Antioxidant premix for polyethylene and preparation method thereof
Through the preparation of modified antioxidants, the combination of multiple hindered amines and titanium dioxide is used to solve the problem of aging of polyethylene materials in the photothermal environment, significantly improving the antioxidant performance and maintaining the mechanical properties.
Patent Information
- Application Number
- CN202410796556.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Existing polyethylene materials are prone to aging in photothermal environments, and the existing antioxidants have poor compatibility with polyethylene, resulting in limited antioxidant effects and affecting mechanical properties.
Using modified antioxidants, amine ester exchange is carried out through tetramethylpiperidineamine and methyl thioglycolate to form end thio hindered amine, combined with tetraallyl silane click addition, suspension and chelation loading to submicron-scale titanium dioxide On the surface, chelating organic matter with alkyl acid chloride is combined with chelated organic matter, and antioxidant premixed agent with multiple hindered amine structures is prepared, and it is uniformly dispersed into the polyvinyl matrix through extrusion granulation technology.
It significantly improves the photooxidation resistance of polyethylene, maintains the good mechanical properties of the material during the aging process, and effectively prevents the in-depth aging through the reflection shielding of titanium dioxide and the capture of multiple hindered amines.
Smart Images

Figure BDA0004901921050000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyethylene additives, and in particular relates to an antioxidant premix for polyethylene and a preparation method thereof. Background Art
[0002] Polyethylene is a thermoplastic resin made from ethylene monomers through polymerization. It is odorless, non-toxic, chemically stable, and has good mechanical properties. It is used in all walks of life as a general plastic. According to the polymerization method, molecular weight, and chain structure, it can be divided into high-density polyethylene (HDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and ultra-high molecular weight polyethylene (UHMWPE). Each has its own strengths in function, but they are all prone to aging in light and heat environments, which leads to serious deterioration of mechanical properties. In view of the aging problem of polyethylene materials, the existing technical solutions are mainly to compound certain antioxidants into polyethylene to slow down aging. Among them, hindered amine antioxidants can effectively capture free radicals generated during the aging process and block the further oxidative damage of active groups to the polymer chain. The use of inorganic substances such as titanium dioxide and zinc white to compound and use the reflective shielding effect to reduce the depth of aging can also slow down aging.
[0003] In the plastics industry, a premix refers to a powdered or granular preparation made by uniformly mixing a functional additive with a base material. The secondary batching is performed during the production process to evenly disperse the functional additive. Therefore, the content of the functional additive in the premix is relatively high. Existing hindered amine antioxidants are not compatible with polyethylene and are difficult to disperse evenly even through premixing, resulting in limited antioxidant effects and a greater impact on the mechanical properties of the polyethylene matrix. The present application aims to provide a highly efficient antioxidant premix for polyethylene. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide an antioxidant premix for polyethylene and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An antioxidant premix for polyethylene comprises, by weight percentage, 48-55wt% of a modified antioxidant, 1.4-1.8wt% of an opening agent, 0.25-0.35wt% of a lubricant, and the remainder being LLDPE resin.
[0007] The modified antioxidant is prepared by the following method:
[0008] Step A1: Tetramethylpiperidinamine, methyl thioglycolate and anhydrous tetrahydrofuran are added and mixed, nitrogen is introduced for protection, the temperature is controlled at 0-10° C. in an ice-water bath, sodium hydride is slowly added while stirring, and the temperature is raised to 40-50° C. after the addition is complete. The total reaction time of the addition of sodium hydride is controlled to be 2.5-3.2 h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water and vacuum dried to obtain an antioxidant;
[0009] Furthermore, the dosage ratio of methyl thioglycolate, tetramethylpiperidinamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.105-0.11 mol: 0.12-0.16 g: 35-50 mL, and under the promotion of sodium hydride, tetramethylpiperidinamine and methyl thioglycolate undergo amine ester exchange.
[0010] Step A2: Add antioxidant, tetraallylsilane, benzoin dimethyl ether and dimethylacetamide and mix them evenly, raise the temperature to 65-85°C, and use UVA ultraviolet light at 240-320W / m 2 Irradiate, stir and react for 1.5-2h, then stop irradiation, add ethanol dispersion of titanium dioxide and mix, let stand for 12h, take the bottom precipitate, wash with water and vacuum dry to obtain a composite precursor;
[0011] Furthermore, the dosage ratio of the antioxidant, tetraallylsilane, benzoin dimethyl ether, dimethylacetamide and titanium dioxide is 0.1 mol: 20-25 mmol: 8-12 mg: 70-80 mL: 120-150 g, and the active thiol introduced into the antioxidant undergoes click addition with tetraallylsilane, and the sulfur, nitrogen and oxygen structures in the addition product form a chelation reaction, which is suspended and chelated and loaded onto the surface of the titanium dioxide;
[0012] Preferably, the titanium dioxide is rutile titanium dioxide, which has good ultraviolet reflection and shielding properties;
[0013] Preferably, the titanium dioxide is a submicron powder, which maintains good dispersibility and facilitates uniform loading of the addition product.
