present invention, the active metal precursor is a salt of an active metal component and / or an acid of an active metal component; further, the salt of the active metal component includes a combination of one or more selected from metal nitrates, metal sulfates, metal halides, metal acetylacetonate complexes, and metal sulfides, and the acid of the active metal component includes a halogenated metal acid.

[0047] According to some specific and preferred aspects of the present invention, the active metal precursor is a combination of one or more selected from palladium chloride, palladium nitrate, platinum acetylacetonate, gold chloride, silver nitrate, ruthenium chloride, ruthenium nitrate, rhodium chloride, rhodium nitrate, cobalt nitrate, nickel nitrate, ferric chloride, ferric sulfate, copper nitrate, copper sulfate, chloroplatinic acid, chloropalladic acid, chloroauric acid, and rhodium acetylacetonate.

[0048] In some preferred embodiments of the present invention, the method for preparing the alumina-supported composite catalyst further satisfies the following conditions:

[0049] (c) The conversion treatment comprises a gelation treatment and a calcination treatment which are performed in sequence, and the gelation treatment is performed in the presence of water, an organic solvent and a surfactant.

[0050] Another technical solution provided by the present invention is a method for preparing the above-mentioned alumina-supported composite catalyst, the preparation method comprising:

[0051] Gelation treatment: mixing and reacting the proton type heteropoly acid with the precursor of aluminum oxide in the presence of water, an organic solvent and a surfactant, and inducing the solvent to evaporate to form a gel;

[0052] Calcination treatment: drying the gel and then calcining it, and performing a reduction treatment in the presence of a reducing agent to obtain the alumina-supported composite catalyst;

[0053] The preparation method further includes the step of adding an active metal precursor before the mixing reaction, or the step of coating with a solution containing the active metal precursor after the calcination treatment and before the reduction treatment, wherein the coating includes spraying, brushing, rolling, dipping or scraping.

[0054] Specifically, according to the timing of adding the active metal precursor, the preparation method of the present invention includes method (i) or method (ii):

[0055] Wherein, the method (i) comprises:

[0056] (i-1) gelation treatment: the proton type heteropoly acid, the active metal precursor and the aluminum oxide precursor are mixed and reacted in the presence of water, an organic solvent and a surfactant, and the solvent is evaporated to induce gelation;

[0057] (i-2) calcination treatment: drying the gel, calcining it, and performing a reduction treatment in the presence of a reducing agent to obtain the alumina-supported composite catalyst;

[0058] The method (ii) comprises:

[0059] (ii-1) gelation treatment: the proton type heteropoly acid and the precursor of aluminum oxide are mixed and reacted in the presence of water, an organic solvent and a surfactant, and the mixture is induced by solvent evaporation to form a gel;

[0060] (ii-2) Calcination treatment: the gel is dried and then calcined to obtain alumina-supported heteropolyacid, and then an active metal precursor is supported on the alumina-supported heteropolyacid, and a reduction treatment is performed in the presence of a reducing agent to obtain the alumina-supported composite catalyst.

[0061] According to some preferred aspects of the present invention, the mass ratio of the water to the aluminum oxide precursor is 0.001 to 15:1. Further, the mass ratio of the water to the aluminum oxide precursor is 0.01 to 10:1.

[0062] In some embodiments of the present invention, the feed mass ratio of the water to the aluminum oxide precursor is 0.01-6:1, for example, 0.01-3:1, or 0.02-3:1, or 0.04-1:1.

[0063] In some embodiments of the present invention, the feed mass ratio of the water to the aluminum oxide precursor is 0.1-5:1.

[0064] According to some preferred aspects of the present invention, the volume ratio of the water to the organic solvent is 0.001-5: 1. Further, the volume ratio of the water to the organic solvent is 0.001-2: 1. In some embodiments of the present invention, the volume ratio of the water to the organic solvent is 0.001-1: 1, for example, 0.001-0.5: 1, or 0.001-0.2: 1.

[0065] In some embodiments of the present invention, the volume ratio of the water to the organic solvent is 0.005-1:1.

[0066] In some preferred embodiments of the present invention, the organic solvent is a polar organic solvent.

[0067] In some preferred embodiments of the present invention, the feed mass ratio of the proton type heteropoly acid to the organic solvent is 1:80-1000.

[0068] In some preferred embodiments of the present invention, the organic solvent is a combination of one or more selected from methanol, ethanol, isopropanol, acetone, tetrahydrofuran, and N,N-dimethylformamide. In some embodiments of the present invention, the organic solvent does not contain water.

[0069] In some preferred embodiments of the present invention, the surfactant is a block copolymer nonionic surfactant and / or an ionic surfactant.

[0070] Furthermore, the block copolymer nonionic surfactant includes a combination of one or more selected from the group consisting of nonionic surfactant P123, nonionic surfactant F127, and nonionic surfactant F108.

[0071] Furthermore, the ionic surfactant includes a combination of one or more selected from cetyltrimethylammonium bromide (CTAB), sodium oleate, sodium dodecylbenzene sulfonate, and sodium stearate.

[0072] In some preferred embodiments of the present invention, the feed mass ratio of the surfactant to the proton-type heteropolyacid is 3-30:1.

[0073] Furthermore, the temperature of the mixed reaction is controlled to be 20-50° C. and the reaction time is controlled to be not less than 12 h.

[0074] In some preferred embodiments of the present invention, the temperature of the mixed reaction is controlled to be 20-40°C.

[0075] In some preferred embodiments of the present invention, the mixing reaction time is controlled to be 12 to 48 hours.

[0076] Furthermore, the time of the mixed reaction is controlled to be 12-15 h, 15-18 h, 18-21 h, 21-24 h, 24-27 h, 27-30 h or 30-48 h.

[0077] In some preferred embodiments of the present invention, the solvent evaporation induction is controlled to be carried out at a temperature of 40-120° C. and a time of 1-72 h.

[0078] In some preferred embodiments of the present invention, the solvent evaporation induction is controlled to be carried out at a temperature of 60-75° C. for a time of 10-60 h.

[0079] In some preferred embodiments of the present invention, the calcination is performed at 200-700°C.

[0080] In some preferred embodiments of the present invention, the calcination is performed in a muffle furnace.

[0081] In some preferred embodiments of the present invention, the calcination time is controlled to be 1-6 h.

[0082] In some preferred embodiments of the present invention, the heating rate of the calcination is controlled to be 1-30° C. / min.

[0083] In some preferred embodiments of the present invention, the calcination is performed in an aerobic environment, which includes an air atmosphere or a pure oxygen atmosphere, wherein the pure oxygen atmosphere is formed by introducing pure oxygen gas with a purity greater than 99%.

[0084] In some preferred embodiments of the present invention, when the preparation method adopts impregnation or spraying with a solution containing the active metal precursor after the calcination and before the reduction treatment, the active metal precursor and the solid obtained by the calcination are respectively dispersed in a solvent, mixed and stirred, and separated to obtain a solid loaded with the active metal precursor, and then the reduction treatment is carried out.

[0085] Furthermore, the solvent may be a ketone solvent, such as acetone.

[0086] Furthermore, when the preparation method adopts the method of impregnating or spraying a solution containing the active metal precursor after the calcination and before the reduction treatment, the active metal precursor is dispersed in a ketone solvent and stirred sufficiently, and then the solid obtained by the calcination is ultrasonically dispersed in the aforementioned solution, continuously stirred, and heated until the ketone solvent is completely evaporated to obtain a solid loaded with the active metal precursor.

[0087] In some preferred embodiments of the present invention, the reduction treatment comprises: performing a first calcination in an oxygen environment and then performing a second calcination in a reducing atmosphere.

[0088] Furthermore, the calcination temperature of the first calcination is 200-400°C.

[0089] Furthermore, the second calcination temperature is 150-300°C.

[0090] In some preferred embodiments of the present invention, the calcination temperature of the second calcination is lower than the calcination temperature of the first calcination.

[0091] In some preferred embodiments of the present invention, during the reduction treatment, the aerobic environment includes an air atmosphere or a pure oxygen atmosphere, wherein the pure oxygen atmosphere is formed by introducing pure oxygen gas having a purity greater than 99%, and the reducing atmosphere includes a hydrogen atmosphere.

[0092] According to some specific aspects of the present invention, when the preparation method adopts adding an active metal precursor before the mixing reaction, the implementation of the gelation treatment includes:

[0093] The proton type heteropoly acid, water and organic solvent are mixed and dispersed uniformly to obtain solution A; then a surfactant, an aluminum oxide precursor and an active metal precursor are added to solution A for mixing and dispersion, reacted at room temperature, and induced by solvent evaporation to prepare a gel.

[0094] Another technical solution provided by the present invention is an alumina-supported composite catalyst, which is prepared by the following method:

[0095] (1) reacting a proton-type heteropoly acid with an alcohol aluminum compound or a C1-C12 hydrocarbon aluminum compound in the presence of water, a C2-C4 alcohol solvent and a surfactant at 20-50°C for 12-48 hours, and inducing solvent evaporation at a temperature of 60-75°C for 10-72 hours to prepare a gel:

[0096] The proton type heteropoly acid is a combination of one or more selected from phosphomolybdic acid, phosphotungstic acid, silicotungstic acid, and silicomolybdic acid;

[0097] (2) drying the gel to obtain a solid, and then calcining the solid at 300-450° C. in an air atmosphere to obtain an alumina-supported heteropoly acid;

[0098] (3) The salt of the active metal component is supported on the alumina-supported heteropoly acid, and then the alumina-supported composite catalyst is obtained by first calcining the alumina-supported composite catalyst at 200-400°C in an air atmosphere and then second calcining the alumina-supported composite catalyst at 150-300°C in a hydrogen atmosphere.

