A high-hardness PET optical film and preparation method thereof
By adding nanoparticle intercalation modified montmorillonite composite material to PET slices and performing extrusion granulation, bidirectional stretching and coating polyacrylate coating liquid, the low surface hardness and visual fatigue of PET optical film are solved. The problem of this paper is to achieve high hardness, moderate haze and high transparency optical films, which improves mechanical properties and transmittance.
Patent Information
- Application Number
- CN202410775040.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-06-17
AI Technical Summary
The existing PET optical film has low surface hardness and is not wear-resistant, and the high transparency optical film may cause visual fatigue on the liquid crystal display screen, and the existing additives cause uneven dispersion, affecting smoothness and transmittance.
Add nanoparticle intercalation modified montmorillonite composite material to PET sections, and optimize the internal structure and surface of the film through extrusion granulation, bidirectional stretching, coating polyacrylate coating liquid and ultraviolet cross-linking steps. Function to produce high hardness and moderate haze optical film.
An optical film with high hardness, moderate haze and high transparency is achieved, which improves the mechanical properties and visual effects of the film, avoids visual fatigue, and maintains high transmittance.
Smart Images

Figure SMS_3 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical-grade PET films, in particular to a high-hardness PET optical film and a preparation method thereof. Background Art
[0002] Biaxially oriented polyester film (BOPET) has excellent properties such as high tensile hardness, good electrical insulation and optical properties, cold and heat resistance, chemical corrosion resistance and stable shrinkage. It is widely used in packaging, magnetic materials, imaging and electronic fields.
[0003] With the rapid development of electronic technology, liquid crystal display screens, as key components in many digital electronic products, have attracted the attention of many researchers. Liquid crystal display screens are fragile and easily scratched or damaged by gravity, so they need to be protected by screen protectors. PET has always been the preferred material for touch and display screen coating substrates. However, BOPET films made from upstream PET slices generally have defects such as low surface hardness and poor wear resistance; in addition, when optical films that blindly pursue high transparency and low haze are applied to liquid crystal display screens, they may cause visual fatigue to people watching the screen due to the excessively high vertical light transmission ratio. In order to solve these problems, auxiliary additives with small particle sizes, such as nanofillers, can be added to PET, but the direct addition of such additives may lead to uneven dispersion, easy agglomeration affecting the smoothness of the film surface, and easy migration leading to a decrease in the transmittance of the film surface. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention adds nanoparticle intercalation modified montmorillonite composite materials to PET slices for melt stretching, and then coats a layer of acrylic coating liquid on the stretched thin sheet. By optimizing the internal structure of the film and modifying the surface function, an optical film with moderate haze, high transparency and high hardness is obtained.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a high-hardness PET optical film comprises the following steps:
[0007] S1, washing, drying, grinding and mixing the nanoparticle intercalation modified montmorillonite composite material with PET slices, putting the mixture into an extruder for extrusion granulation to obtain a cast sheet;
[0008] S2, feeding the cast sheet into a biaxial stretching machine and forming a thin sheet by longitudinal stretching;
[0009] S3, coating the polyacrylate coating liquid on the thin green sheet by online coating;
[0010] S4, the coated thin sheet is stretched transversely to obtain a PET film with a surface coating;
[0011] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, followed by relaxation and cooling, and winding up under the traction of a traction roller, to obtain;
[0012] The preparation process of the nanoparticle intercalation modified montmorillonite composite material is as follows:
[0013] 1) A certain amount of inorganic nanoparticles is placed in a 5wt% potassium hydroxide solution for activation treatment, and then the treated inorganic nanoparticles are redispersed in deionized water and an equal amount of KH550 is added, stirred at 50°C for 24 hours, filtered, washed, dried, and ground to obtain an inorganic powder; the inorganic powder is redispersed in deionized water, and ammonium persulfate is added and stirred to make it evenly dispersed;
[0014] 2) Sodium montmorillonite is ultrasonically dispersed in deionized water to form a montmorillonite suspension with a mass fraction of 30-50wt%, and the temperature is raised to 60-70°C. The dispersion in step 1) is slowly added under stirring. After the addition is completed, nitrogen is introduced. Under light-proof conditions, hydroxypropyl methacrylate and methyl coumarin methyl methacrylate are mixed and slowly added to the mixture. The mixture is stirred for reaction for 1-5h. After the reaction is completed, the mixture is filtered, washed and dried to obtain the product;
[0015] The polyacrylate coating liquid is prepared by using methacrylate, butyl acrylate, styrene, acrylic acid, vinyl triethoxysilane and methyl coumarin methyl methacrylate as polymerization monomers and ammonium persulfate as initiator in a composite emulsifier and deionized water.