[0014] Step A3: Mix the composite precursor, triethylamine and anhydrous toluene, introduce dry nitrogen for protection, control the temperature of the reaction system in a water bath to be no higher than 20°C, add alkyl acyl chloride and stir to react for 6-8h, centrifuge to obtain the bottom precipitate after the reaction is completed, wash with ethanol and water in turn, and dry to obtain a modified antioxidant;
[0015] Furthermore, the usage ratio of the composite precursor, alkyl acyl chloride, triethylamine and anhydrous toluene is 100 g: 0.14-0.17 mol: 15-20 mL: 80-110 mL, and the alkyl acyl chloride replaces the secondary amine in the chelated organic matter on the surface of the composite precursor to reduce the basicity of the surface organic matter;
[0016] Preferably, the alkyl acid chloride has an alkyl chain length of C6-C10, good reactivity, and good compatibility and dispersibility in polyethylene.
[0017] Furthermore, the opening agent is ethylene bisoleamide.
[0018] Furthermore, the lubricant is polyethylene wax.
[0019] A method for preparing an antioxidant premix for polyethylene comprises the following steps:
[0020] Step S1: After drying the raw materials, mix them according to the weight ratio, add them into a high-speed mixer and mix them evenly to obtain a batch material;
[0021] Step S2: The compounded materials are transferred into an internal mixer, and are internally mixed at 130±5° C. until the torque is stable, and then extruded and granulated by a twin-screw extruder to obtain an antioxidant premix.
[0022] Beneficial effects of the present invention:
[0023] The antioxidant premix for polyethylene disclosed in the present invention uses linear low-density polyethylene as a dispersing material and a modified antioxidant independently developed as a functional material. It has good compatibility with a polyethylene matrix and significantly improves the anti-photooxidation performance of polyethylene. The modified antioxidant uses submicron rutile titanium dioxide as a carrier, and is prepared by amine ester exchange between tetramethylpiperidinamine and methyl thioglycolate to form a hindered amine compound with a terminal thiol group, namely, an antioxidant; then tetraallylsilane is click-added to the thiol group in the antioxidant to form an addition product with a multi-branched hindered amine structure, and the sulfur, nitrogen and oxygen structures in the molecule form a chelating effect, which is loaded onto the surface of titanium dioxide through suspended chelation. The multi-branched hindered amine has a more efficient anti-photooxidation ability, and the multi-branched sulfur, nitrogen and oxygen structures form multiple chelating sites, making the loading more stable; finally, the alkyl acyl chloride is used to replace the secondary amine in the chelated organic matter on the surface of the composite precursor to reduce the alkalinity of the surface organic matter, while at the same time The introduction of alkyl chains on the surface improves the compatibility with the polyethylene matrix. During the blending process, it can be evenly dispersed into the matrix to form a protective effect. Under light and heat conditions, the titanium dioxide in the modified antioxidant reflects light to form a shielding effect. The hindered amine on its surface captures the aging free radicals caused by the incident and reflected light, slowing down the progression of aging. The organosilicon doping introduced by the click addition of tetraallylsilane increases the refractive index disorder of the surface chelated organic layer, producing strong diffuse reflection in the near-surface layer of the modified antioxidant. Combined with the multi-hindered amine structure in the near-surface layer, the energy in the light is fully released on the surface of the material, more effectively preventing the progression of aging and allowing the material to maintain good mechanical properties during the aging process. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1, preparation of antioxidant premix, the specific implementation process is as follows:
[0026] (1) Preparation of modified antioxidant
[0027] Step A1: Tetramethylpiperidinamine, methyl thioglycolate and anhydrous tetrahydrofuran are mixed, nitrogen is introduced for protection, the temperature is controlled at 10°C in an ice-water bath, stirring is applied at 240rpm, sodium hydride is slowly added within 0.8h, and the temperature is raised to 50°C after complete addition. The total reaction time of sodium hydride addition is controlled to be 2.5h, wherein the amount ratio of methyl thioglycolate, tetramethylpiperidinamine, sodium hydride and anhydrous tetrahydrofuran is 0.1mol:0.11mol:0.12g:50mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water and vacuum dried to obtain an antioxidant.