[0099] Furthermore, the C2-C4 alcohol solvent is ethanol, isopropanol, etc.

[0100] Furthermore, the aluminum alcohol compound is aluminum isopropoxide, aluminum n-butoxide, etc.

[0101] Furthermore, the C1-C12 hydrocarbon aluminum compound includes triethylaluminum, triisobutylaluminum, and the like.

[0102] Another technical solution provided by the present invention is: a catalyst composition, comprising the alumina-loaded composite catalyst as described above and at least one other catalyst different from the alumina-loaded composite catalyst; wherein, in terms of mass percentage, the mass content of the alumina-loaded composite catalyst in the catalyst composition exceeds 50%.

[0103] In some embodiments of the present invention, in the catalyst composition, the mass content of the alumina-supported composite catalyst exceeds 55%, or exceeds 60%, or exceeds 65%, or exceeds 70%, or exceeds 75%, or exceeds 80%, or exceeds 85%, or exceeds 90%, or exceeds 95%, or exceeds 96%, or exceeds 97%, or exceeds 98%, or exceeds 99%.

[0104] Another technical solution provided by the present invention is: an application of the above-mentioned alumina-supported composite catalyst, or the alumina-supported composite catalyst prepared by the above-mentioned method for preparing the alumina-supported composite catalyst, in the following reactions: oxidation reaction of aromatic hydrocarbons, alcohols or aldehydes, esterification reaction of olefins with acids or esterification reaction of alcohols with acids, epoxidation reaction of olefins, alkylation reaction of aromatic compounds, isomerization reaction, dehydration reaction of alcohols, etherification reaction, hydration reaction of olefins, hydrogenation reaction, amination reaction of alcohols, ketones or olefins.

[0105] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating o-tert-butylphenol in the presence of an alumina-supported composite catalyst to produce o-tert-butyl cyclohexanol; further, the reaction is carried out at a pressure of 1-3 MPa and a reaction temperature of 60-90°C.

[0106] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating cyclopentylbutyrolactone in an alcohol-containing system in the presence of the alumina-supported composite catalyst to prepare cyclohexylpropionate. Further, the alcohol in the alcohol-containing system is selected from C 1-20 The hydrocarbon alcohol may be, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, allyl alcohol, etc. The reaction is carried out at 1-4 MPa and 100-150°C.

[0107] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating rose oxide in the presence of an alumina-supported composite catalyst to prepare phenylpentanol; further, the amount of the alumina-supported composite catalyst added is 0.01wt.%-1.0wt.% of the amount of rose oxide added; and the reaction is carried out at 80-150°C and 1-3 MPa.

[0108] In some embodiments of the present invention, the isomerization reaction comprises: hydroisomerizing 2-pentylcyclopentanone in the presence of an alumina-supported composite catalyst to prepare 2-pentylcyclopentenone; further, the reaction is carried out at 20-60°C, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-1.0wt.% of the amount of 2-pentylcyclopentanone added.

[0109] In some embodiments of the present invention, the amination reaction comprises: 2-6 Preparation of C by Hydroamination of Alkyl Alcohols with Ammonia in the Presence of Alumina-Supported Composite Catalyst 2-6 Alkylamine; further, the reaction is carried out at 100-150 ° C and a pressure of 0.1-0.6 MPa; C 2-6 The alkyl alcohol may be ethanol, propanol, etc.

[0110] In some embodiments of the present invention, the amination reaction comprises: 3-6 Preparation of C by Hydroamination of Alkyl Ketones with Ammonia in the Presence of Alumina-Supported Composite Catalyst 3-6 Alkylamine; further, the reaction is carried out at 100-150 ° C and a pressure of 0.1-0.6 MPa; C 3-6 The alkyl ketone may be acetone, butanone or the like.

[0111] In some embodiments of the present invention, the amination reaction comprises: 2-10 Preparation of C from olefins and ammonia in the presence of alumina-supported composite catalyst 2-10further, reacting at 120-180 ° C and 2-6 MPa; C 2-10 The olefin may be isobutylene, ethylene, propylene, etc.

[0112] In some embodiments of the present invention, the oxidation reaction comprises: 1-6 Preparation of phenyl C by reaction of alkyl alcohol with hydrogen peroxide in the presence of alumina supported composite catalyst 1-6 Alkyl aldehyde; further, the reaction is carried out at 40-70 ° C; the amount of the alumina-supported composite catalyst added is phenyl C 1-6 The addition amount of alkyl alcohol is 0.01wt.%-3.0wt.%; phenyl C 1-6 The alkyl alcohol may be benzyl alcohol, phenylethyl alcohol or the like.

[0113] In some embodiments of the present invention, the oxidation reaction comprises: subjecting C3-C10 aldehyde, C3-C10 alcohol or aromatic hydrocarbon to oxidation reaction in the presence of an oxidant and an alumina-supported composite catalyst to prepare C3-C10 acid; further, the oxidant may be oxygen or air, etc., and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of the C3-C10 aldehyde added. Furthermore, when the C3-C10 aldehyde is used as a substrate, the reaction is carried out at 30-55°C; when the C3-C10 alcohol is used as a substrate, the reaction is carried out at 70-100°C; when the aromatic hydrocarbon is used as a substrate, the reaction is carried out at 120-160°C.

[0114] In some embodiments of the present invention, the epoxidation reaction comprises: reacting α-pinene with hydrogen peroxide to prepare epoxypinene, and the reaction is carried out at 50-80°C; or reacting limonene with hydrogen peroxide to prepare epoxylimonene, and the reaction is carried out at 50-80°C.

[0115] In some embodiments of the present invention, the esterification reaction comprises: an acid and an alcohol undergo an esterification reaction in the presence of an alumina-supported composite catalyst to prepare an ester;

[0116] Furthermore, the acid may be 2-methylbutyric acid, and the alcohol may be methanol, ethanol, isopropanol, n-butanol, n-hexanol, n-pentanol, or n-hexanol. The reaction is carried out at 40-80° C., and the amount of the alumina-supported composite catalyst added is 0.01 wt.%-2.0 wt.% of the amount of the acid added.

[0117] Furthermore, the acid can be salicylic acid, and the alcohol can be n-pentanol, n-hexanol, benzyl alcohol, leaf alcohol, cyclohexanol, isooctyl alcohol, isophorol, and the reaction is carried out at 60-100°C and 300-700 mmHg, and the addition amount of the alumina-supported composite catalyst is 0.01wt.%-2.0wt.% of the addition amount of the acid.

[0118] Furthermore, the acid can be acetic acid, hexanoic acid, heptanoic acid, phenylpropionic acid, phenoxyacetic acid, cyclohexyloxyacetic acid, and the alcohol can be allyl alcohol. The reaction is carried out at 60-100°C, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of the alcohol added.

[0119] Further, the acid may be acetic acid, the alcohol may be o-tert-butyl cyclohexanol, p-tert-butyl cyclohexanol, α-phenylethanol, β-phenylethanol, the reaction is carried out at 60-100 ° C, 300-700 mmHg, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of the alcohol added. In some embodiments of the present invention, the esterification reaction comprises: an acid and an olefin undergo an esterification reaction in the presence of an alumina-supported composite catalyst to prepare an ester; further, the olefin may be dicyclopentadiene, etc., the acid may be acetic acid, propionic acid, n-butyric acid, isobutyric acid, etc., the reaction is carried out at 60-100 ° C, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of the olefin added.

[0120] In some embodiments of the present invention, the alkylation reaction comprises: continuously alkylating propylene and m-cresol in the presence of an alumina-supported composite catalyst to prepare thymol; further, the reaction is carried out at 200-240° C. and 0.05-0.5 MPa.

[0121] In some embodiments of the present invention, the isomerization reaction comprises: isomerizing o-cresol to prepare m-cresol and p-cresol in the presence of an alumina-supported composite catalyst; further, the reaction is carried out at 240-300° C. and 0.05-0.4 MPa.

[0122] In some embodiments of the present invention, the dehydration reaction comprises: dehydrating 2-(1-hydroxypentyl)-cyclopentanone to prepare 2-pentylidenecyclopentanone in the presence of an alumina-supported composite catalyst; carrying out the reaction at 70-100°C and 100-500 mmHg, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of 2-(1-hydroxypentyl)-cyclopentanone added.

[0123] In some embodiments of the present invention, the dehydration reaction comprises: dehydrating hydroxycyclopentadecalactone to prepare harbanolide in the presence of an alumina-supported composite catalyst; further, the reaction is carried out at 80-110°C and 150-500 mmHg, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of the hydroxycyclopentadecalactone added.

[0124] In some embodiments of the present invention, the etherification reaction comprises: in the presence of an alumina-supported composite catalyst, self-etherifying 2-(3-hydroxypropyl)cyclododecanone to prepare trideca-oxabicyclo[10.4.0]hexadecene; further, the reaction is carried out at 80-100°C and 150-500 mmHg, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-2.0wt.% of the amount of 2-(3-hydroxypropyl)cyclododecanone added.

[0125] In some embodiments of the present invention, the hydration reaction comprises: hydrating propylene to prepare isopropanol in the presence of an alumina-supported composite catalyst; further, the reaction is carried out at 100-160° C. and 1-8 MPa.

[0126] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating halbalactone to prepare cyclopentadecalactone in the presence of an alumina-supported composite catalyst; further, the reaction is carried out at 30-50°C, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-1.0wt.% of the amount of halbalactone added.

[0127] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating p-tert-butylphenol to prepare p-tert-butyl cyclohexanol in the presence of an alumina-supported composite catalyst; further, the reaction is carried out at a pressure of 1-5 MPa and a temperature of 60-90°C.

