A method for controlling carbon in cemented carbide mixture
Through liquid-solid mixing and ball milling, combined with raw material and process control, the problem of uneven carbon content in cemented carbide is solved, and precise carbon content control and performance improvement of cemented carbide are achieved.
Patent Information
- Application Number
- CN202411115046.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-14
AI Technical Summary
In the existing cemented carbide production, the carbon content is not accurately controlled, resulting in uneven hardness and wear resistance. The post-processing method is complex and costly, making it difficult to control accurately.
The carbon slurry is prepared using a liquid-solid mixing method. Through ball milling and carbonization treatment, combined with the carbon amount control of the raw material WC and the carbon amount control of the mixture preparation process, the carbon slurry is used to supplement the carbon slurry to achieve precise control of the carbon uniformity and performance of the cemented carbide. .
It improves the uniformity of carbon distribution of WC in cemented carbide, simplifies the production process, reduces costs, achieves precise control of the carbon content of cemented carbide, and improves product quality and performance consistency.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a carbon control method for a cemented carbide mixture. Background Art
[0002] Cemented carbide is a material with high wear resistance and high toughness, which is widely used in cutting tools, wear-resistant parts and special application fields. As a key parameter of cemented carbide, carbon content plays a vital role in its performance. Carbon content can directly affect the hardness and wear resistance of cemented carbide products. The presence of carbon can refine the hard phase and enhance the bonding force between hard particles, thereby improving the wear resistance of the alloy. In the production process of cemented carbide, there are two main ways to control the carbon content. One is to control the carbon content of raw materials. Select appropriate raw materials to control the carbon content. This method is affected by the uniformity of raw material carbon distribution and the uncertainty of powder oxygenation in the process, which will lead to the problem of inaccurate control of carbon content in cemented carbide production; the other is to control the carbon content through post-processing. The carbon content is controlled by post-processing (heat treatment) of the product and controlling the temperature and time. The post-processing method is complicated, has poor feasibility, cannot accurately control the carbon content, and is too expensive, which is not conducive to cost control.
[0003] The control of the carbon content of cemented carbide mainly involves the carbon content control of the raw material WC and the carbon content control in the mixture preparation process. The appropriate carbon range is found in the early stage, the appropriate carbon point is determined, and then the appropriate and stable raw materials are selected to prepare the mixture. However, there will be carbon black aggregation in the carbon blending of WC raw materials and the carbon control in the mixture preparation process. At present, W powder carbon blending mainly involves mixing W powder and carbon black in a plow mixer. This method uses a solid-solid mixing method. The density of W powder and carbon black is quite different, which will lead to uneven mixing and uneven total carbon of the raw materials, affecting the back-end use. The addition of carbon black during the preparation of the mixture will cause the prepared alloy Com to be uneven and the performance to be unqualified due to the low density of carbon black, which is easy to float on the liquid surface and the wall of the ball mill, making it difficult to achieve the expected effect. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a carbon control method for a cemented carbide mixture.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A method for controlling carbon in a cemented carbide mixture comprises the following steps:
[0007] S1. Prepare a carbon slurry, wherein the carbon black content of the carbon slurry is 20-35wt% and the viscosity is 20-30MPa·s;
[0008] S2, ball-milling the tungsten powder and the carbon slurry together, and then carbonizing to obtain a WC raw material with uniform carbon content;
[0009] S3. Prepare cemented carbide mixture according to the requirements of cemented carbide composition. Do not add oleic acid and paraffin wax for ball milling in the early stage. Stop the machine after 15-18 hours of ball milling to take the slurry, then add oleic acid and paraffin wax. After vacuum drying the slurry, test it. Add carbon slurry according to the test results, continue ball milling, and then spray to obtain the cemented carbide mixture.