[0028] Step A2: Take antioxidant, tetraallylsilane, benzoin dimethyl ether and dimethylacetamide, mix well, heat to 85°C, use UVA light source with an intensity of 320W / m 2 The mixture was irradiated with ultraviolet light and stirred at 90 rpm for 1.5 h, then the irradiation was stopped, titanium dioxide and ethanol were ultrasonically dispersed to prepare a dispersion with a solid content of 30%, the dispersion was added to the reaction solution, stirred and mixed at 600 rpm, and then allowed to stand for 12 h. In the implementation process, THR-218 submicron rutile titanium dioxide from Panzhihua Titanium Sea Technology Co., Ltd. was used, and the dosage ratio of antioxidant, tetraallyl silane, benzoin dimethyl ether, dimethylacetamide and titanium dioxide was 0.1 mol: 25 mmol: 8 mg: 80 mL: 150 g. After standing, the bottom precipitate was washed with water and dried in vacuo to obtain a composite precursor.
[0029] Step A3: Mix the composite precursor, triethylamine and anhydrous toluene, introduce dry nitrogen for protection, control the temperature of the reaction system to be no higher than 20°C in a water bath, add hexanoyl chloride and stir at 60rpm for 6h, wherein the amount ratio of the composite precursor, hexanoyl chloride, triethylamine and anhydrous toluene is 100g:0.17mol:20mL:110mL. After the reaction is completed, centrifuge and take the bottom precipitate, wash it with ethanol and water in turn, and dry it to obtain a modified antioxidant.
[0030] (2) Preparation of antioxidant premix
[0031] Step S1: drying the raw materials required for the implementation, and mixing them according to weight percentage: 55wt% of modified antioxidant, which is self-made in this embodiment; 1.4wt% of opening agent, which uses industrial-grade ethylene bisoleamide provided by Guangzhou Qiansan Chemical Technology Co., Ltd. during the implementation; 0.35wt% of lubricant, which uses H100P polyethylene wax from Qingdao Haihao Chemical Co., Ltd. during the implementation; 43.25wt% of LLDPE resin, which uses DFDA-7042 resin from Dushanzi Petrochemical Company of China Petroleum during the implementation; adding each raw material into a high-speed mixer and mixing at 1200rpm for 15min to obtain a batch.
[0032] Step S2: The compounded materials are transferred into an internal mixer, and are internally mixed at 130±5° C. until the torque is stable, and then extruded and granulated by a twin-screw extruder to obtain an antioxidant premix.
[0033] Example 2, preparation of antioxidant premix, the specific implementation process is as follows:
[0034] (1) Preparation of modified antioxidant
[0035] Step A1: Tetramethylpiperidinamine, methyl thioglycolate and anhydrous tetrahydrofuran are mixed, nitrogen is introduced for protection, the temperature is controlled at 0°C in an ice-water bath, stirring is applied at 180 rpm, sodium hydride is slowly added within 1.2 hours, and the temperature is raised to 40°C after complete addition. The total reaction time of sodium hydride addition is controlled to be 3.2 hours, wherein the amount ratio of methyl thioglycolate, tetramethylpiperidinamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.105 mol: 0.16 g: 35 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water and vacuum dried to obtain an antioxidant.
[0036] Step A2: Take antioxidant, tetraallylsilane, benzoin dimethyl ether and dimethylacetamide, mix well, heat to 65°C, use UVA light source with an intensity of 240W / m 2 The mixture was irradiated with ultraviolet light and stirred at 60 rpm for 2 hours, then the irradiation was stopped, titanium dioxide (THR-218) and ethanol were ultrasonically dispersed to prepare a dispersion with a solid content of 30%, the dispersion was added to the reaction solution, stirred and mixed at 600 rpm, and then allowed to stand for 12 hours, wherein the amount ratio of antioxidant, tetraallylsilane, benzoin dimethyl ether, dimethylacetamide and titanium dioxide was 0.1 mol: 20 mmol: 12 mg: 70 mL: 120 g, and after standing, the bottom precipitate was washed with water and dried in vacuo to obtain a composite precursor.
[0037] Step A3: Mix the composite precursor, triethylamine and anhydrous toluene, introduce dry nitrogen for protection, control the temperature of the reaction system to be no higher than 20°C in a water bath, add octanoyl chloride and stir to react for 8 hours, wherein the amount ratio of the composite precursor, octanoyl chloride, triethylamine and anhydrous toluene is 100g:0.14mol:15mL:80mL. After the reaction is completed, centrifuge and take the bottom precipitate, wash it with ethanol and water in turn, and dry it to obtain a modified antioxidant.