[0128] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0129] Based on in-depth research, the present invention proposes a formation mechanism and a new catalyst structure that are different from the existing alumina-supported heteropolyacids. On the one hand, the three-dimensional hollow porous structure of the catalyst is significantly different from the existing nanosheet structure or solid sphere. On the other hand, based on the new structure, the present invention proposes and realizes the composite of the monodispersed heteropolyacid and the single atomic distribution of the metal active component, achieving a significant synergistic effect. The catalyst of the present invention has been proven to have higher catalytic activity and stability in multiple reaction systems. The preparation method of the present invention is simple to operate and has low raw material cost. In addition, it has good controllability and strong versatility. It can stably form a three-dimensional hollow porous structure and various parameters of the catalyst, such as the size of the hollow part, the size of the pores, and the content of the catalytic active component, can be adjusted within a wide range. BRIEF DESCRIPTION OF THE DRAWINGS

[0130] Figure 1 A schematic diagram showing the formation mechanism of the three-dimensional hollow porous structure of the catalyst of the present invention;

[0131] Figure 2 XRD spectrum of the catalyst Pd-H3PMo / AS-20H prepared in Example 1;

[0132] Figure 3 This is a scanning electron microscope image of the catalyst Pd-H3PMo / AS-20H prepared in Example 1;

[0133] Figure 4 The transmission electron microscope image of the catalyst Pd-H3PMo / AS-20H prepared in Example 1;

[0134] Figure 5 The spherical aberration electron microscope image of the catalyst Pd-H3PMo / AS-20H prepared in Example 1;

[0135] Figure 6 The particle size distribution histogram of the heteropoly acid corresponding to the catalyst Pd-H3PMo / AS-20H prepared in Example 1;

[0136] Figure 7 Figure 1 shows the nitrogen absorption and desorption of the catalyst Pd-H3PMo / AS-20H prepared in Example 1;

[0137] Figure 8 XRD spectrum of the catalyst Pd-H3PW / AS-20H prepared in Example 2;

[0138] Fig. 9 This is a scanning electron microscope image of the catalyst Pd-H3PW / AS-20H prepared in Example 2;

[0139] Fig.10 The transmission electron microscope image of the catalyst Pd-H3PW / AS-20H prepared in Example 2;

[0140] Fig.11 This is a spherical aberration electron microscope image of the catalyst Pd-H3PW / AS-20H prepared in Example 2;

[0141] Fig.12 The particle size distribution histogram of the heteropoly acid corresponding to the catalyst Pd-H3PW / AS-20H prepared in Example 2;

[0142] Fig.13 Figure 2 shows the nitrogen absorption and desorption of the catalyst Pd-H3PW / AS-20H prepared in Example 2;

[0143] Fig.14 The XRD spectrum of the catalyst Pd-H4SiW / AS-20H prepared in Example 3;

[0144] Fig.15 This is a scanning electron microscope image of the catalyst Pd-H4SiW / AS-20H prepared in Example 3;

[0145] Fig.16 This is a transmission electron microscopy image of the catalyst Pd-H4SiW / AS-20H prepared in Example 3;

[0146] Fig.17 This is a nitrogen absorption and desorption diagram of the catalyst Pd-H4SiW / AS-20H prepared in Example 3;

[0147] Fig.18 XRD spectrum of the catalyst Pd-H4SiMo / AS-20H prepared in Example 4;

[0148] Fig.19 This is a scanning electron microscope image of the catalyst Pd-H4SiMo / AS-20H prepared in Example 4;

[0149] Fig. 20 The transmission electron microscope image of the catalyst Pd-H4SiMo / AS-20H prepared in Example 4;

[0150] Fig.21 Figure 1 is a nitrogen absorption and desorption diagram of the catalyst Pd-H4SiMo / AS-20H prepared in Example 4;

[0151] Fig. 22 The transmission electron microscope image of the catalyst Pd-H3PMo / AS-14H prepared in Example 5;

[0152] Fig.23 A transmission electron microscopy image of the catalyst Pd-H3PMo / AS-8H prepared in Example 6;

[0153] Fig.24The transmission electron microscope image of the catalyst Pd-H3PMo / AS-2H prepared in Example 7;

[0154] Fig.25 It is a transmission electron microscope image of the catalyst Pd-H3PMo / AS-30H prepared in Example 8;

[0155] Fig.26 This is a transmission electron microscopy image of the catalyst Pd-H3PMo / AS-50H prepared in Example 9;

[0156] Fig. 27 TEM image of the catalyst Pd-H3PMo / AS-100H prepared in Example 10;

[0157] Fig.28 XRD spectrum of the catalyst Pt-H3PMo / AS-20H prepared in Example 11;

[0158] Fig.29 A transmission electron microscopy image of the catalyst Pt-H3PMo / AS-20H prepared in Example 11;

[0159] Fig.30 XRD spectrum of the catalyst Co-H3PMo / AS-20H prepared in Example 12;

[0160] Fig.31 XRD spectrum of the catalyst Ni-H3PMo / AS-20H prepared in Example 13;

[0161] Fig.32 This is a transmission electron microscopy image of the catalyst Pd-H3PMo / AS-20H-85 prepared in Example 14;

[0162] Fig.33 A transmission electron microscopy image of the catalyst Pd-H3PMo / AS-F-20H prepared in Example 17;

[0163] Fig.34 TEM image of the catalyst Pd-H3PMo / AS-C-20H prepared in Example 18;

[0164] Fig.35 This is a transmission electron microscope image of the catalyst Pd-7%H3PMo / AS-20H prepared in Example 19;

[0165] Fig.36 XRD spectrum of the catalyst Pd@H3PMo / AS-20H prepared in Example 20;

[0166] Fig.37 This is a transmission electron microscopy image of the catalyst Pd@H3PMo / AS-20H prepared in Example 20;

[0167] Fig.38 XRD spectrum of the catalyst H3PMo@AS prepared in Comparative Example 1;

[0168] Fig.39 It is a transmission electron microscope image of the catalyst Pd-H3PMo / AS prepared in Comparative Example 1;

[0169] Fig.40 XRD spectrum of the catalyst Pd-APMo / AS-20H prepared in Comparative Example 2;

[0170] Fig.41 It is a transmission electron microscope image of the catalyst Pd-APMo / AS-20H prepared in Comparative Example 2;

[0171] Fig.42 This is a transmission electron microscopy image of the catalyst Pd-H3PMo / Al2O3-ethanol prepared in Comparative Example 3. DETAILED DESCRIPTION

[0172] In view of the problems of insufficient exposure of active sites and loss of heteropolyacid in alumina-supported heteropolyacid catalysts in the prior art, and insufficient synergistic effect of heteropolyacid-metal composite catalysts, the present invention proposes and realizes a new catalyst structure. Specifically, in some specific embodiments, the alumina-supported composite catalyst provided by the present invention includes an alumina carrier having a three-dimensional hollow porous structure, a proton-type heteropolyacid dispersed in a single molecule state and connected to the alumina carrier, and an active metal component dispersed in a single atom state and connected to the heteropolyacid. By introducing a proton-type heteropoly acid that can be dispersed in a single molecule state and connected to the alumina carrier with a three-dimensional hollow porous structure and an active metal component that can be dispersed in a single atom state and connected to the proton-type heteropoly acid and / or the alumina carrier with a three-dimensional hollow porous structure, respectively, on the basis of an alumina carrier with a three-dimensional porous structure, a catalyst form of double monodispersed three-dimensional hollow porous alumina is formed. The proton-type heteropoly acid is uniformly distributed in a single molecule state, so that the active sites of the proton-type heteropoly acid are fully exposed. At the same time, the single molecule state promotes the active metal component to be dispersed in a single atom form and always maintain a uniform dispersion state. In particular, the presence of the alumina carrier allows the alumina and proton-type heteropoly acid, the proton-type heteropoly acid and the active metal component to form a stable strong interaction and improve the microstructure, thereby constructing a stable loading state. At the same time, a catalyst with a three-dimensional hollow porous structure can be formed, which significantly improves the catalytic performance. Practice has shown that the alumina-loaded composite catalyst of the present invention not only obtains unexpectedly excellent stability, catalytic activity and selectivity in the catalytic process, has a long service life and a good catalytic effect, but can also significantly improve the conditions of certain catalytic reactions, making the reaction milder; in addition, the catalyst cost is relatively low, and the preparation method is simple and controllable. In particular, the hollow degree of the alumina-loaded composite catalyst of the present invention is adjustable and the hollow size is controllable.

[0173] The above scheme is further described below in conjunction with specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.

[0174] The raw materials used in the following examples, unless otherwise specified, were purchased from commercial sources or prepared by conventional methods in the art, wherein the surfactants: P123 was purchased from Sigma-Aldrich; F127 was purchased from Sigma-Aldrich.

[0175] Embodiment 1:

[0176] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0177] Weigh 2.9 g of phosphomolybdic acid (H3PMo for short), mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-20H.

[0178] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0179] Figure 2 This is the XRD diagram of Pd-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the catalyst.

[0180] Figure 3 This is the SEM image (scanning electron microscope image) of Pd-H3PMo / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets.

[0181] Figure 4 This is the TEM image (transmission electron microscope image) of Pd-H3PMo / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets with a diameter of about 181 nm. The diameter of the hollow part is about 80 nm, and no palladium particles are observed, indicating that the palladium is highly dispersed.

[0182] Figure 5 This is the STEM-HAADF image of Pd-H3PMo / AS-20H (spherical aberration electron microscope image). Figure 6The corresponding particle size distribution histogram shows that single clusters of phosphomolybdic acid with a size of about 0.71 nm are distributed on the catalyst, indicating that phosphomolybdic acid is dispersed in a single molecule on the catalyst Pd-H3PMo / AS-20H.