[0010] As a preferred embodiment of the carbon control method of a cemented carbide mixture described in the present invention, wherein: in the step S1, by weight, 20-30 parts of carbon black, 3-5 parts of dispersant, 2-4 parts of binder, and 0.1-0.2 parts of defoamer are taken, and water is added to make up 100 parts; the dispersant is first slowly added to 60-70 parts of water and stirred to obtain solution A; the binder is added to the remaining amount of water, stirred and the defoamer is added until dissolved to obtain solution B; the carbon black and solution A are added to a planetary ball mill with a ball-to-material ratio of (2-5):1, ball milled for 3-5 hours, and then solution B is added, and then ball milled for 3-5 hours to obtain carbon slurry.
[0011] As a preferred embodiment of the carbon control method for a cemented carbide mixture described in the present invention, in step S1, the dispersant is sodium hexametaphosphate, the adhesive is PEG4000, and the defoaming agent is water-soluble acrylic acid.
[0012] As a preferred embodiment of the carbon control method of a cemented carbide mixture described in the present invention, wherein: in the step S2, the amount of carbon slurry added is determined according to the required amount of carbon black added and the carbon black content of the carbon slurry, and the amount of carbon black added is determined according to the following formula:
[0013] Qc=(Ct / (100-Ct)+(0.75×O) / 100)×Qw
[0014] Where Qc is the amount of carbon black added, Ct is the total carbon content of the WC raw material, O is the oxygen content in the tungsten powder, and Qw is the weight of the tungsten powder.
[0015] As a preferred embodiment of the carbon control method of a cemented carbide mixture described in the present invention, wherein: in the step S2, the ball-to-material ratio during ball milling is (1.5-2.5):1, alcohol is added during ball milling, and the liquid-to-solid ratio of alcohol to tungsten powder is (0.25-0.35):1.
[0016] As a preferred embodiment of the carbon control method for a cemented carbide mixture described in the present invention, wherein: in the step S2, the ball milling speed is 110-130 r / min, and the time is 1.5-2.5 h.
[0017] As a preferred embodiment of the carbon control method of a cemented carbide mixture described in the present invention, in which: in the step S3, the total carbon is detected after the slurry is vacuum dried, and carbon slurry is added according to the difference between the total carbon detection result and the cemented carbide component requirements, ball milling is continued, and then the cemented carbide mixture is obtained by spraying.
[0018] As a preferred embodiment of the carbon control method of a cemented carbide mixture described in the present invention, wherein: in the step S3, the slurry is vacuum dried and then pressed and sintered to prepare cemented carbide blocks / bars, and performance testing is performed. The level of carbon control of the cemented carbide mixture is reflected by the cemented carbide performance, and carbon slurry is added according to the performance results, ball milling is continued, and then the cemented carbide mixture is obtained by spraying.
[0019] As a preferred embodiment of the carbon control method for a cemented carbide mixture described in the present invention, wherein: in the step S3, the ball milling is continued for 2 to 4 hours.
[0020] The beneficial effects of the present invention are as follows:
[0021] The present invention proposes a method for controlling carbon in cemented carbide mixtures. When tungsten powder is mixed with carbon, a liquid-solid mixing method is adopted, which can improve the uniformity of material mixing, reduce the agglomeration of carbon black, and make the prepared WC carbon distribution uniform, thereby improving the total carbon uniformity of WC; by adding carbon slurry, the dispersion efficiency and success of carbon supplementation in the mixture preparation process can be improved, and the problems of low carbon black density and long carbon black dispersion time that affect the total carbon uniformity of the mixture and the quality of cemented carbide can be reduced. The method of the present invention controls the carbon amount of the raw material WC and the carbon amount of the mixture preparation process. The combination of the two can achieve accurate control of the carbon amount of cemented carbide. The method has a simple process and high controllability, which is conducive to the quality control of cemented carbide. DETAILED DESCRIPTION
[0022] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] According to one aspect of the present invention, the present invention provides the following technical solution:
[0024] A method for controlling carbon in a cemented carbide mixture comprises the following steps:
[0025] S1. Prepare a carbon slurry, wherein the carbon black content of the carbon slurry is 20-35wt% and the viscosity is 20-30MPa·s;
[0026] S2, ball-milling the tungsten powder and the carbon slurry together, and then carbonizing to obtain a WC raw material with uniform carbon content;
[0027] S3. Prepare cemented carbide mixture according to the requirements of cemented carbide composition. Do not add oleic acid and paraffin wax for ball milling in the early stage. Stop the machine after 15-18 hours of ball milling to take the slurry, then add oleic acid and paraffin wax. After vacuum drying the slurry, test it. Add carbon slurry according to the test results, continue ball milling, and then spray to obtain the cemented carbide mixture.