[0016] More optimally, in step S1, the mass ratio of the nanoparticle intercalation modified montmorillonite composite material to the PET slice is 5-20:95-80; in step S3, the coating amount is 5 g / m 2 ~15 g / m 2 .
[0017] More optimally, the longitudinal stretching ratio is 2.8-3.5:1, and the temperature is 90-115°C; the transverse stretching ratio is 3.5-4.5:1, and the temperature is 100-125°C.
[0018] Preferably, the inorganic nanoparticles are nano-titanium oxide or nano-zirconium oxide or a mixture of the two.
[0019] Preferably, in step 1), the mass fraction of the inorganic powder in deionized water is 30-40%; the mass of ammonium persulfate is 3-4% of the inorganic powder.
[0020] More optimally, in the step 2), the mass ratio of sodium montmorillonite to the inorganic powder in the dispersion is 1:0.5-1; the molar ratio of hydroxypropyl methacrylate to methyl coumarin methyl methacrylate is 6-9:1-4; and the mass ratio of the mixture of hydroxypropyl methacrylate and methyl coumarin methyl methacrylate to the inorganic powder is 3-5:1.
[0021] More optimally, the composite emulsifier is a mixture of nonylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate.
[0022] More optimally, the preparation process of the polyacrylate coating liquid is as follows:
[0023] In a reaction bottle, 0.5-1 part of a composite emulsifier is dissolved in 25-35 parts of deionized water and stirred evenly, and then 10-20 parts of methyl methacrylate, 5-10 parts of butyl acrylate, 2-5 parts of styrene, 1-3 parts of acrylic acid, 2-5 parts of vinyl triethoxy silane and 0.5-1 part of ammonium persulfate are added to the reaction bottle, and the pre-emulsion is obtained by rapid emulsification;
[0024] Take another clean reaction bottle, add 5-10 parts of methyl methacrylate, 1-3 parts of butyl acrylate, 2-5 parts of methyl coumarin methyl methacrylate, 0.3-0.6 parts of composite emulsifier and 0.2-0.5 parts of ammonium persulfate, add 0.5 parts of sodium bicarbonate and 15-20 parts of deionized water, stir evenly, heat to 50-60°C, emulsify quickly for 15 minutes, heat to 70-80°C, add the pre-emulsion dropwise to the reaction bottle, continue to react for 1-2 hours after the addition is completed, dissolve 0.2 parts of ammonium persulfate in water and add it to the reaction bottle, keep warm at 80°C for 1 hour;
[0025] After the reaction is completed, cool naturally to room temperature and add 1 to 3 parts of a neutralizing agent to obtain the product.
[0026] More optimally, the neutralizing agent is one of triethylamine, N-dimethylethanolamine, diethylene glycolamine, and triethanolamine.
[0027] The second object of the present invention is to further provide a high-hardness PET optical film prepared by the preparation method as described above.