[0183] Figure 7 This is the nitrogen adsorption and desorption diagram of Pd-H3PMo / AS-20H. It is observed that the nitrogen adsorption and desorption diagram of the catalyst shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0184] The alumina-supported composite catalyst is spherical with a diameter of about 181 nm and a specific surface area of ​​about 697 m 2 / g, the average pore size is about 6.6 nm, the average pore volume is about 1.3 cc / g, and the average density is about 2.6 g / cm 3 .

[0185] Embodiment 2:

[0186] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0187] Weigh 2.9 g of phosphotungstic acid (H3PW for short), mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Pd-H3PW / AS-20H.

[0188] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphotungstic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0189] Figure 8This is the XRD diagram of Pd-H3PW / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the catalyst.

[0190] Fig. 9 This is the SEM image (scanning electron microscope image) of Pd-H3PW / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets.

[0191] Fig.10 This is the TEM image (transmission electron microscope image) of Pd-H3PW / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0192] Fig.11 This is the STEM-HAADF image of Pd-H3PW / AS-20H (spherical aberration electron microscope image). Fig.12 The corresponding particle size distribution histogram shows that single clusters of phosphomolybdic acid with a size of about 0.71 nm are distributed on the catalyst, indicating that phosphomolybdic acid is dispersed in a single molecule on the catalyst Pd-H3PW / AS-20H.

[0193] Fig.13 This is the nitrogen adsorption / desorption diagram of Pd-H3PW / AS-20H. It is observed that the nitrogen adsorption / desorption diagram of the catalyst shows a typical type IV adsorption / desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0194] The alumina-supported composite catalyst is spherical with a diameter of about 178 nm and a specific surface area of ​​about 650 m 2 / g, the average pore size is about 5.9 nm, the average pore volume is about 1.1 cc / g, and the average density is about 2.8 g / cm 3 .

[0195] Embodiment 3:

[0196] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0197] Weigh 2.9 g of silicotungstic acid (abbreviated as H4SiW), mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H4SiW / AS-20H.

[0198] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of silicotungstic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0199] Fig.14 This is the XRD diagram of Pd-H4SiW / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the catalyst.

[0200] Fig.15 This is the SEM image (scanning electron microscope image) of Pd-H4SiW / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets.

[0201] Fig.16 This is the TEM image (transmission electron microscope image) of Pd-H4SiW / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0202] Fig.17 This is the nitrogen adsorption and desorption diagram of Pd-H4SiW / AS-20H. It is observed that the nitrogen adsorption and desorption diagram of the catalyst shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0203] The alumina-supported composite catalyst is spherical with a diameter of about 175 nm and a specific surface area of ​​about 647 m 2 / g, the average pore size is about 5.8 nm, the average pore volume is about 0.9 cc / g, and the average density is about 3.0 g / cm 3 .

[0204] Embodiment 4:

[0205] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0206] Weigh 2.9 g of silicomolybdic acid (H4SiMo for short), mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H4SiMo / AS-20H.

[0207] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of silicomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.5%.

[0208] Fig.18 This is the XRD diagram of Pd-H4SiMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the catalyst.

[0209] Fig.19 This is the SEM image (scanning electron microscope image) of Pd-H4SiMo / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets.

[0210] Fig. 20 This is the TEM image (transmission electron microscope image) of Pd-H4SiMo / AS-20H. It was observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0211] Fig.21 This is the nitrogen adsorption and desorption diagram of Pd-H4SiMo / AS-20H. It is observed that the nitrogen adsorption and desorption diagram of the catalyst shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0212] The alumina-supported composite catalyst is spherical with a diameter of about 177 nm and a specific surface area of ​​about 682 m 2 / g, the average pore size is about 6.4 nm, the average pore volume is about 1.2 cc / g, and the average density is about 2.8 g / cm 3 .

[0213] Embodiment 5:

[0214] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0215] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 14 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250°C for 2h, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-14H.

[0216] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.7%.

[0217] Fig. 22 This is the TEM image (transmission electron microscope image) of Pd-H3PMo / AS-14H. It is observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets. When the amount of water added is reduced, the hollowness of the catalyst decreases. No palladium particles are observed, indicating that the palladium is highly dispersed.

[0218] The alumina-supported composite catalyst is spherical with a diameter of about 157 nm and a specific surface area of ​​about 619 m 2 / g, the average pore size is about 6.3 nm, the average pore volume is about 1.0 cc / g, and the average density is about 3.1 g / cm 3 .

[0219] Embodiment 6:

[0220] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0221] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 8 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250°C for 2h, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-8H.

[0222] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0223] Fig.23 The TEM image (transmission electron microscope image) of Pd-H3PMo / AS-8H shows that as the amount of water added further decreases, the hollow structure becomes less obvious. No palladium particles are observed, indicating that palladium is highly dispersed.

[0224] The alumina-supported composite catalyst is spherical with a diameter of about 152 nm and a specific surface area of ​​about 384 m 2 / g, the average pore size is about 6.6 nm, the average pore volume is about 0.7 cc / g, and the average density is about 3.3 g / cm 3 .

[0225] Embodiment 7:

[0226] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0227] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 2 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250 °C for 2 h, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-2H.

[0228] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0229] Fig.24 The TEM image (transmission electron microscope image) of Pd-H3PMo / AS-2H shows that when the amount of water added is reduced to 2 mL, the hollow structure is very small and difficult to observe clearly. No palladium particles are observed, indicating that palladium is highly dispersed.

[0230] The alumina-supported composite catalyst is spherical with a diameter of about 141 nm and a specific surface area of ​​about 573 m 2 / g, the average pore size is about 5.5 nm, the average pore volume is about 0.8 cc / g, and the average density is about 2.9 g / cm 3 .

[0231] Embodiment 8:

[0232] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0233] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 30 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250°C for 2h, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-30H.

[0234] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0235] Fig.25 This is the TEM image (transmission electron microscope image) of Pd-H3PMo / AS-30H. It was observed that no palladium particles were observed, indicating that palladium was highly dispersed.

[0236] The specific surface area of ​​the alumina-supported composite catalyst is approximately 480 m 2 / g, the average pore size is about 9.2 nm, the average pore volume is about 1.1 cc / g, and the average density is about 3.1 g / cm 3 .

[0237] Embodiment 9:

[0238] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0239] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 50 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250°C for 2h, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-50H.

[0240] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.5%.

[0241] Fig.26 This is the TEM image (transmission electron microscope image) of Pd-H3PMo / AS-50H. It was observed that no palladium particles were observed, indicating that the palladium was highly dispersed.

[0242] The specific surface area of ​​the alumina-supported composite catalyst is approximately 402 m 2 / g, the average pore size is about 8.6 nm, the average pore volume is about 1.0 cc / g, and the average density is about 3.3 g / cm 3 .

[0243] Embodiment 10:

[0244] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0245] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 100 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-100H.

[0246] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0247] Fig. 27 This is the TEM image (transmission electron microscope image) of Pd-H3PMo / AS-100H. It was observed that no palladium particles were observed, indicating that the palladium was highly dispersed.

[0248] The specific surface area of ​​the alumina-supported composite catalyst is approximately 441 m 2 / g, the average pore size is about 11.7 nm, the average pore volume is about 1.29 cc / g, and the average density is about 3.2 g / cm 3 .

[0249] Embodiment 11:

[0250] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0251] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of acetylacetonate platinum solution (100 mg of acetylacetonate platinum dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 200 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pt-H3PMo / AS-20H.

[0252] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of platinum was 0.6%.

[0253] Fig.28 This is the XRD diagram of Pt-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or platinum, indicating that the heteropoly acid and platinum were uniformly dispersed on the catalyst.

[0254] Fig.29 This is a TEM image (transmission electron microscope image) of Pt-H3PMo / AS-20H. It is observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets. No palladium particles are observed, indicating that platinum is highly dispersed.

[0255] The alumina-supported composite catalyst is spherical with a diameter of about 180 nm and a specific surface area of ​​about 690 m 2 / g, the average pore size is about 6.7 nm, the average pore volume is about 1.3 cc / g, and the average density is about 2.7 g / cm 3 .

[0256] Embodiment 12:

[0257] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0258] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of cobalt nitrate solution (100 mg of cobalt nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250 °C for 2 h, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Co-H3PMo / AS-20H.

[0259] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of cobalt was 0.7%.

[0260] Fig.30 This is the XRD diagram of Co-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or cobalt, indicating that the heteropoly acid and cobalt were uniformly dispersed on the catalyst.

[0261] Embodiment 13:

[0262] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0263] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, obtain gel after 48 h, and then put it in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of nickel nitrate solution (100 mg of nickel nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250°C for 2h, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Ni-H3PMo / AS-20H.

[0264] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of nickel was 0.5%.

[0265] Fig.31 This is the XRD diagram of Ni-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or nickel, indicating that the heteropoly acid and nickel were uniformly dispersed on the catalyst.

[0266] Embodiment 14:

[0267] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0268] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous isopropanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 85 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-20H-85.

[0269] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0270] Fig.32 This is a TEM image (transmission electron microscope image) of Pd-H3PMo / AS-20H-85. It is found that the catalyst is roughly a hollow porous spherical structure. No palladium particles are observed, indicating that the palladium is highly dispersed.

[0271] Embodiment 15:

[0272] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0273] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of triisobutylaluminum in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and the alumina-supported composite catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-20H-T.

[0274] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0275] Embodiment 16:

[0276] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0277] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum acetate in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250 °C for 2 h, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-20H-E.

[0278] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.7%.

[0279] Embodiment 17:

[0280] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0281] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of F127 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 72 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250°C for 2h, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-F-20H.

[0282] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0283] Fig.33 This is a TEM image (transmission electron microscope image) of Pd-H3PMo / AS-F-20H. It is observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets. No palladium particles are observed, indicating that palladium is highly dispersed.

