Pure titanium sputtering target with specific texture and preparation method thereof

By forging and rolling pure titanium materials, the tightest packed surface texture is formed, which solves the problem of many particles in the sputtering process of titanium targets, improves the uniformity of the coating and the film formation speed, and is suitable for High precision semiconductor devices.

CN118621280BActive Publication Date: 2024-11-12XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111421.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing titanium targets have more particles during the sputtering process, which makes it difficult to meet the requirements of precision and miniaturization of semiconductor devices, and lacks methods to control surface texture.

Method used

By forging, heating, and rolling pure titanium ingots, the single-pass processing rate of each roll is controlled, the tightest packed surface texture is formed, the proportion of rough planes is reduced, and the ratio of surface to surface is ensured is ensured. Above 19.

Benefits of technology

It achieves a small and uniform grain distribution, reduces particle generation, improves the uniformity of sputtering coating and film formation speed, and is suitable for integrated circuits, industrial glass and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621280B_ABST
    Figure CN118621280B_ABST
Patent Text Reader

Abstract

The present invention discloses a pure titanium sputtering target with a specific texture, wherein the most densely packed surface of the target is planar textured, and the proportion of the rough surface is reduced, and the ratio of the most densely packed surface to the rough surface is above 19. The present invention also discloses a method for preparing the above target, which adopts a specific rolling process, and the single pass processing rates of each pass cooperate with each other and work together to achieve the best effect. The method of the present invention can obtain small and uniform grains, which can reduce the generation of particles and improve the uniformity of sputtering coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and relates to a pure titanium sputtering target material with a specific texture. The invention also relates to a preparation method of the target material. Background Art

[0002] Target materials are often used for sputtering film formation. The specific film formation principle is: in an inert gas atmosphere, a high voltage electric field is applied between the substrate and the target material. At this time, the inert gas is excited to form a plasma. The positively charged ions in the plasma will bombard the surface of the target material (cathode), causing the atoms on the surface of the target material to fall off and then deposit on the surface of the substrate to form a coating. During the sputtering film formation process, large particles will be generated on the surface of the target material due to the bombardment of the plasma. After these larger particles fall off, they will be embedded in the coating, thereby affecting the performance of the coating. With the sophistication and miniaturization of semiconductor devices, the requirements for the uniformity of the coating composition are getting higher and higher, which puts higher requirements on sputtering targets.

[0003] One factor that causes particles to form on the target surface is the grain size. Comparatively speaking, a smaller grain size has a higher deposition rate. The grain boundary is a relatively fragile area, and particles are easily generated during bombardment. Evenly and continuously distributed grains have lower discontinuities at their grain boundaries, and are less likely to generate particles.

[0004] Another important factor in the generation of particles on the target surface is grain orientation, that is, the grains have a specific orientation relative to the reference plane, also known as texture. Crystal surface, The crystal plane is parallel to the rolling direction, that is, , Surface texture.

[0005] The most densely packed surface. Targets with a high texture ratio are less likely to produce particles, and the deposited coating has better uniformity; The target material with a high proportion of rough surface is more likely to produce particles, and the uniformity of the deposited coating is poor. However, there is no public control method in the prior art. , The surface texturing method results in more particles in the titanium target during the sputtering process, and the uniformity of the film is difficult to meet the requirements of precision and miniaturization of semiconductor devices. Summary of the invention

[0006] The purpose of the present invention is to provide a pure titanium sputtering target with a specific texture, having the most densely packed surface Textured and rough surface The characteristics of small proportion, Surface and The ratio of the surface is above 19.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned pure titanium sputtering target.