[0028] Preferably, in step S1, 20-30 parts of carbon black, 3-5 parts of dispersant, 2-4 parts of binder, and 0.1-0.2 parts of defoamer are taken in parts by weight, and water is added to make up to 100 parts; the dispersant is first slowly added to 60-70 parts of water and stirred to obtain solution A; the binder is added to the remaining amount of water, stirred and the defoamer is added until dissolved to obtain solution B; the carbon black and solution A are added to a planetary ball mill with a ball-to-material ratio of (2-5):1, ball milled for 3-5 hours, and then solution B is added, and then ball milled for 3-5 hours to obtain carbon slurry.
[0029] Preferably, in step S1, the dispersant is sodium hexametaphosphate, the adhesive is PEG4000, and the defoaming agent is water-soluble acrylic acid.
[0030] Preferably, in step S2, the amount of carbon slurry added is determined according to the required amount of carbon black added and the carbon black content of the carbon slurry, and the amount of carbon black added is determined according to the following formula:
[0031] Qc=(Ct / (100-Ct)+(0.75×O) / 100)×Qw
[0032] Where Qc is the amount of carbon black added, Ct is the total carbon content of the WC raw material, O is the oxygen content in the tungsten powder, and Qw is the weight of the tungsten powder.
[0033] Preferably, in step S2, the ball-to-material ratio during ball milling is (1.5-2.5):1, alcohol is added during ball milling, and the liquid-to-solid ratio of alcohol to tungsten powder is (0.25-0.35):1.
[0034] Preferably, in step S2, the ball milling speed is 110-130 r / min, and the time is 1.5-2.5 h.
[0035] Preferably, in step S3, paraffin and oleic acid will crack at high temperature to form carbon, which will affect the result of carbon measurement in the cemented carbide mixture process. In order to ensure the accuracy of the test result, oleic acid and paraffin are not added in the early stage, and oleic acid and paraffin are added after the slurry is taken.
[0036] Preferably, in step S3, after the slurry is vacuum dried, a total carbon test is performed, and carbon slurry is added according to the difference between the total carbon test result and the cemented carbide component requirements, and ball milling is continued, and then the cemented carbide mixture is obtained by spraying.
[0037] Preferably, in step S3, the slurry is vacuum dried and then pressed and sintered to prepare cemented carbide blocks / bars, and performance testing is performed. The level of carbon control in the cemented carbide mixture is reflected by the cemented carbide performance. Carbon slurry is added according to the performance results, ball milling is continued, and then the cemented carbide mixture is obtained by spraying.
[0038] Preferably, in step S3, the ball milling is continued for 2 to 4 hours.
[0039] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0040] Example 1
[0041] A method for controlling carbon in a cemented carbide mixture comprises the following steps:
[0042] S1. In parts by weight, take 30 parts of carbon black, 5 parts of dispersant, 3 parts of binder, 0.2 parts of defoamer, and add water to make up to 100 parts; first slowly add the dispersant to 60 parts of water and stir to obtain solution A; add the binder to the remaining amount of water, stir and add the defoamer until it dissolves to obtain solution B; add the carbon black and solution A to a planetary ball mill with a ball-to-material ratio of 5:1, ball mill for 4 hours, then add solution B, and then ball mill for 4 hours to obtain a carbon slurry, wherein the dispersant is sodium hexametaphosphate, the binder is PEG4000, the defoamer is water-soluble acrylic acid, and the carbon black content of the carbon slurry is 30wt% and the viscosity is 28MPa·s;
[0043] S2. Ball mill the tungsten powder and carbon slurry together. The amount of carbon slurry added is determined according to the required amount of carbon black added and the carbon black content of the carbon slurry. The amount of carbon black added is determined according to the carbon point of WC being 6.12wt%. The ball-to-material ratio during ball milling is 2:1. Alcohol is added during ball milling, and the liquid-solid ratio of alcohol to tungsten powder is 0.3:1. The ball milling speed is 120r / min, and the time is 2h. Three samples after ball milling at different positions are taken for inspection of total carbon, which are 6.08wt% / 6.11wt% / 6.09wt% respectively. Then they are sent to a molybdenum wire furnace for carbonization to obtain WC raw materials with uniform carbon content.