[0284] The alumina-supported composite catalyst is spherical with a diameter of about 174 nm and a specific surface area of ​​about 630 m 2 / g, the average pore size is about 7.1 nm, the average pore volume is about 1.2 cc / g, and the average density is about 3.1 g / cm 3 .

[0285] Embodiment 18:

[0286] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0287] Weigh 2.9 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of hexadecyltrimethylammonium bromide (CTAB) and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 10 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300 °C for 2 h at a heating rate of 5 °C / min in an air atmosphere. Next, the obtained sample was reduced at 250 °C for 2 h in a pure H2 atmosphere in a muffle furnace, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS-C-20H.

[0288] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.5%.

[0289] Fig.34 This is a TEM image (transmission electron microscope image) of Pd-H3PMo / AS-C-20H. It is observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets. No palladium particles are observed, indicating that palladium is highly dispersed.

[0290] The alumina-supported composite catalyst is spherical with a diameter of about 173 nm and a specific surface area of ​​about 641 m 2 / g, the average pore size is about 6.9 nm, the average pore volume is about 1.2 cc / g, and the average density is about 3.2 g / cm 3 .

[0291] Embodiment 19:

[0292] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0293] Weigh 0.8 g of phosphomolybdic acid, mix with 500 mL of anhydrous ethanol and 20 mL of deionized water, stir thoroughly, and after uniform dispersion, add 20 g of P123 and 50 g of aluminum isopropoxide in turn, react fully at room temperature for 24 h, then induce solvent evaporation at 70 °C, and obtain a gel after 48 h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350 °C for 3 h in an air atmosphere at a heating rate of 5 °C / min to obtain alumina-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of alumina-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 °C until the acetone is completely evaporated. The obtained solid is then placed in a muffle furnace and calcined at 300 °C for 2 h in an air atmosphere at a heating rate of 5 °C / min. Next, the obtained sample was reduced in a muffle furnace in a pure H2 atmosphere at 250 °C for 2 h, and after natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-7%H3PMo / AS-20H.

[0294] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 7%, and the actual loading amount of palladium was 0.4%.

[0295] Fig.35 This is a TEM image (transmission electron microscope image) of Pd-7%H3PMo / AS-20H. It is found that the catalyst has a three-dimensional hollow porous structure. No palladium particles are observed, indicating that palladium is highly dispersed.

[0296] The alumina-supported composite catalyst is spherical with a diameter of about 152 nm and a specific surface area of ​​about 589 m 2 / g, the average pore size is about 7.0 nm, the average pore volume is about 1.2 cc / g, and the average density is about 3.5 g / cm 3 .

[0297] Embodiment 20:

[0298] This example provides a method for preparing an alumina-supported composite catalyst and the alumina-supported composite catalyst prepared therefrom, the preparation method comprising:

[0299] Weigh 2.9g of phosphomolybdic acid, mix with 500mL of anhydrous ethanol and 20mL of deionized water, stir thoroughly, and after uniform dispersion, add 20g of P123, 31.2mg of palladium nitrate and 50g of aluminum isopropoxide in sequence, fully react at room temperature for 24h, then induce solvent evaporation at 70℃, and obtain gel after 48h, which is then placed in an oven to dry overnight. The solid obtained after drying is placed in a muffle furnace and calcined at 350℃ for 3h in an air atmosphere with a heating rate of 5℃ / min to obtain alumina-supported heteropoly acid. Next, the obtained sample is reduced at 250℃ in a pure H2 atmosphere in a muffle furnace for 2h, and the alumina-supported composite catalyst is obtained after natural cooling, which is recorded as Pd@H3PMo / AS-20H.

[0300] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.7%.

[0301] Fig.36 This is the XRD diagram of Pd@H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the catalyst.

[0302] Fig.37 This is a TEM image (transmission electron microscope image) of Pd@H3PMo / AS-20H. It is observed that the catalyst is a three-dimensional hollow porous structure assembled from two-dimensional sheets. No palladium particles are observed, indicating that palladium is highly dispersed.

[0303] The alumina-supported composite catalyst is spherical with a diameter of about 166 nm and a specific surface area of ​​about 625 m 2 / g, the average pore size is about 6.7 nm, the average pore volume is about 1.1 cc / g, and the average density is about 3.1 g / cm 3 .

[0304] Comparative Example 1:

[0305] This example provides an alumina-supported composite catalyst, the preparation process of which is as follows: 20g of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) is placed in 400mL of anhydrous ethanol, and 2.2g of phosphomolybdic acid is dispersed in 80mL of anhydrous ethanol, and then uniformly added dropwise to the ethanol solution of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, stirred and mixed, to obtain a first configuration. 40.8g of aluminum isopropoxide is placed in the first configuration, stirred for 6h, to obtain a second configuration.

[0306] The second configuration was placed in an oven at 60 ° C for aging for 48 hours to obtain a solid mixture, which was calcined in an air furnace at a calcination temperature of 350 ° C, a heating rate of 1 ° C / min, and a calcination time of 4 hours to obtain the catalyst H3PMo@AS. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) was added to 150 mL of acetone and stirred thoroughly. Then, 3 g of the catalyst H3PMo@AS was ultrasonically dispersed in the above solution. After continuous stirring for 6 hours, the mixture was heated to 40 ° C until the acetone was completely evaporated. Then the obtained solid was placed in a muffle furnace and calcined at 300 ° C for 2 hours at a heating rate of 5 ° C / min in an air atmosphere. Next, the obtained sample was reduced at 250 ° C for 2 hours in a pure H2 atmosphere in a muffle furnace. After natural cooling, an alumina-supported composite catalyst was obtained, which was recorded as Pd-H3PMo / AS.

[0307] Fig.38 This is the XRD spectrum of H3PMo@AS prepared in this example. It can be seen from the figure that the diffraction peak of heteropoly acid appears, indicating that the heteropoly acid is not dispersed on the catalyst in a single molecule state.

[0308] Fig.39 This is the TEM image (transmission electron microscope image) of Pd-H3PMo / AS. It was observed that the catalyst has a three-dimensional solid structure.

[0309] Comparative Example 2:

[0310] This example provides an alumina-supported composite catalyst, which is prepared in the same manner as in Example 1, except that phosphomolybdic acid is replaced with an equal mass of aprotic heteropolyacid-ammonium phosphomolybdate (APMo for short). The resulting catalyst is recorded as Pd-APMo / AS-20H.

[0311] The structure of the alumina-supported composite catalyst was characterized. The actual loading amount of ammonium phosphomolybdate in the catalyst was 21%, and the actual loading amount of palladium was 0.3%.

[0312] Fig.40 The XRD pattern of Pd-APMo / AS-20H shows that the characteristic diffraction peak of ammonium phosphomolybdate appears in the XRD spectrum of the sample, indicating that the salt form of the heteropoly acid cannot be monodispersed on the porous alumina support. Analysis suggests that this is due to the lack of protons H + When the reaction between the raw materials is insufficient, the polyacid salt cannot be well dispersed.

[0313] Fig.41 This is the TEM image (transmission electron microscope image) of Pd-APMo / AS-20H. It was observed that the catalyst basically presents a two-dimensional nanosheet structure.

[0314] Comparative Example 3:

[0315] This example provides an alumina-supported composite catalyst, which is prepared in the same manner as in Example 1, except that deionized water is replaced with an equal volume of anhydrous ethanol. The resulting catalyst is recorded as Pd-H3PMo / Al2O3-ethanol.

[0316] Fig.42 The TEM image (transmission electron microscope image) of Pd-H3PMo / Al2O3-ethanol shows that the obtained catalyst is a solid structure, proving that adding water during the catalyst preparation process is a necessary condition for the formation of a hollow structure.

[0317] Application Example 1 (O-tert-butylphenol hydrogenation reaction):

[0318] (1) The performance of the catalysts prepared in Examples 1-10, Examples 14-20 and Comparative Examples 1-3 in the hydrogenation of o-tert-butylphenol to prepare o-tert-butyl cyclohexanol was evaluated. The operation process was as follows: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm. The catalyst loading was 10 g. The reaction pressure was 3 MPa, the reaction temperature was 80-85 °C, and the mass liquid hourly space velocity of o-tert-butylphenol was 1 h -1 , hydrogen is the hydrogenating agent, and the molar ratio of hydrogen to o-tert-butylphenol is 5:1.

[0319] See Table 1 for specific results.

[0320]

[0321] Application Example 2 (Hydrogenation of Cyclopentylbutyrolactone):

[0322] (1) The performance of the catalysts prepared in Examples 1-10, Examples 14-20 and Comparative Examples 1-3 in the hydrogenation reaction of cyclopentylbutyrolactone was evaluated. The operation process was as follows: 0.1 g of catalyst, 20 g of cyclopentylbutyrolactone, and 20 g of methanol were added to a 100 mL high-pressure reactor in sequence, and the pressure was increased to 4 MPa after hydrogen replacement, and then the temperature was raised to 150 ° C for reaction for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0323] The reaction formula is:

[0324] .

[0325] For specific results, see Table 2-1.

[0326]

[0327] (2) Cyclic stability test:

[0328] The catalytic reaction was carried out in a fixed bed reactor with a mass space velocity of 0.5 h -1 The molar ratio of methanol to cyclopentylbutyrolactone is 5:1, the molar ratio of hydrogen to cyclopentylbutyrolactone is 20:1, the catalyst loading is 8 g, the reaction temperature is 145 °C, the reaction pressure is 4 MPa, and the results of conversion rate and selectivity at each operating time stage are shown in Table 2-2.