[0028] Compared with the prior art, the beneficial effects of the present invention are as follows: when preparing the PET optical film, the present invention first adds a self-made nanoparticle intercalation modified montmorillonite composite material during the extrusion granulation process, and the inorganic nanoparticles are combined with the montmorillonite through organic modification, so that the composite material can be evenly dispersed in the PET matrix, and the haze of the PET film can be adjusted by adjusting the proportion of the composite material in the PET matrix. Secondly, after the casting sheet is formed by extrusion granulation, it is first longitudinally stretched once to form a thin blank sheet, and then a layer of polyacrylate coating liquid is coated on the thin blank sheet. The coating liquid is an aqueous emulsion prepared by emulsion polymerization and is environmentally friendly. It is coated on the PET thin blank sheet to enhance the surface hardness of the film layer and the smoothness of the film layer surface, improve the bonding force between the coating layer and the base film layer, and further improve the mechanical properties of the final optical film; improve the rainbow pattern phenomenon of the film layer. DETAILED DESCRIPTION
[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0031] Example: A high-hardness PET optical film
[0032] S1, washing, drying, grinding and mixing the nanoparticle intercalated modified montmorillonite composite material with PET slices in a mass ratio of 5-20:95-80, putting them into an extruder for extrusion granulation to obtain a cast sheet;
[0033] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 2.8-3.5:1, and forming a thin sheet by longitudinal stretching;
[0034] S3, coating the polyacrylate coating liquid on the thin green sheet by online coating;
[0035] S4, the coated thin sheet is stretched transversely, the transverse stretching temperature is 100-125° C., and the stretching ratio is 3.5-4.5:1 to obtain a PET film with a surface coating;
[0036] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, followed by relaxation and cooling, and winding up under the traction of a traction roller, to obtain;
[0037] Among them, PET chips were purchased directly from the market, and the nanoparticle intercalation modified montmorillonite composite material and polyacrylate coating liquid were homemade.
[0038] The above-mentioned process for preparing high-hardness PET optical film adopts the traditional manufacturing process, i.e., extrusion granulation-biaxial stretching-traction winding. The difference is that a homemade nanoparticle intercalation modified montmorillonite composite material is first added in the extrusion granulation process. The nanoparticles are composed of nano-titanium oxide or nano-zirconium oxide or a mixture of the two. Adding them to PET can adjust the haze of the material. Direct addition is easy to agglomerate and thus affect the mechanical properties of the film. However, in the present application, first, the nanoparticles are activated and then treated with a silane coupling agent so that they can be chemically bonded with organic substances to improve their dispersibility. An aminosilane coupling agent is used for treatment, and ammonium persulfate is added to the dispersion to form a cationic dispersion. Montmorillonite has a lamellar structure, and its application in PET can improve the opening performance of the film. By mixing a cationic nanoparticle dispersion with a montmorillonite suspension, the cationic structure undergoes an intercalation reaction on the montmorillonite layer structure. At the same time, due to the presence of ammonium persulfate, the polymerization of acrylate monomers can be initiated. Hydroxypropyl methacrylate containing a hydrophilic hydroxyl structure and a longer chain and methyl coumarin methyl methacrylate that can be cross-linked by ultraviolet light are used as copolymerization monomers, which improves the intercalation efficiency and provides active sites for subsequent cross-linking. The inorganic nanoparticles are organically modified to be combined with the montmorillonite, so that the composite material can be evenly dispersed in the PET matrix. The haze of the PET film can be controlled by adjusting the proportion of the composite material in the PET matrix.
[0039] After the nanoparticle intercalation modified montmorillonite composite material is blended with PET slices and extruded to form a cast sheet, it is first stretched longitudinally to form a thin sheet, and then a layer of polyacrylate coating liquid is coated on the thin sheet. The coating liquid is an aqueous emulsion prepared by emulsion polymerization, which is environmentally friendly. It is coated on the PET thin sheet to enhance the surface hardness and smoothness of the film layer and improve the rainbow pattern phenomenon of the film layer. In the preparation process, methyl methacrylate is used as the main monomer, and the emulsion is cured with high hardness by adding monomers such as butyl acrylate and styrene; vinyl triethoxysilane is added to improve the surface friction of the film layer and reduce the rainbow pattern phenomenon; and methyl coumarin methyl methacrylate is added to enable it to be cured by ultraviolet light. The coated thin sheet is stretched laterally and shaped and then sent under a UV lamp for final photocuring and cross-linking. The methyl coumarin methyl methacrylate on the surface of the film layer acts as a UV cross-linking agent and forms a cross-linking structure with the polymer chains contained in the thin sheet, thereby improving the bonding strength between the coating layer and the base film layer, and further improving the mechanical properties of the final optical film.