[0044] S3. According to the requirements of cemented carbide composition (WC-6Co%-Cr3C2 grade was selected), a cemented carbide mixture with a total carbon content of 5.81wt% was prepared. No oleic acid and paraffin were added during ball milling in the early stage. After 16 hours of ball milling, the machine was stopped to take the slurry, and then oleic acid and paraffin were added. The slurry was vacuum dried and then tested for total carbon. Two samples were taken from different positions, and the total carbon contents were 5.79wt% / 5.80wt% respectively. The amount of carbon slurry added was converted based on the result difference of 0.015wt% of total carbon. The machine was stopped to add carbon slurry, and ball milling was continued for 3 hours. The cemented carbide mixture was then obtained by spraying.
[0045] The cemented carbide mixture prepared in this embodiment was used to press the sample strips, which were sintered in the furnace to obtain cemented carbide. Three points were randomly selected and the cobalt magnetic Com was detected to be 5.3% / 5.2% / 5.3%, and the HV20 was 1905 / 1910 / 1908, respectively, achieving the expected effect and the cobalt magnetic uniformity.
[0046] Example 2
[0047] A method for controlling carbon in a cemented carbide mixture comprises the following steps:
[0048] S1. In parts by weight, take 20 parts of carbon black, 3 parts of dispersant, 3 parts of binder, 0.1 parts of defoamer, and add water to make up to 100 parts; first slowly add the dispersant to 70 parts of water and stir to obtain solution A; add the binder to the remaining amount of water, stir and add the defoamer until it dissolves to obtain solution B; add the carbon black and solution A to a planetary ball mill with a ball-to-material ratio of 5:1, ball mill for 4 hours, then add solution B, and then ball mill for 4 hours to obtain a carbon slurry, wherein the dispersant is sodium hexametaphosphate, the binder is PEG4000, the defoamer is water-soluble acrylic acid, and the carbon black content of the carbon slurry is 20wt% and the viscosity is 20MPa·s;
[0049] S2. Ball mill the tungsten powder and carbon slurry together. The amount of carbon slurry added is determined according to the required amount of carbon black added and the carbon black content of the carbon slurry. The amount of carbon black added is determined according to the carbon content of WC being 6.12wt%. The ball-to-material ratio during ball milling is 2:1. Alcohol is added during ball milling, and the liquid-solid ratio of alcohol to tungsten powder is 0.3:1. The ball milling speed is 120r / min, and the time is 2h. Three samples after ball milling at different positions are taken for inspection of total carbon, which are 6.12wt% / 6.10wt% / 6.11wt% respectively. Then they are sent to a molybdenum wire furnace for carbonization to obtain WC raw materials with uniform carbon content.
[0050] S3. According to the requirements of cemented carbide composition (select WC-6Co%-Cr3C2 grade), prepare a cemented carbide mixture with a total carbon content of 5.81wt%. Do not add oleic acid and paraffin wax in the early stage of ball milling. Stop the machine after 16 hours of ball milling to take the slurry, then add oleic acid and paraffin wax. After vacuum drying, press and sinter the slurry to prepare cemented carbide blocks / bars. Perform performance testing. The cobalt magnetic Com is 5.0% / 4.9% / 5.1% respectively. According to experience, 0.01wt% of carbon needs to be added. Continue ball milling for 3 hours, and then spray to obtain the cemented carbide mixture.