[0329]

[0330] Application Example 3 (Preparation of 2-pentylcyclopentenone by hydroisomerization of 2-pentylidenecyclopentanone):

[0331] The reaction performance of the catalysts prepared in Examples 1-10, Examples 14-20 and Comparative Examples 1-3 in the preparation of 2-pentylcyclopentenone by hydroisomerization of 2-pentylcyclopentanone was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of 2-pentylcyclopentenone were added to a 2 L reactor in sequence, and hydrogen was continuously introduced after nitrogen replacement at a hydrogen flow rate of 200 mL / min, and then the temperature was raised to 40 ° C and the reaction was kept at a constant temperature for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector.

[0332] The reaction formula is:

[0333]

[0334] See Table 3 for specific results.

[0335]

[0336] Application Example 4 (Preparation of phenylpentanol by hydrogenation of rose ether):

[0337] The reaction performance of the catalyst prepared in Example 11 in the preparation of phenylpentanol by hydrogenation of rose oxide was evaluated. The operation process was as follows: 0.1 g of catalyst and 50 g of rose oxide were added to a 100 mL high-pressure reactor in sequence, and the pressure was increased to 3 MPa after hydrogen replacement, and then the temperature was raised to 140 ° C for reaction for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0338] The reaction formula is:

[0339] .

[0340] See Table 4 for specific results.

[0341]

[0342] Application Example 5 (Preparation of ethylamine by hydroamination of ethanol):

[0343] Evaluation of the performance of the catalyst prepared in Example 12 in the preparation of ethylamine by ethanol amination: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 140 °C, reaction pressure 0.4 MPa, mass liquid hourly space velocity of ethanol 0.5 h -1 , the molar ratio of ammonia to alcohol is 1: 1. After separation, the product is analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is TCD detector.

[0344] The reaction formula is:

[0345]

[0346] See Table 5 for specific results.

[0347]

[0348] Note: The selectivity of ethylamine is the total selectivity of monoethylamine + diethylamine + triethylamine.

[0349] Application Example 6 (Preparation of Isopropylamine by Amination of Acetone):

[0350] Evaluation of the performance of the catalyst prepared in Example 13 in the preparation of isopropylamine by amination of acetone: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 90°C, reaction pressure 0.4 MPa, mass liquid hourly space velocity of acetone 2 h -1 , the molar ratio of ammonia to acetone is 2:1, and the molar ratio of hydrogen to acetone is 1.5:1. After separation, the products are analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is TCD detector.

[0351] The reaction formula is:

[0352]

[0353] See Table 6 for specific results.

[0354]

[0355] Note: Isopropylamine selectivity refers to the total selectivity of monoisopropylamine and diisopropylamine.

[0356] Application Example 7 (Preparation of tert-butylamine by amination of isobutylene):

[0357] The performance of the catalyst prepared in Example 13 in the reaction of preparing tert-butylamine by amination of isobutylene was evaluated. A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 170 °C, reaction pressure 6 MPa, mass liquid hourly space velocity of isobutylene 0.5 h -1 , the molar ratio of ammonia to isobutylene is 1: 1. After separation, the product is analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is TCD detector.

[0358] The reaction formula is:

[0359] .

[0360] See Table 7 for specific results.

[0361]

[0362] Application Example 8:

[0363] The performance of the catalysts prepared in Examples 1-4 and Comparative Examples 1-3 in the hydrogen peroxide oxidation reaction of benzyl alcohol was evaluated. The operation process was as follows: 10 g of the catalyst, 600 g of benzyl alcohol, 620 mL of 30% by mass hydrogen peroxide and 1000 mL of acetonitrile were added in sequence into a 5 L round-bottom flask, condensed and refluxed, and the temperature was raised to 60 ° C for reaction for 10 h.

[0364] The reaction formula is:

[0365] .

[0366] See Table 8 for specific results.

[0367]

[0368] Application Example 9 (Selective oxidation of C3-C10 aldehydes to produce acids):

[0369] The performance of the catalysts prepared in Example 1, Example 12, 13 and Comparative Examples 1-3 in the selective oxidation reaction of C3-C10 aldehydes to prepare the corresponding acid reaction was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of substrate were added to a 2 L reactor in sequence, and oxygen was continuously introduced after nitrogen replacement at an oxygen flow rate of 30 mL / min. The temperature was raised to 45 °C for reaction, and the reaction was stopped after 8 hours. After separation, the product was analyzed using a Shimadzu GC2014 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0370] See Table 9 for specific results.

[0371]

[0372] Application Example 10 (Selective oxidation of alcohol to produce acid):

[0373] The performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the selective oxidation of alcohol to produce acid was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of substrate were added to a 2 L reactor in sequence, oxygen was continuously introduced after nitrogen replacement, the pressure was increased to 0.5 MPa, the oxygen flow rate was 50 mL / min, the temperature was increased to 95 ° C, and the reaction was stopped after 8 hours. After separation, the product was analyzed by Shimadzu GC2014 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was FID detector. The conversion rate and selectivity were calculated by normalization method.

[0374] See Table 10 for specific results.

[0375]

[0376] Application Example 11 (Selective oxidation of aromatic hydrocarbons to prepare aromatic acids):

[0377] The performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the selective oxidation of aromatic hydrocarbons to prepare aromatic acids was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of substrate were added to a 2 L reactor in sequence, oxygen was continuously introduced after nitrogen replacement, the pressure was increased to 2 MPa, the oxygen flow rate was 50 mL / min, the temperature was increased to 145 ° C, and the reaction was stopped after 8 hours. After separation, the product was analyzed by Shimadzu GC2014 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was FID detector. The conversion rate and selectivity were calculated by normalization method. See Table 11 for specific results.

[0378]

[0379] Application Example 12 (esterification reaction):

[0380] The esterification performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in 2-methylbutyric acid with methanol, ethanol, isopropanol, n-butanol and n-hexanol was evaluated. The operation process was as follows: 0.1 g of catalyst and 20 g of 2-methylbutyric acid and the corresponding alcohol (the acid-alcohol molar ratio was controlled to be 0.7:1) were added to a 100 mL high-pressure reactor, and the temperature was raised to 65 ° C for 6 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method. For specific results, see Table 12 (the conversion rate is the conversion rate of 2-methylbutyric acid, and the selectivity is the selectivity of the corresponding ester prepared).

[0381]

[0382] Application Example 13 (esterification reaction):

[0383] The esterification performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in salicylic acid with n-pentanol, n-hexanol, benzyl alcohol, leaf alcohol, cyclohexanol, isooctyl alcohol and isophorol was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of salicylic acid and the corresponding alcohol (the acid-alcohol molar ratio was controlled to be 0.95:1) were added to a 2 L reactor in sequence, the temperature was raised to 80 ° C, the system pressure was controlled to be 500 mmHg, the generated water was separated by a water separator, the oil phase was refluxed, and the reaction was carried out for 6 hours. After separation, the product was analyzed by Agilent 1260 liquid chromatograph. The conversion rate and selectivity were calculated by normalization method.

[0384] For specific results, please refer to Table 13 (the conversion rate is the conversion rate of salicylic acid, and the selectivity is the selectivity of the corresponding ester prepared).

[0385]

[0386] Application Example 14 (esterification reaction):

[0387] The catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 were evaluated for their esterification performance in acetic acid, hexanoic acid, heptanoic acid, phenylpropionic acid, phenoxyacetic acid, cyclohexyloxyacetic acid and allyl alcohol. The operation process was as follows: 0.1 g of catalyst and 20 g of allyl alcohol and the corresponding acid (the acid-alcohol molar ratio was controlled to be 1.1:1) were added sequentially into a 100 mL autoclave, and the temperature was raised to 75 °C for 9 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0388] See Table 14 for specific results.

[0389]

[0390] Application Example 15 (esterification reaction):

[0391] The catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 were evaluated for their esterification performance in catalyzing acetic acid with o-tert-butyl cyclohexanol, p-tert-butyl cyclohexanol, α-phenylethanol and β-phenylethanol. The operation process was as follows: 4 g of catalyst and 800 g of acetic acid, as well as the corresponding alcohol (the acid-alcohol molar ratio was controlled to be 1.2) were added to a 2L reactor in sequence, the temperature was raised to 80 °C, the vacuum degree of the system was controlled to be 500 mmHg, the water produced was separated by a water separator, the oil phase was refluxed, and the reaction was performed for 6 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0392] See Table 15 for specific results.

[0393]

[0394] Application Example 16 (esterification reaction):

[0395] The esterification performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in acetic acid, propionic acid, n-butyric acid, isobutyric acid and dicyclopentadiene was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of dicyclopentadiene and the corresponding acid (the acid-olefin molar ratio was controlled to be 1.2:1) were added to a 2 L reactor in sequence, and the temperature was raised to 80 °C for 6 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0396] See Table 16 for specific results.

[0397]

[0398] Application Example 17:

[0399] (1) Preparation of epoxypinene by reaction of α-pinene with hydrogen peroxide

[0400] The reaction performance of the catalysts prepared in Examples 1-20 and Comparative Examples 1-3 in the preparation of epoxy pinane by the reaction of α-pinene with hydrogen peroxide was evaluated. The operation process was as follows: 4 g of catalyst, 600 g of toluene, and 300 g of α-pinene were added to a 2 L reactor in sequence, the temperature was raised to 70°C, 200 g of hydrogen peroxide (mass fraction 50%) was added dropwise, the addition was continued for 12 hours, and the reaction was carried out at a constant temperature for 3 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector.

[0401] Reaction:

[0402] .