[0040] Embodiment 1:
[0041] Firstly, a nanoparticle intercalation modified montmorillonite composite material was prepared:
[0042] 1) A certain amount of nano-titanium oxide was placed in a 5wt% potassium hydroxide solution for activation treatment, and then the treated inorganic nanoparticles were redispersed in deionized water and an equal amount of KH550 was added, stirred at 50°C for 24h, filtered, washed, dried, and ground to obtain inorganic powder; 30g of the inorganic powder was redispersed in 70g of deionized water, and 1g of ammonium persulfate was added and stirred to make it evenly dispersed;
[0043] 2) 30g of sodium montmorillonite was ultrasonically dispersed in 70g of deionized water to form a montmorillonite suspension with a mass fraction of 30wt%, and the temperature was raised to 60-70°C. 50g of the dispersion obtained in step 1) was slowly added under stirring. After the addition was completed, nitrogen was introduced. Under light-proof conditions, 18.5g of hydroxypropyl methacrylate and 26.5g of methyl coumarin methyl methacrylate were mixed and slowly added to the mixture. The mixture was stirred for reaction for 1-5h. After the reaction was completed, it was filtered, washed and dried to obtain the product;
[0044] Hydroxypropyl Methacrylate: ;Molecular weight 114 g / mol;
[0045] Coumarin Methyl Methacrylate ; Molecular weight 244 g / mol.
[0046] The preparation process of polyacrylate coating liquid is as follows:
[0047] In a reaction bottle, 0.5 parts of a composite emulsifier (a mixture of nonylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate) was dissolved and stirred evenly with 33 parts of deionized water, and then 15 parts of methyl methacrylate, 5 parts of butyl acrylate, 3 parts of styrene, 2 parts of acrylic acid, 3 parts of vinyl triethoxysilane and 0.5 parts of ammonium persulfate were added to the reaction bottle, and the pre-emulsion was prepared by rapid emulsification;
[0048] Take another clean reaction bottle, add 10 parts of methyl methacrylate, 3 parts of butyl acrylate, 3 parts of methyl coumarin methyl methacrylate, 0.3 parts of composite emulsifier and 0.2 parts of ammonium persulfate, add 0.5 parts of sodium bicarbonate and 20 parts of deionized water, stir evenly, heat to 50-60°C, emulsify quickly for 15 minutes, heat to 70-80°C, add the pre-emulsion dropwise to the reaction bottle, continue to react for 1-2 hours after the addition is completed, dissolve 0.2 parts of ammonium persulfate in water and add it to the reaction bottle, keep warm at 80°C for 1 hour;
[0049] After the reaction is completed, the mixture is naturally cooled to room temperature, and N-dimethylethanolamine is added to adjust the pH to weak alkalinity to obtain the product.
[0050] A high hardness PET optical film:
[0051] S1, washing, drying, grinding and mixing the nanoparticle intercalated modified montmorillonite composite material with PET slices in a mass ratio of 5:95, putting them into an extruder for extrusion granulation to obtain a cast sheet;
[0052] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0053] S3, using online coating method to apply polyacrylate coating liquid on the thin blank, the coating amount is 5g / m 2 ;
[0054] S4, the coated thin sheet is stretched transversely, the transverse stretching temperature is 100-125° C., and the stretching ratio is 3.5:1 to obtain a PET film with a surface coating;
[0055] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, then relaxing and cooling, and winding up under the traction of a traction roller to obtain the film.
[0056] Embodiment 2:
[0057] According to the process of Example 1, a nanoparticle intercalation modified montmorillonite composite material and a polyacrylate coating liquid were prepared.