[0051] The cemented carbide mixture prepared in this embodiment was used to press the sample strips, which were sintered in the furnace to obtain cemented carbide. Three points were randomly selected and the cobalt magnetic Com was detected to be 5.3% / 5.1% / 5.3%, and the HV20 was 1915 / 1910 / 1912, respectively, achieving the expected effect and the cobalt magnetic uniformity.
[0052] Comparative Example 1
[0053] A method for preparing a cemented carbide mixture comprises the following steps:
[0054] S1. Ball mill tungsten powder and carbon black together. The amount of carbon black added is determined according to the carbon content of WC being 6.12wt%. The ball-to-material ratio during ball milling is 2:1. Alcohol is added during ball milling. The liquid-solid ratio of alcohol to tungsten powder is 0.3:1. The ball milling speed is 120r / min for 2h. Three samples after ball milling at different positions are taken for inspection of total carbon, which are 5.78wt% / 6.11wt% / 6.32wt% respectively. Then they are sent to a molybdenum wire furnace for carbonization to obtain WC raw material.
[0055] S2. According to the requirements of cemented carbide composition (WC-6Co%-Cr3C2 grade was selected), a cemented carbide mixture with a total carbon content of 5.81wt% was prepared. No oleic acid and paraffin were added during ball milling in the early stage. After 16 hours of ball milling, the machine was stopped to take the slurry, and then oleic acid and paraffin were added. The slurry was vacuum dried and then the total carbon was tested. Two samples were taken from different positions, and the total carbon content was 5.78wt% / 5.89wt% respectively. According to the result difference of 0.03wt% of total carbon, the machine was stopped to add carbon black, and the ball milling was continued for 3 hours. After that, the cemented carbide mixture was obtained by spraying.
[0056] The cemented carbide mixture prepared in this comparative example was used to press the sample strips, and the cemented carbide was sintered in the furnace. Three points were randomly selected, and the cobalt magnetic Com was detected to be 5.4% / 5.5% / 5.7%, and the HV20 was 1889 / 1901 / 1873, respectively. Since the total carbon of the raw material WC is unstable, it is difficult to control the carbon content of the alloy and the alloy performance is unstable.
[0057] Comparative Example 2
[0058] The difference from Example 1 is that, in step S3, according to the requirements of the composition of cemented carbide (WC-6Co%-Cr3C2 grade is selected), a cemented carbide mixture with a total carbon content of 5.81wt% is prepared, and oleic acid and paraffin are not added in the early stage for ball milling. After 16 hours of ball milling, the machine is stopped to take the slurry, and then oleic acid and paraffin are added. The slurry is vacuum dried and pressed and sintered to prepare cemented carbide blocks / bars, and performance tests are carried out. The cobalt magnetic Com is detected to be 5.0% / 4.9% / 5.1% respectively. According to production experience, 0.01wt% of carbon needs to be added, and carbon black is added to continue ball milling for 8 hours, and then the cemented carbide mixture is sprayed.
[0059] The cemented carbide mixture prepared in this comparative example was used to press the sample strips, and the cemented carbide was sintered in the furnace. Three points were randomly selected and the cobalt magnetic Com was detected to be 5.0% / 4.8% / 5.1%, and the HV20 was 1932 / 1929 / 1926, respectively. The cobalt magnetic was uneven and the carbon control effect was poor.
[0060] Comparative Example 3
[0061] The difference from Example 1 is that in step S1, 50 parts of carbon black, 5 parts of dispersant, 4 parts of binder, and 0.1 parts of defoamer are taken in parts by weight, and water is added to make up 100 parts; the dispersant is sodium hexametaphosphate, the binder is PEG4000, and the defoamer is water-soluble acrylic acid; the dispersant is first slowly added to 40 parts of water and stirred to obtain solution A; the binder is added to the remaining amount of water, stirred and the defoamer is added until dissolved to obtain solution B; the carbon black and solution A are added to a planetary ball mill with a ball-to-material ratio of 5:1, ball milled for 4 hours, the slurry is relatively thick, and then solution B is added, and then ball milled for 4 hours. The slurry has more carbon black agglomerated together, and the dispersion effect is poor. The carbon black content of the carbon slurry is 50wt%, which cannot be measured by a viscometer.