[0403] (2) Preparation of epoxylimonene by reaction of limonene with hydrogen peroxide

[0404] The reaction performance of the catalysts prepared in Examples 1-20 and Comparative Examples 1-3 in the preparation of epoxylimonene by the reaction of limonene with hydrogen peroxide was evaluated. The operation process was as follows: 4 g of catalyst, 600 g of toluene, and 300 g of limonene were added to a 2 L reactor in sequence, the temperature was raised to 70 ° C, 60 g of hydrogen peroxide (mass fraction 50%) was added dropwise, the addition lasted for 8 hours, and the reaction was carried out at a constant temperature for 3 hours. After separation, the product was analyzed using an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was an FID detector.

[0405] Reaction:

[0406]

[0407] See Table 17 for specific results.

[0408]

[0409] Application Example 18 (Continuous Alkylation of Propylene and Meta-Cresol):

[0410] Evaluation of the performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the continuous alkylation of propylene and m-cresol to prepare thymol: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 220 °C, reaction pressure 0.2 MPa, mass liquid hourly space velocity of m-cresol was 2.5 h -1 The molar ratio of propylene to m-cresol was 0.6:1 and the operation was 200 h. The specific results are shown in Table 18.

[0411]

[0412] Application Example 19 (Isomerization of o-cresol to prepare m-cresol and p-cresol):

[0413] Evaluation of the performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the isomerization of o-cresol to prepare m-cresol and p-cresol: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 280 °C, reaction pressure 0.15 MPa, mass liquid hourly space velocity of o-cresol was 0.8 h -1 , and run for 100 h. The single-pass conversion rate of o-cresol, m-cresol selectivity, and p-cresol selectivity were analyzed by chromatography. See Table 19 for specific results.

[0414]

[0415] Application Example 20 (Dehydration of 2-(1-hydroxypentyl)-cyclopentanone to prepare 2-pentylidenecyclopentanone):

[0416] The reaction performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the dehydration of 2-(1-hydroxypentyl)-cyclopentanone to prepare 2-pentylidenecyclopentanone was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of 2-(1-hydroxypentyl)-cyclopentanone were added to a 2 L reactor in sequence, the temperature was raised to 90 ° C, the vacuum degree of the system was controlled to be about 350 mmHg, and the reaction was carried out at a constant temperature for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0417] Reaction:

[0418] .

[0419] See Table 20 for specific results.

[0420]

[0421] Application Example 21 (Preparation of Habanolide by Dehydration of Hydroxycyclopentadecalactone):

[0422] The reaction performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the dehydration of hydroxycyclopentadecalactone to prepare harpa lactone was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of hydroxycyclopentadecalactone were added to a 2 L reactor in sequence, and the temperature was raised to 100 ° C. The vacuum degree of the system was controlled to be about 350 mmHg, and the reaction was carried out at a constant temperature for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0423] Reaction:

[0424] .

[0425] See Table 21 for specific results.

[0426]

[0427] Application Example 22 (Self-etherification of 2-(3-hydroxypropyl)cyclododecanone to prepare trideca-oxabicyclo[10.4.0]hexadecene):

[0428] The reaction performance of the catalyst prepared in Example 1 and Comparative Examples 1-3 in the self-etherification of 2-(3-hydroxypropyl)cyclododecanone to prepare trideca-oxabicyclo[10.4.0]hexadecene was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of 2-(3-hydroxypropyl)cyclododecanone were added to a 2 L reactor in sequence, and the temperature was raised to 90 ° C. The vacuum degree of the system was controlled to be about 350 mmHg, and the reaction was carried out at a constant temperature for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector.

[0429] Reaction:

[0430]

[0431] See Table 22 for specific results.

[0432]

[0433] Application Example 23 (Propylene Hydration to Prepare Isopropanol):

[0434] The performance of the catalysts prepared in Example 1, Example 12, Example 13 and Comparative Examples 1-3 in the preparation of isopropanol by hydration of propylene was evaluated: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature was 150 °C, reaction pressure was 7 MPa, and the volume liquid hourly space velocity of propylene was 0.8 h -1 , the molar ratio of water to propylene is 10:1. After separation, the product was analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was FID detector. See Table 23 for specific results.

[0435]

[0436] Application Example 24 (Preparation of Cyclopentadecalactone by Hydrogenation of Habanolide):

[0437] The reaction performance of the catalyst prepared in Example 11 in the hydrogenation of halbalactone to prepare cyclopentadecalactone was evaluated. The operation process was as follows: 0.1 g of catalyst and 50 g of halbalactone were added to a 100 mL high-pressure reactor in sequence, and the pressure was increased to 0.5 MPa after hydrogen replacement, and then the temperature was raised to 40 ° C for reaction for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0438] The reaction formula is:

[0439]

[0440] See Table 24 for specific results.

[0441]

[0442] Application Example 25 (Preparation of p-tert-butyl cyclohexanol by hydrogenation of p-tert-butylphenol):

[0443] The performance of the catalyst prepared in Example 12 in the hydrogenation reaction of tert-butylphenol was evaluated. The operation process was as follows: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm. The catalyst loading was 10 g. The reaction pressure was 3 MPa, the reaction temperature was 80-85 °C, and the mass liquid hourly space velocity of tert-butylphenol was 0.5 h -1 , hydrogen was used as the hydrogenating agent, and the molar ratio of hydrogen to p-tert-butylphenol was 5: 1. See Table 25 for specific results.

[0444]

[0445] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

[0446] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. An alumina-supported composite catalyst, characterized in that: The alumina-supported composite catalyst comprises an alumina carrier, a heteropoly acid dispersed in a single molecule state and connected to the alumina carrier, and an active metal component dispersed in a single atom state and connected to one or both of the heteropoly acid and the alumina carrier, wherein the heteropoly acid is a proton-type heteropoly acid capable of providing hydrogen ions, and the alumina carrier has a three-dimensional hollow porous structure; The alumina-supported composite catalyst is prepared by a preparation method that meets the following conditions: (a) using an aluminum oxide precursor and an active metal precursor as raw materials, respectively, wherein the aluminum oxide precursor and the active metal precursor refer to substances that can be converted into aluminum oxide or active metal components through one or more conversion treatments, and the conversion treatment at least includes a treatment for producing a chemical reaction; (b) carrying out the one or more conversion treatments in the presence of the protic heteropolyacid and water; (c) The conversion treatment comprises a solvent evaporation-induced gelation treatment and a calcination treatment performed sequentially, and the solvent evaporation-induced gelation treatment is performed in the presence of water, an organic solvent and a surfactant.

2. The alumina-supported composite catalyst according to claim 1, characterized in that: In the proton-type heteropolyacid, heteroatoms and polyatoms are coordinated and bridged by oxygen atoms, the heteroatoms include at least one selected from P, Si, Fe, and Co, and the polyatoms include at least one selected from Mo, W, V, Nb, and Ta.

3. The alumina-supported composite catalyst according to claim 1, characterized in that: In the alumina-supported composite catalyst, the proton-type heteropoly acid is connected to the alumina support at least through a covalent bond.

4. The alumina-supported composite catalyst according to claim 1, characterized in that: A covalent bond is formed between the polyatoms in the proton type heteropoly acid, the terminal oxygen in the proton type heteropoly acid, and the aluminum atom in the alumina support.

5. The alumina-supported composite catalyst according to claim 1, characterized in that: The proton type heteropoly acid is uniformly dispersed in the skeleton, inside the pores and on the surface of the alumina carrier.

6. The alumina-supported composite catalyst according to claim 1, characterized in that: The active metal component is connected to the proton type heteropoly acid through a chemical bond, wherein the chemical bond includes a coordination bond, and the active metal component is also selectively adsorbed on the alumina carrier.

7. The alumina-supported composite catalyst according to claim 1, characterized in that: The pores in the three-dimensional hollow porous structure are randomly distributed in the three-dimensional direction.

8. The alumina-supported composite catalyst according to claim 1, characterized in that: The three-dimensional hollow porous structure has a single hollow chamber or a cavity combination formed by a plurality of hollow chambers gathered in a connected state or a partially connected state.

9. The alumina-supported composite catalyst according to claim 8, characterized in that: The diameter of the hollow cavity or the cavity combination is 1-90 nm; or, the ratio of the diameter of the hollow cavity or the cavity combination to the particle size of the alumina-supported composite catalyst is 0.3-0.9:

1.

10. The alumina-supported composite catalyst according to claim 1, characterized in that: The average pore size of the alumina-supported composite catalyst is 2-30 nm, and the average pore volume is 0.4-1.5 cc / g; and / or the average density of the alumina-supported composite catalyst is 0.5-4.0 g / cm 3 .

11. The alumina-supported composite catalyst according to claim 1, characterized in that: The average particle size of the alumina-supported composite catalyst is 10-350 nm.

12. The alumina-supported composite catalyst according to claim 11, characterized in that: The average particle size of the alumina-supported composite catalyst is 80-250 nm.

13. The alumina-supported composite catalyst according to claim 1, characterized in that: The alumina-supported composite catalyst is in a spherical structure.

14. The alumina-supported composite catalyst according to claim 1, characterized in that: The active metal component is a combination of one or more selected from transition metals; and / or, in terms of mass percentage, the mass content of the active metal component in the alumina-supported composite catalyst is 0.01%-15%.

15. The alumina-supported composite catalyst according to claim 14, characterized in that: The active metal component is a combination of one or more selected from Group IB-IIB and Group VB-VIIIB.

16. The alumina-supported composite catalyst according to claim 15, characterized in that: The active metal component is a combination of one or more selected from Pd, Pt, Ru, Au, Ag, Rh, Ni, Cu, Fe and Co; and / or, in terms of mass percentage, the mass content of the active metal component in the alumina-supported composite catalyst is 0.04%-15%.