[0058] A high hardness PET optical film:
[0059] S1, washing, drying, grinding and mixing the nanoparticle intercalated modified montmorillonite composite material with PET slices in a mass ratio of 12:88, putting them into an extruder for extrusion granulation to obtain a cast sheet;
[0060] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0061] S3, using online coating method to apply polyacrylate coating liquid on the thin blank, the coating amount is 5g / m 2 ;
[0062] S4, the coated thin sheet is stretched transversely, the transverse stretching temperature is 100-125° C., and the stretching ratio is 3.5:1 to obtain a PET film with a surface coating;
[0063] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, then relaxing and cooling, and winding up under the traction of a traction roller to obtain the film.
[0064] Embodiment 3:
[0065] According to the process of Example 1, a nanoparticle intercalation modified montmorillonite composite material and a polyacrylate coating liquid were prepared.
[0066] A high hardness PET optical film:
[0067] S1, washing, drying, grinding and mixing the nanoparticle intercalated modified montmorillonite composite material with PET slices in a mass ratio of 20:80, putting them into an extruder for extrusion granulation to obtain a cast sheet;
[0068] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0069] S3, using online coating method to apply polyacrylate coating liquid on the thin blank, the coating amount is 5g / m 2 ;
[0070] S4, the coated thin sheet is stretched transversely, the transverse stretching temperature is 100-125° C., and the stretching ratio is 3.5:1 to obtain a PET film with a surface coating;
[0071] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, then relaxing and cooling, and winding up under the traction of a traction roller to obtain the film.
[0072] Embodiment 4:
[0073] According to the process of Example 1, a nanoparticle intercalation modified montmorillonite composite material and a polyacrylate coating liquid were prepared.
[0074] A high hardness PET optical film:
[0075] S1, washing, drying, grinding and mixing the nanoparticle intercalated modified montmorillonite composite material with PET slices in a mass ratio of 12:88, putting them into an extruder for extrusion granulation to obtain a cast sheet;
[0076] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0077] S3, using online coating method to apply polyacrylate coating liquid on the thin blank, the coating amount is 10 g / m 2 ;
[0078] S4, the coated thin sheet is stretched transversely, the transverse stretching temperature is 100-125° C., and the stretching ratio is 3.5:1 to obtain a PET film with a surface coating;
[0079] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, then relaxing and cooling, and winding up under the traction of a traction roller to obtain the film.
[0080] Embodiment 5:
[0081] Firstly, a nanoparticle intercalation modified montmorillonite composite material was prepared:
[0082] 1) A certain amount of nano-titanium oxide was placed in a 5wt% potassium hydroxide solution for activation treatment, and then the treated inorganic nanoparticles were redispersed in deionized water and an equal amount of KH550 was added, stirred at 50°C for 24h, filtered, washed, dried, and ground to obtain inorganic powder; 30g of the inorganic powder was redispersed in 70g of deionized water, and 1g of ammonium persulfate was added and stirred to make it evenly dispersed;
[0083] 2) Take 30g of sodium montmorillonite and ultrasonically disperse it in 70g of deionized water to form a montmorillonite suspension with a mass fraction of 30wt%, heat it to 60-70°C, slowly add 100g of the dispersion in step 1) under stirring, and after the addition is completed, pass nitrogen. Under light-proof conditions, mix 37g of hydroxypropyl methacrylate and 53g of methyl coumarin methyl methacrylate and slowly add them to the mixture, stir and react for 1-5h, and after the reaction is completed, filter it with suction, wash and dry it to obtain the product.
[0084] The preparation of the polyacrylate coating solution was carried out according to Example 1.
[0085] A high hardness PET optical film:
[0086] S1, washing, drying, grinding and mixing the nanoparticle intercalated modified montmorillonite composite material with PET slices in a mass ratio of 5:95, putting them into an extruder for extrusion granulation to obtain a cast sheet;
[0087] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0088] S3, using online coating method to apply polyacrylate coating liquid on the thin blank, the coating amount is 5 g / m 2 ;
[0089] S4, the coated thin sheet is stretched transversely, the transverse stretching temperature is 100-125° C., and the stretching ratio is 3.5:1 to obtain a PET film with a surface coating;
[0090] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, then relaxing and cooling, and winding up under the traction of a traction roller to obtain the film.