[0008] The technical solution adopted by the present invention is a method for preparing a pure titanium sputtering target with a specific texture, which is specifically implemented according to the following steps:

[0009] Step 1, forging the pure titanium ingot to obtain a pure titanium rod;

[0010] Step 2, heating the pure titanium rod treated in step 1 to 890°C-1010°C and keeping the temperature for 2h-8h;

[0011] Step 3, rolling the pure titanium bar processed in step 2 for four passes;

[0012] Step 4, keeping the pure titanium bar treated in step 3 at 890°C-1010°C for 2h-8h, and continuing to roll it for two passes;

[0013] Step 5: Keep the pure titanium rod treated in step 4 at 890° C.-1010° C. for 2 h-8 h, and continue rolling for three times to obtain a pure titanium sputtering target.

[0014] The present invention is also characterized in that:

[0015] During forging in step 1, the starting forging temperature is 980°C-1180°C.

[0016] The diameter of the pure titanium rod after forging in step 1 is 80mm-200mm.

[0017] In step 3, the single pass processing rate of the first pass is 40%-60%, the single pass processing rate of the second pass is 40%-60%, the single pass processing rate of the third pass is 20%-30%, and the single pass processing rate of the fourth pass is 30%-35%.

[0018] In step 4, the processing rate of the first pass is 35%-45%, and the processing rate of the second pass is 35%-45%.

[0019] In step 5, the single-pass processing rate of the first pass is 30%-35%, the single-pass processing rate of the second pass is 30%-35%, and the single-pass processing rate of the last pass is less than 20%.

[0020] Another technical solution adopted by the present invention is that the pure titanium sputtering target material with a specific texture is prepared by the above preparation method, and its most densely packed surface Planar texture and most densely packed surface With rough surface The ratio is not less than 19.

[0021] The beneficial effects of the present invention are:

[0022] The method of the present invention adopts a specific rolling process to make the most densely packed surface Planar texture and reduced rough surface The proportion of Surface and The ratio of the surface is above 19. In addition, the method of the present invention can also obtain fine and uniform grains, which can reduce the generation of particles and improve the uniformity of sputtering coating. The titanium target material produced by the method of the present invention has a fast film forming speed and uniform film thickness during the sputtering coating process, and can be used in engineering fields such as integrated circuits, industrial glass, and liquid crystal displays. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a rolling process Texture and Schematic diagram of texture strength change. DETAILED DESCRIPTION

[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0025] The method for preparing the pure titanium sputtering target with a specific texture of the present invention is specifically implemented according to the following steps:

[0026] Step 1, forging the pure titanium ingot to obtain a pure titanium bar with a diameter of 80 mm-200 mm, and the forging temperature during forging is 980° C.-1180° C.;

[0027] Step 2, heating the pure titanium rod treated in step 1 to 890°C-1010°C and keeping the temperature for 2h-8h;

[0028] Step 3, rolling the pure titanium bar processed in step 2, controlling the single pass processing rate of the first pass to 40%-60%, the single pass processing rate of the second pass to 40%-60%, the single pass processing rate of the third pass to 20%-30%, and the single pass processing rate of the fourth pass to 30%-35%;

[0029] Step 4, the pure titanium bar treated in step 3 is kept at 890°C-1010°C for 2h-8h, and then rolled in two passes, with the first pass processing rate being controlled at 35%-45%, and the second pass processing rate being controlled at 35%-45%;

[0030] Step 5, keeping the pure titanium bar treated in step 4 at 890°C-1010°C for 2h-8h, and continuing rolling, rolling three times, controlling the single-pass processing rate of the first pass to 30%-35%, controlling the single-pass processing rate of the second pass to 30%-35%, and the single-pass processing rate of the last pass to less than 20%.