17. The alumina-supported composite catalyst according to claim 1, characterized in that: The proton-type heteropolyacid comprises a combination of one or more selected from phosphomolybdic acid, phosphotungstic acid, silicotungstic acid, silicomolybdic acid, phosphovanadium heteropolyacid, phosphoniobic acid, phosphotantalum heteropolyacid, ferromolybdenum heteropolyacid, ferrotungsten heteropolyacid, ferrovanadium heteropolyacid, cobaltmolybdenum heteropolyacid, cobalttungsten heteropolyacid, and cobaltvanadium heteropolyacid; and / or, in terms of mass percentage, the mass content of the proton-type heteropolyacid in the alumina-supported composite catalyst is 1%-68%.

18. The alumina-supported composite catalyst according to claim 17, characterized in that: In terms of mass percentage, the mass content of the proton-type heteropoly acid in the alumina-supported composite catalyst is 7%-45%.

19. The alumina-supported composite catalyst according to claim 18, characterized in that: In terms of mass percentage, the mass content of the proton-type heteropoly acid in the alumina-supported composite catalyst is 7%-25%.

20. The alumina-supported composite catalyst according to claim 1, characterized in that: The specific surface area of ​​the alumina-supported composite catalyst is greater than or equal to 200 m 2 / g.

21. The alumina-supported composite catalyst according to claim 20, characterized in that: The specific surface area of ​​the alumina-supported composite catalyst is less than or equal to 1000 m 2 / g.

22. The alumina-supported composite catalyst according to claim 20 or 21, characterized in that: The specific surface area of ​​the alumina-supported composite catalyst is 200-800 m 2 / g.

23. The alumina-supported composite catalyst according to claim 1, characterized in that: The aluminum oxide precursor is a compound containing aluminum and an organic group selected from acidic, alkaline or neutral compounds.

24. The alumina-supported composite catalyst according to claim 1 or 23, characterized in that: The aluminum oxide precursor is a combination of one or more selected from aluminum alcohol compounds, hydrocarbon aluminum compounds, and organic aluminates.

25. The alumina-supported composite catalyst according to claim 1, characterized in that: The precursor of aluminum oxide is a combination of one or more selected from trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum chloride, aluminum isopropoxide, aluminum n-butoxide, aluminum acetate, and aluminum propionate.

26. The alumina-supported composite catalyst according to claim 1, characterized in that: The active metal precursor is a salt of an active metal component and / or an acid of an active metal component. The salt of the active metal component includes a combination of one or more selected from metal nitrates, metal sulfates, metal halides, metal acetylacetonate complexes, and metal sulfides. The acid of the active metal component includes a halogenated metal acid.

27. The alumina-supported composite catalyst according to claim 1, characterized in that: The active metal precursor is a combination of one or more selected from palladium chloride, palladium nitrate, platinum acetylacetonate, gold chloride, silver nitrate, ruthenium chloride, ruthenium nitrate, rhodium chloride, rhodium nitrate, cobalt nitrate, nickel nitrate, ferric chloride, ferric sulfate, copper nitrate, copper sulfate, chloroplatinic acid, chloropalladic acid, chloroauric acid, and rhodium acetylacetonate.

28. A method for preparing an alumina-supported composite catalyst according to any one of claims 1 to 27, characterized in that: The preparation method comprises: Gelation treatment: mixing the proton type heteropoly acid with the precursor of aluminum oxide in the presence of water, an organic solvent and a surfactant, and inducing the solvent evaporation to form a gel, wherein: the temperature of the mixing reaction is controlled to be 20-50° C. and the reaction time is controlled to be not less than 12 h; Calcination treatment: drying the gel and then calcining it, and performing a reduction treatment in the presence of a reducing agent to obtain the alumina-supported composite catalyst; The preparation method further includes the step of adding an active metal precursor before the mixing reaction, or the step of coating with a solution containing the active metal precursor after the calcination and before the reduction treatment, wherein the coating includes spraying, brushing, rolling, dipping or scraping.

29. The method for preparing an alumina-supported composite catalyst according to claim 28, characterized in that: The feed mass ratio of the water to the aluminum oxide precursor is 0.001-15:1; and / or the feed volume ratio of the water to the organic solvent is 0.001-5:

1.

30. The method for preparing an alumina-supported composite catalyst according to claim 29, characterized in that: The feed mass ratio of the water to the aluminum oxide precursor is 0.01-10:1; and / or the feed volume ratio of the water to the organic solvent is 0.001-2:

1.

31. The method for preparing an alumina-supported composite catalyst according to claim 29, characterized in that: The feed mass ratio of the water to the aluminum oxide precursor is 0.1-5:1; and / or the feed volume ratio of the water to the organic solvent is 0.005-1:

1.

32. The method for preparing an alumina-supported composite catalyst according to claim 28, characterized in that: The surfactant is a block copolymer nonionic surfactant and / or an ionic surfactant, the block copolymer nonionic surfactant includes a combination of one or more selected from nonionic surfactant P123, nonionic surfactant F127, and nonionic surfactant F108, the ionic surfactant includes a combination of one or more selected from hexadecyltrimethylammonium bromide, sodium oleate, sodium dodecylbenzene sulfonate, and sodium stearate; and / or the feed mass ratio of the surfactant to the proton-type heteropolyacid is 3~30:

1.

33. The method for preparing the alumina-supported composite catalyst according to claim 28, characterized in that: The organic solvent is a polar organic solvent; and / or the feed mass ratio of the proton type heteropoly acid to the organic solvent is 1:80-1000.

34. The method for preparing an alumina-supported composite catalyst according to claim 28, characterized in that: The organic solvent is a combination of one or more selected from methanol, ethanol, isopropanol, acetone, tetrahydrofuran, and N,N-dimethylformamide.

35. The method for preparing the alumina-supported composite catalyst according to any one of claims 28 to 34, characterized in that: The time of the mixed reaction is controlled to be 12-15 h, 15-18 h, 18-21 h, 21-24 h, 24-27 h, 27-30 h or 30-48 h.

36. The method for preparing the alumina-supported composite catalyst according to any one of claims 28 to 34, characterized in that: The solvent evaporation induction is controlled to be carried out at a temperature of 40-120°C and a time of 1-72 h.

37. The method for preparing the alumina-supported composite catalyst according to any one of claims 28 to 34, characterized in that: The solvent evaporation induction is controlled to be carried out at a temperature of 60-75°C for a time of 10-60 hours.

38. The method for preparing the alumina-supported composite catalyst according to any one of claims 28 to 34, characterized in that: The calcination is performed at 200-700°C; and / or, the calcination is performed in a muffle furnace, the calcination time is controlled to be 1-6 h, and the heating rate is 1-30°C / min; and / or, the calcination is performed in an aerobic environment, the aerobic environment includes an air atmosphere or a pure oxygen atmosphere, and the pure oxygen atmosphere is formed by introducing pure oxygen gas with a purity greater than 99%.

39. An alumina-supported composite catalyst, characterized in that: It is prepared by the following method: (1) reacting a proton-type heteropoly acid with an alcohol aluminum compound and / or a C1-C12 hydrocarbon aluminum compound in the presence of water, a C2-C4 alcohol solvent and a surfactant at 20-50°C for 12-48 hours, and inducing solvent evaporation at a temperature of 60-75°C for 10-72 hours to prepare a gel: The proton type heteropoly acid is a combination of one or more selected from phosphomolybdic acid, phosphotungstic acid, silicotungstic acid, and silicomolybdic acid; (2) drying the gel to obtain a solid, and then calcining the solid at 300-450° C. in an air atmosphere to obtain an alumina-supported heteropoly acid; (3) The salt of the active metal component and / or the acid of the active metal component is loaded on the alumina-loaded heteropolyacid, and then the alumina-loaded composite catalyst is obtained by first calcining the alumina-loaded composite catalyst in an air atmosphere at 200-400°C and then second calcining the alumina-loaded composite catalyst in a hydrogen atmosphere at 150-300°C. The alumina-loaded composite catalyst comprises an alumina carrier, a proton-type heteropolyacid dispersed in a single molecule state and connected to the alumina carrier, and an active metal component dispersed in a single atom state and connected to one or both of the proton-type heteropolyacid and the alumina carrier, wherein the alumina carrier has a three-dimensional hollow porous structure.

40. A catalyst composition, characterized in that: It comprises the alumina-loaded composite catalyst as described in any one of claims 1 to 27 and 39 and at least one other catalyst different from the alumina-loaded composite catalyst; wherein, in terms of mass percentage, the mass content of the alumina-loaded composite catalyst in the catalyst composition exceeds 50%.

41. Use of the alumina-supported composite catalyst according to any one of claims 1 to 27 and 39, or the alumina-supported composite catalyst prepared by the preparation method according to any one of claims 28 to 38, or the catalyst composition according to claim 40 in the following reactions: oxidation reaction of aromatic hydrocarbons, alcohols or aldehydes, esterification reaction of olefins with acids or esterification reaction of alcohols with acids, epoxidation reaction of olefins, alkylation reaction of aromatic compounds, isomerization reaction, dehydration reaction of alcohols, etherification reaction, hydration reaction of olefins, hydrogenation reaction, amination reaction of alcohols, ketones or olefins.

Citation Information

Patent Citations

  • Composite nano-catalyst as well as preparation method and application thereof

    CN117138812A

  • Method for preparing sulfonic acid group-modified mesoporous material-loaded heteropolyacid catalyst and application thereof during esterification reaction

    CN105854942A

  • Monomolecular heteropolyacid inlaid honeycomb-shaped carbon material loaded nano-metal catalyst as well as preparation method and application thereof

    CN111167515A

  • Porous carbon supported monomolecular heteropolyacid catalyst as well as preparation method and application thereof

    CN111167516A

  • Supported hydrogenation and hydrotreating catalysts and process

    EP0494528A1

Cited By

  • Method for preparing aviation oil component through alkylation-hydrodeoxygenation of biomass platform compound

    CN122214037A