[0091] Comparative Example 1:
[0092] S1, washing, drying and grinding equal masses of nano-titanium dioxide and montmorillonite, and then mixing with PET slices in a mass ratio of 5:95, putting them into an extruder for extrusion granulation, and obtaining a cast sheet;
[0093] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0094] S3, stretching the thin blank sheet transversely at a temperature of 100-125°C and a stretching ratio of 3.5:1, followed by relaxation and cooling, and winding up under the traction of a traction roller.
[0095] Comparative Example 2:
[0096] S1, putting PET slices into an extruder for extrusion and granulation to obtain cast sheets;
[0097] S2, sending the cast sheet into a biaxial stretching machine, setting the temperature to 90-115°C, the longitudinal stretching ratio to 3:1, and forming a thin sheet through longitudinal stretching;
[0098] S3, using online coating method to apply polyacrylate coating liquid on the thin blank, the coating amount is 5g / m 2 ;
[0099] S4, stretching the thin sheet transversely at a temperature of 100-125° C. and a stretching ratio of 3.5:1 to obtain a PET film with a surface coating;
[0100] S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, then relaxing and cooling, and winding up under the traction of a traction roller to obtain the film.
[0101] Table 1
[0102]
[0103] The haze of the current commercially available optical film reaches 3%, and most of the modifications to the optical film are concentrated on reducing its haze, so that the haze reaches about 1%. However, if the anti-glare function is to be achieved, the haze needs to be greater than 5%. As can be seen from the above table, increasing the feed ratio of the nanoparticle intercalation modified montmorillonite composite material can effectively improve the haze of the optical film, and the transmittance can be maintained at more than 90%. The haze value in the embodiment of the present application is between 5 and 10%, and it is kept in a suitable range interval, which can achieve anti-glare while the transmittance and clarity of the film are high, and the hardness is also high. If the haze value needs to be increased again, the mass of the nanoparticle intercalation modified montmorillonite composite material can be appropriately increased. By comparing Examples 1-3 and Example 5, it can be seen that the more nanoparticle intercalation modified montmorillonite composite materials, the higher the haze, but at the same time the transmittance will decrease, but if the nanoparticle content is appropriately increased during the preparation process of the nanoparticle intercalation modified montmorillonite composite material, the haze can also be increased without reducing the transmittance. Comparing Example 2 and Example 4, it can be found that increasing the polyacrylate coating liquid can further increase the hardness, but the thickness of the corresponding film will increase. The specific ratio can be adjusted according to actual production needs, with high flexibility. In Comparative Example 1, nano titanium dioxide and montmorillonite are directly added to PET slices, resulting in unconcentrated stress of the film, uneven distribution of the film layer, and poor effect of the prepared film.
[0104] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for preparing a high-hardness PET optical film, characterized in that: The steps include: S1, washing, drying, grinding and mixing the nanoparticle intercalation modified montmorillonite composite material with PET slices, putting the mixture into an extruder for extrusion granulation to obtain a cast sheet; S2, feeding the cast sheet into a biaxial stretching machine and forming a thin sheet by longitudinal stretching; S3, coating the polyacrylate coating liquid on the thin green sheet by online coating; S4, the coated thin sheet is stretched transversely to obtain a PET film with a surface coating; S5, sending the PET film with the surface coating to a UV lamp for UV cross-linking and curing, followed by relaxation and cooling, and winding up under the traction of a traction roller, to obtain; The preparation process of the nanoparticle intercalation modified montmorillonite composite material is as follows: 1) A certain amount of inorganic nanoparticles is placed in a 5wt% potassium hydroxide solution for activation treatment, and then the treated inorganic nanoparticles are redispersed in deionized