[0031] Embodiment 1:

[0032] The preparation method of a pure titanium sputtering target with a specific texture is specifically implemented according to the following steps:

[0033] Step 1, forging the pure titanium ingot to obtain a pure titanium rod with a diameter of 100 mm, wherein the starting forging temperature is 1000° C.;

[0034] Step 2, heating the pure titanium rod treated in step 1 to 895°C and keeping the temperature for 6 hours;

[0035] Step 3, rolling the pure titanium bar processed in step 2, controlling the single pass processing rate of the first pass to be 45%, the single pass processing rate of the second pass to be 45%, the single pass processing rate of the third pass to be 25%, and the single pass processing rate of the fourth pass to be 30%;

[0036] Step 4, the pure titanium bar treated in step 3 is kept at 895°C for 4 hours, and then rolled twice, with the first pass processing rate being controlled at 35% and the second pass processing rate being controlled at 35%;

[0037] Step 5, keeping the pure titanium bar treated in step 4 at 895°C for 4h, and continuing rolling for three passes, controlling the single pass processing rate of the first pass to 30%, the single pass processing rate of the second pass to 30%, and the single pass processing rate of the last pass to 18%.

[0038] Embodiment 2:

[0039] The difference from Example 1 is that the single-pass processing rate of the first pass in step 3 is 42%, the single-pass processing rate of the third pass in step 3 is 28%, the single-pass processing rate of the first pass in step 4 is 45%, and the single-pass processing rate of the last pass in step 5 is 17%.

[0040] Embodiment 3:

[0041] The difference from Example 1 is that the single-pass processing rate of the first pass in step 3 is 50%, the single-pass processing rate of the third pass in step 3 is 22%, the single-pass processing rate of the first pass in step 4 is 38%, and the single-pass processing rate of the last pass in step 5 is 16%.

[0042] Embodiment 4:

[0043] The difference from Example 1 is that the single-pass processing rate of the first pass in step 3 is 40%, the single-pass processing rate of the third pass in step 3 is 30%, the single-pass processing rate of the first pass in step 4 is 40%, and the single-pass processing rate of the last pass in step 5 is 17%.

[0044] Embodiment 5:

[0045] The difference from Example 1 is that the single-pass processing rate of the first pass in step 3 is 60%, the single-pass processing rate of the third pass in step 3 is 20%, the single-pass processing rate of the first pass in step 4 is 45%, and the single-pass processing rate of the last pass in step 5 is 19%.

[0046] Embodiment 6:

[0047] The preparation method of a pure titanium sputtering target with a specific texture is specifically implemented according to the following steps:

[0048] Step 1, forging the pure titanium ingot to obtain a pure titanium rod with a diameter of 200 mm, wherein the starting forging temperature is 1180° C.;

[0049] Step 2, heating the pure titanium rod treated in step 1 to 1010° C. and keeping the temperature for 8 hours;

[0050] Step 3, rolling the pure titanium bar processed in step 2, controlling the single pass processing rate of the first pass to be 45%, the single pass processing rate of the second pass to be 60%, the single pass processing rate of the third pass to be 25%, and the single pass processing rate of the fourth pass to be 35%;

[0051] Step 4, the pure titanium bar treated in step 3 is kept at 890°C for 8 hours, and then rolled twice, with the processing rate of the first pass being controlled to be 35%, and the processing rate of the second pass being controlled to be 45%;

[0052] Step 5, keeping the pure titanium bar treated in step 4 at 950°C for 6h, and continuing rolling for three passes, controlling the single pass processing rate of the first pass to 35%, the single pass processing rate of the second pass to 35%, and the single pass processing rate of the last pass to 19%.

[0053] Embodiment 7:

[0054] The preparation method of a pure titanium sputtering target with a specific texture is specifically implemented according to the following steps:

[0055] Step 1, forging the pure titanium ingot to obtain a pure titanium rod with a diameter of 150 mm, wherein the starting forging temperature is 1080° C.;

[0056] Step 2, heating the pure titanium rod treated in step 1 to 980°C and keeping the temperature for 6 hours;

[0057] Step 3, rolling the pure titanium bar processed in step 2, controlling the single pass processing rate of the first pass to be 45%, the single pass processing rate of the second pass to be 50%, the single pass processing rate of the third pass to be 25%, and the single pass processing rate of the fourth pass to be 32%;

[0058] Step 4, the pure titanium bar treated in step 3 is kept at 1010° C. for 5 hours, and then rolled twice, with the processing rate of the first pass being controlled to be 35%, and the processing rate of the second pass being controlled to be 40%;

[0059] Step 5, keeping the pure titanium bar treated in step 4 at 1010°C for 8h, and continuing rolling for three passes, controlling the single pass processing rate of the first pass to 33%, the single pass processing rate of the second pass to 33%, and the single pass processing rate of the last pass to 18%.