[0062] It can be seen from the above embodiments and comparative examples that the liquid-solid mixing method is used when the tungsten powder of the present invention is mixed with carbon, which can improve the uniformity of material mixing, reduce the agglomeration of carbon black, and make the prepared WC carbon distribution uniform, thereby improving the total carbon uniformity of WC; the addition of carbon slurry can improve the dispersion efficiency and success of carbon supplementation in the mixture preparation process, and reduce the problems of low carbon black density and long carbon black dispersion time that affect the total carbon uniformity of the mixture and the quality of cemented carbide. The method of the present invention controls the carbon amount of the raw material WC and the carbon amount of the mixture preparation process. The combination of the two can achieve accurate control of the carbon amount of cemented carbide. The method has a simple process and high controllability, which is conducive to the quality control of cemented carbide.
[0063] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for controlling carbon in a cemented carbide mixture, characterized in that: The steps include: S1. Prepare a carbon slurry, wherein the carbon black content of the carbon slurry is 20-35wt% and the viscosity is 20-30MPa·s; S2, ball-milling the tungsten powder and the carbon slurry together, and then carbonizing to obtain a WC raw material with uniform carbon content; S3. Prepare cemented carbide mixture according to the requirements of cemented carbide composition. Do not add oleic acid and paraffin wax for ball milling in the early stage. Stop the machine after 15-18 hours of ball milling to take the slurry, then add oleic acid and paraffin wax. After vacuum drying the slurry, test it. Add carbon slurry according to the test results, continue ball milling, and then spray to obtain the cemented carbide mixture.
2. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In the step S1, 20-30 parts of carbon black, 3-5 parts of dispersant, 2-4 parts of binder, and 0.1-0.2 parts of defoamer are taken in parts by weight, and water is added to make up to 100 parts; the dispersant is first slowly added to 60-70 parts of water and stirred to obtain solution A; the binder is added to the remaining amount of water and stirred and the defoamer is added until dissolved to obtain solution B; the carbon black and solution A are added to a planetary ball mill with a ball-to-material ratio of (2-5):1, ball milled for 3-5 hours, and then solution B is added, and then ball milled for 3-5 hours to obtain carbon slurry.
3. The carbon control method of cemented carbide mixture according to claim 2, characterized in that: In the step S1, the dispersant is sodium hexametaphosphate, the adhesive is PEG4000, and the defoaming agent is water-soluble acrylic acid.
4. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In step S2, the amount of carbon slurry added is determined according to the required amount of carbon black added and the carbon black content of the carbon slurry, and the amount of carbon black added is determined according to the following formula: Qc=(Ct / (100-Ct)+(0.75×O) / 100)×Qw Where Qc is the amount of carbon black added, Ct is the total carbon content of the WC raw material, O is the oxygen content in the tungsten powder, and Qw is the weight of the tungsten powder.
5. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In step S2, the ball-to-material ratio during ball milling is (1.5-2.5):1, alcohol is added during ball milling, and the liquid-to-solid ratio of alcohol to tungsten powder is (0.25-0.35):
1.
6. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In step S2, the ball milling speed is 110-130 r / min, and the time is 1.5-2.5 h.
7. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In step S3, the slurry is vacuum dried and then subjected to total carbon detection. Carbon slurry is added according to the difference between the total carbon detection result and the cemented carbide component requirements, ball milling is continued, and then the cemented carbide mixture is obtained by spraying.
8. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In step S3, the slurry is vacuum dried and then pressed and sintered to prepare cemented carbide blocks / bars, and performance testing is performed. The cemented carbide performance reflects the level of carbon control in the cemented carbide mixture. Carbon slurry is added according to the performance results, ball milling is continued, and then the cemented carbide mixture is sprayed.
9. The method for controlling carbon in a cemented carbide mixture according to claim 1, characterized in that: In step S3, the ball milling is continued for 2 to 4 hours.
Citation Information
Patent Citations
Preparation method for cemented carbide mixture
CN101514405A
Carbon control methods in cemented carbide paraffin processing
CN102296197A