water and an equal amount of KH550 is added, stirred at 50°C for 24 hours, filtered, washed, dried, and ground to obtain an inorganic powder; the inorganic powder is redispersed in deionized water, and ammonium persulfate is added and stirred to make it evenly dispersed; 2) Sodium montmorillonite is ultrasonically dispersed in deionized water to form a montmorillonite suspension with a mass fraction of 30-50wt%, and the temperature is raised to 60-70°C. The dispersion in step 1) is slowly added under stirring. After the addition is completed, nitrogen is introduced. Under light-proof conditions, hydroxypropyl methacrylate and methyl coumarin methyl methacrylate are mixed and slowly added to the mixture. The mixture is stirred for reaction for 1-5h. After the reaction is completed, the mixture is filtered, washed and dried to obtain the product; The polyacrylate coating liquid is prepared by using methacrylate, butyl acrylate, styrene, acrylic acid, vinyl triethoxysilane and methyl coumarin methyl methacrylate as polymerization monomers and ammonium persulfate as initiator in a composite emulsifier and deionized water; The chemical structural formula of the methyl coumarin methyl methacrylate is: ; In step S1, the mass ratio of the nanoparticle intercalation modified montmorillonite composite material to the PET slice is 5-20:95-80; in step S3, the coating amount is 5 g / m 2 ~15 g / m 2 ; In the step 1), the mass fraction of the inorganic powder in the deionized water is 30-40%; the mass of the ammonium persulfate is 3-4% of the inorganic powder; In the step 2), the mass ratio of sodium montmorillonite to the inorganic powder in the dispersion is 1:0.5-1; the molar ratio of hydroxypropyl methacrylate to methyl coumarin methyl methacrylate is 6-9:1-4; and the mass ratio of the mixture of hydroxypropyl methacrylate and methyl coumarin methyl methacrylate to the inorganic powder is 3-5:
1.
2. The method for preparing a high-hardness PET optical film according to claim 1, characterized in that: The longitudinal stretching ratio is 2.8-3.5:1, and the temperature is 90-115°C; the transverse stretching ratio is 3.5-4.5:1, and the temperature is 100-125°C.
3. The method for preparing a high-hardness PET optical film according to claim 1, characterized in that: The inorganic nanoparticles are nano-titanium oxide or nano-zirconium oxide or a mixture of the two.
4. The method for preparing a high-hardness PET optical film according to claim 1, characterized in that: The composite emulsifier is a mixture of nonylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate.
5. The method for preparing a high-hardness PET optical film according to claim 1, characterized in that: The preparation process of polyacrylate coating liquid is as follows: In a reaction bottle, 0.5-1 part of a composite emulsifier is dissolved in 25-35 parts of deionized water and stirred evenly, and then 10-20 parts of methyl methacrylate, 5-10 parts of butyl acrylate, 2-5 parts of styrene, 1-3 parts of acrylic acid, 2-5 parts of vinyl triethoxy silane and 0.5-1 part of ammonium persulfate are added to the reaction bottle, and the pre-emulsion is obtained by rapid emulsification; Take another clean reaction bottle, add 5-10 parts of methyl methacrylate, 1-3 parts of butyl acrylate, 2-5 parts of methyl coumarin methyl methacrylate, 0.3-0.6 parts of composite emulsifier and 0.2-0.5 parts of ammonium persulfate, add 0.5 parts of sodium bicarbonate and 15-20 parts of deionized water, stir evenly, heat to 50-60°C, emulsify quickly for 15 minutes, heat to 70-80°C, add the pre-emulsion dropwise to the reaction bottle, continue to react for 1-2 hours after the addition is completed, dissolve 0.2 parts of ammonium persulfate in water and add it to the reaction bottle, keep warm at 80°C for 1 hour; After the reaction is completed, cool naturally to room temperature and add 1 to 3 parts of a neutralizing agent to obtain the product.
6. The method for preparing a high-hardness PET optical film according to claim 5, characterized in that: The neutralizing agent is one of triethylamine, N-dimethylethanolamine, diethylene glycolamine and triethanolamine.
7. A high-hardness PET optical film prepared by the preparation method as described in any one of claims 1 to 6.
Citation Information
Cited By
High-strength PET optical film and preparation method thereof
CN120059256A
A high-strength PET optical film and its preparation method
CN120059256B