[0060] Embodiment 8:

[0061] The preparation method of a pure titanium sputtering target with a specific texture is specifically implemented according to the following steps:

[0062] Step 1, forging the pure titanium ingot to obtain a pure titanium rod with a diameter of 80 mm, wherein the starting forging temperature is 980° C.;

[0063] Step 2, heating the pure titanium rod treated in step 1 to 1010° C. and keeping the temperature for 2 hours;

[0064] Step 3, rolling the pure titanium bar processed in step 2, controlling the single pass processing rate of the first pass to be 45%, the single pass processing rate of the second pass to be 40%, the single pass processing rate of the third pass to be 25%, and the single pass processing rate of the fourth pass to be 30%;

[0065] Step 4, keeping the pure titanium bar treated in step 3 at 950° C. for 2 hours, and continuing rolling, rolling two passes, controlling the single pass processing rate of the first pass to 35%, and controlling the single pass processing rate of the second pass to 40%;

[0066] Step 5, keep the pure titanium bar treated in step 4 at 1010°C for 2h, and continue rolling for three passes, controlling the single pass processing rate of the first pass to 30%, the single pass processing rate of the second pass to 33%, and the single pass processing rate of the last pass to 16%.

[0067] In order to verify the technical effect of the solution of the present invention, the following 8 comparative examples are set for comparison, wherein the solutions of the 8 comparative examples are:

[0068] Comparative Example 1:

[0069] The difference between Comparative Example 1 and Example 1 is that the single pass processing rate of the first pass in step 3 is 35%.

[0070] Comparative Example 2:

[0071] The difference between Comparative Example 2 and Example 1 is that the single pass processing rate of the third pass in step 3 is 35%.

[0072] Comparative Example 3:

[0073] The difference between Comparative Example 3 and Example 1 is that the single pass processing rate of the first pass in step 4 is 30%.

[0074] Comparative Example 4:

[0075] The difference between Comparative Example 4 and Example 1 is that the single-pass processing rate of the last pass in step 5 is 24%.

[0076] Comparative Example 5:

[0077] The difference between Comparative Example 5 and Example 1 is that the single-pass processing rate of the first pass in step 3 is 62%.

[0078] Comparative Example 6:

[0079] The difference between Comparative Example 6 and Example 1 is that the single-pass processing rate of the first pass in step 4 is 47%.

[0080] Comparative Example 7:

[0081] The difference between Comparative Example 7 and Example 1 is that the single pass processing rate of the third pass in step 3 is 15%.

[0082] Comparative Example 8:

[0083] The difference between Comparative Example 8 and Example 1 is that the single-pass processing rate of the first pass in step 3 is 30%, and the single-pass processing rate of the third pass in step 3 is 35%.

[0084] Table 1 shows the process conditions and performance test results of Examples 1-5 and Comparative Examples 1-8:

[0085] Table 1 Process conditions and performance of Examples 1-5 and Comparative Examples 1-8

[0086]

[0087] In addition, the target materials prepared in Examples 6-8 / The ratios are 20.0, 22.5 and 21.1 respectively. It can be seen that the ratios of the most densely packed surface and the rough surface of the target material prepared by the method of the present invention are both high.

[0088] By comparing Example 1 with Comparative Examples 1 and 5, it can be seen that when the single pass processing rate of the first pass in step 3 is not between 40% and 60%, the most densely packed surface Less plane texture, rough surface The proportion is relatively large, and the ratio between the two is only 9.8 and 7.7, which is much smaller than 22.1 in Example 1.