[0038] (2) Preparation of antioxidant premix
[0039] Step S1: drying the raw materials required for the implementation, and mixing them according to weight percentage: 48wt% of modified antioxidant, which is prepared in this embodiment; 1.8wt% of anti-blocking agent, 0.25wt% of lubricant and 49.95wt% of LLDPE resin; adding the raw materials into a high-speed mixer and mixing at 1200rpm for 15min to obtain a batch.
[0040] Step S2: The compounded materials are transferred into an internal mixer, and are internally mixed at 130±5° C. until the torque is stable, and then extruded and granulated by a twin-screw extruder to obtain an antioxidant premix.
[0041] Example 3, preparation of antioxidant premix, the specific implementation process is as follows:
[0042] (1) Preparation of modified antioxidant
[0043] Step A1: Tetramethylpiperidinamine, methyl thioglycolate and anhydrous tetrahydrofuran are mixed, nitrogen is introduced for protection, the temperature is controlled at 5°C with an ice-water bath, stirring is applied at 240rpm, sodium hydride is slowly added within 1.1 hours, and the temperature is raised to 45°C after complete addition. The total reaction time of sodium hydride addition is controlled to be 3 hours, wherein the amount ratio of methyl thioglycolate, tetramethylpiperidinamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.108 mol: 0.14 g: 45 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water and vacuum dried to obtain an antioxidant.
[0044] Step A2: Take antioxidant, tetraallylsilane, benzoin dimethyl ether and dimethylacetamide, mix well, heat to 78°C, use UVA light source with an intensity of 320W / m 2 The mixture was irradiated with ultraviolet light and stirred at 90 rpm for 1.8 h, then the irradiation was stopped, titanium dioxide (THR-218) and ethanol were ultrasonically dispersed to prepare a dispersion with a solid content of 30%, the dispersion was added to the reaction solution, stirred and mixed at 600 rpm, and then allowed to stand for 12 h, wherein the amount ratio of antioxidant, tetraallylsilane, benzoin dimethyl ether, dimethylacetamide and titanium dioxide was 0.1 mol: 22 mmol: 10 mg: 80 mL: 135 g, and after standing, the bottom precipitate was washed with water and dried in vacuo to obtain a composite precursor.
[0045] Step A3: Take a composite precursor, triethylamine and anhydrous toluene, mix them, introduce dry nitrogen for protection, control the temperature of the reaction system to be no higher than 20°C in a water bath, add octanoyl chloride and stir to react for 8 hours, wherein the amount ratio of the composite precursor, octanoyl chloride, triethylamine and anhydrous toluene is 100g:0.15mol:18mL:100mL. After the reaction is completed, centrifuge and take the bottom precipitate, wash it with ethanol and water in turn, and dry it to obtain a modified antioxidant.
[0046] (2) Preparation of antioxidant premix
[0047] Step S1: drying the raw materials required for the implementation, and mixing them according to weight percentage: 52wt% of modified antioxidant, which is prepared in this embodiment; 1.5wt% of anti-blocking agent, 0.32wt% of lubricant and 46.18wt% of LLDPE resin; adding each raw material into a high-speed mixer and mixing at 1200rpm for 15min to obtain a batch.
[0048] Step S2: The compounded materials are transferred into an internal mixer, and are internally mixed at 130±5° C. until the torque is stable, and then extruded and granulated by a twin-screw extruder to obtain an antioxidant premix.
[0049] In the comparative example, light stabilizer 944 and light stabilizer 531 were used to prepare the antioxidant premix, specifically:
[0050] The ingredients are prepared according to weight percentage: 94418wt% of light stabilizer and 5319wt% of light stabilizer, both of which are industrial-grade raw materials; 25wt% of oleophilic titanium dioxide, NT-014B type raw material of Jiangsu Hehai Nano Technology Co., Ltd.; 1.7wt% of anti-blocking agent; 0.3wt% of lubricant and 46wt% of LLDPE resin; the raw materials are added into a high-speed mixer and mixed at a high speed of 1200rpm for 15 minutes to obtain a compound material.
[0051] Step S2: The compounded materials are transferred into an internal mixer, and are internally mixed at 130±5° C. until the torque is stable, and then extruded and granulated by a twin-screw extruder to obtain an antioxidant premix.
[0052] In order to verify the antioxidant effect of the antioxidant premix obtained above on polyethylene, HD-6081 high-density polyethylene and LL0220AA linear low-density polyethylene were compounded in a mass ratio of 5:1 as a masterbatch, 2.5% of the antioxidant premix was added to the masterbatch, and granulated by extrusion using a twin-screw extruder, and then hot-pressed into sheets using a flat vulcanizer, wherein the molding temperature was 180°C and the molding pressure was 10MPa;
[0053] Take samples from the above sheets and perform tensile performance test according to GB / T 1040.2-2022 standard, and perform impact performance test according to GB / T1843-2008 standard;
[0054] Take the samples from the same batch, place them in an aging box, control the temperature at 60℃, use a 500W fluorescent lamp at a distance of 1m from the sample for continuous irradiation, simulate the strong sunlight environment to accelerate aging, the test cycle is 720h, and test the tensile properties and impact properties again, and compare the test data with the initial data to calculate the change rate. The specific test results are shown in the following table:
[0055]
[0056] It can be seen from the test data in the above table that the antioxidant premix obtained in the example has little effect on the mechanical properties of the polyethylene matrix when compounded in the polyethylene matrix, and the mechanical properties decrease even less after aging, showing a stable anti-photooxidation effect.
[0057] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0058] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An antioxidant premix for polyethylene, characterized in that: The composition comprises, by weight percentage, 48-55 wt % of a modified antioxidant, 1.4-1.8 wt % of an anti-blocking agent, 0.25-0.35 wt % of a lubricant, and the balance being LLDPE resin; The modified antioxidant is prepared by the following method: Step A1: Tetramethylpiperidinamine, methyl thioglycolate and anhydrous tetrahydrofuran are added and mixed, nitrogen is introduced for protection, the temperature is controlled at 0-10° C. in an ice-water bath, sodium hydride is slowly added while stirring, and the temperature is raised to 40-50° C. after the addition is complete. The total reaction time of the addition of sodium hydride is controlled to be 2.5-3.2 h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water and vacuum dried to obtain an antioxidant; Step A2: Add antioxidant, tetraallylsilane, benzoin dimethyl ether and dimethylacetamide and mix them evenly, raise the temperature to 65-85°C, and use UVA ultraviolet light at 240-320W / m 2 Irradiate, stir and react for 1.5-2h, then stop irradiation, add ethanol dispersion of titanium dioxide and mix, let stand for 12h, take the bottom precipitate, wash with water and vacuum dry to obtain a composite precursor; Step A3: Mix the composite precursor, triethylamine and anhydrous toluene, introduce dry nitrogen for protection, control the temperature of the reaction system to be no higher than 20°C in a water bath, add alkyl acyl chloride and stir to react for 6-8h, after the reaction is completed, centrifuge to obtain the bottom precipitate, wash it with ethanol and water in turn, and dry it to obtain a modified antioxidant.
2. The antioxidant premix for polyethylene according to claim 1, characterized in that: The usage ratio of methyl thioglycolate, tetramethylpiperidinamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.105-0.11 mol: 0.12-0.16 g: 35-50 mL.
3. The antioxidant premix for polyethylene according to claim 2, characterized in that: The dosage ratio of the antioxidant, tetraallylsilane, benzoin dimethyl ether, dimethylacetamide and titanium dioxide is 0.1 mol: 20-25 mmol: 8-12 mg: 70-80 mL: 120-150 g.
4. The antioxidant premix for polyethylene according to claim 3, characterized in that: Titanium dioxide is rutile titanium dioxide.
5. The antioxidant premix for polyethylene according to claim 4, characterized in that: Titanium dioxide is a submicron powder.
6. The antioxidant premix for polyethylene according to claim 5, characterized in that: The usage ratio of the composite precursor, alkyl acyl chloride, triethylamine and anhydrous toluene is 100 g: 0.14-0.17 mol: 15-20 mL: 80-110 mL.
7. An antioxidant premix for polyethylene according to claim 6, characterized in that: The alkyl chain length of the alkyl acid chloride is C6-C10.
8. The antioxidant premix for polyethylene according to claim 1, characterized in that: The opening agent is ethylene bisoleamide.
9. The antioxidant premix for polyethylene according to claim 1, characterized in that: The lubricant is polyethylene wax.
10. The method for preparing an antioxidant premix for polyethylene according to any one of claims 1 to 9, characterized in that: The steps include: Step S1: After drying the raw materials, mix them according to the weight ratio, add them into a high-speed mixer and mix them evenly to obtain a batch material; Step S2: The compounded materials are transferred into an internal mixer, and are internally mixed at 130±5° C. until the torque is stable, and then extruded and granulated by a twin-screw extruder to obtain an antioxidant premix.