[0089] By comparing Example 1 with Comparative Examples 2 and 7, it can be seen that when the single pass processing rate of the third pass in step 3 is not between 20% and 30%, the most densely packed surface Less plane texture, rough surface The proportion is relatively large, and the ratio between the two is only 6.5 and 6.3, which is much smaller than 22.1 in Example 1.

[0090] By comparing Example 1 with Comparative Examples 3 and 6, it can be seen that when the single pass processing rate of the first pass in step 4 is not between 35% and 45%, the most densely packed surface Less plane texture, rough surface The proportion is relatively large, and the ratio between the two is only 4.3 and 8.4, which is much smaller than 22.1 in Example 1.

[0091] By comparing Example 1 and Comparative Example 4, it can be seen that when the single pass processing rate of the last pass of step 5 is greater than 20%, the most densely packed surface Less plane texture, rough surface The proportion is relatively large, and the ratio between the two is only 7.2, which is much smaller than 22.1 in Example 1.

[0092] Therefore, from the comparison between Examples 1-5 and Comparative Examples 1-8, it can be seen that the single pass processing rates of each pass in the specific rolling process of the present invention cooperate with each other and achieve the best effect. In particular, the single pass processing rates of the first and third passes in step 3, the single pass processing rate of the first pass in step 4, and the single pass processing rate of the last pass in step 5 have a decisive influence on the final texture, such as Figure 1 As shown, after step 3 After step 4, a strong Focused orientation, after step 5 The basal plane concentration orientation is further enhanced; on the contrary, after steps 3, 4 and 5, The degree of plane concentration orientation is significantly weakened and relatively dispersed.

[0093] The method of the present invention adopts a specific rolling process to make the most densely packed surface Planar texture and reduced rough surface The proportion of Surface and The ratio of the surface to the surface is above 19. In addition, fine and uniform grains can be obtained. This can reduce the generation of particles and improve the uniformity of the sputtering coating. Using the rolling process of comparative examples 1-8 will make the rough surface This increases the possibility of particle generation and reduces the uniformity of sputtering coating.

Claims

1. A method for preparing a pure titanium sputtering target with a specific texture, characterized in that: Follow the steps below to implement it: Step 1, forging the pure titanium ingot to obtain a pure titanium rod; Step 2, heating the pure titanium rod treated in step 1 to 890°C-1010°C and keeping the temperature for 2h-8h; Step 3, rolling the pure titanium bar processed in step 2 for four passes; Step 4, keeping the pure titanium bar treated in step 3 at 890°C-1010°C for 2h-8h, and continuing to roll it for two passes; Step 5, keeping the pure titanium rod treated in step 4 at 890° C.-1010° C. for 2 h-8 h, and continuing to roll for three times to obtain a pure titanium sputtering target; In step 3, the single pass processing rate of the first pass is 40%-60%, the single pass processing rate of the second pass is 40%-60%, the single pass processing rate of the third pass is 20%-30%, and the single pass processing rate of the fourth pass is 30%-35%; In step 4, the processing rate of the first pass is 35%-45%, and the processing rate of the second pass is 35%-45%; In step 5, the single-pass processing rate of the first pass is 30%-35%, the single-pass processing rate of the second pass is 30%-35%, and the single-pass processing rate of the last pass is less than 20%.

2. The method for preparing a pure titanium sputtering target with a specific texture according to claim 1, characterized in that: During forging in step 1, the starting forging temperature is 980°C-1180°C.

3. The method for preparing a pure titanium sputtering target with a specific texture according to claim 1, characterized in that: The diameter of the pure titanium rod after forging in step 1 is 80mm-200mm.

4. A pure titanium sputtering target with a specific texture, characterized in that: The target material is prepared by the preparation method according to any one of claims 1 to 3, wherein the most densely packed surface of the target material Planar texture and most densely packed surface With rough surface The ratio is not less than 19.