Semiconductor material, semiconductor device and preparation method

By forming a new wide-bandgap semiconductor material β-(RhxGa1-x)2yO3 through Rh solid solution β-Ga2O3, the problem of low valence band top energy level and doping of β-Ga2O3 is solved, and a higher carrier mobility and The lower effective hole mass improves the power characteristics of semiconductor devices.

CN118621440BActive Publication Date: 2024-11-22深圳平湖实验室
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411098062.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The valence band top of β-Ga2O3 is contributed by the 2p orbital orbital energy level position, resulting in a flat dispersion relationship, making it difficult to excite the formation of hole carriers, and common doping elements are difficult to increase their valence band top energy level. This limits the implementation of p-type doping and affects the power characteristics of semiconductor devices.

Method used

Through Rh solid solution β-Ga2O3, the electron orbital action of Rh solid solution β-Ga2O3 forms a new valence band top, which increases the energy level of the valence band top and improves the dispersion relationship and reduces holes. Self-capture phenomenon to achieve p-type doping.

Benefits of technology

The performance of semiconductor devices is improved, higher carrier mobility and lower effective hole mass are achieved, the power characteristics and stability of semiconductor devices are enhanced, and the p-type doping problem of β-Ga2O3 is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621440B_ABST
    Figure CN118621440B_ABST
Patent Text Reader

Abstract

The present application discloses a semiconductor material, a semiconductor device and a preparation method. The chemical formula of the semiconductor material is β-(Rh x Ga 1‑x ) 2y O 3 , where 0<x≤0.5, and 0.9≤y≤1.1. The semiconductor material is formed by Rh solid solution β-Ga 2 O 3 Rh solid solution in β-Ga 2 O 3 Afterwards, the electron orbits of Rh and O interact to form a new valence band top, which has a higher energy level than β-Ga 2 O 3 The energy level of the valence band top has increased significantly. The new valence band top dispersion relation is steep, and a steep dispersion relation represents a lower hole effective mass, which will reduce the occurrence of hole self-capture and polarization. x Ga 1‑x ) 2y O 3 Potential solution to β-Ga 2 O 3 The p-type doping problem can be used to prepare power semiconductor devices with better performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a semiconductor material, a semiconductor device and a preparation method thereof. Background Art

[0002] The power characteristics of semiconductor devices are positively correlated with the band gap and carrier mobility of semiconductor materials. Gallium oxide has an ultra-wide band gap (about 4.9 eV) and a mature preparation method, making it an ideal material for preparing high-power semiconductor devices. β-phase gallium oxide (β-Ga2O3) has the most stable crystal structure and can be used in high temperature, high pressure and high power fields. Similar to many oxides, the valence band top of β-Ga2O3 is mainly contributed by the 2p orbital of oxygen atoms, the orbital energy level position is low, and the dispersion relation is flat. The energy levels of common neighboring elements (such as Mg, Zn, etc.) doped acceptors are mostly above 1 eV, which are difficult to excite to form hole carriers. The flat dispersion relation indicates a high hole effective mass, and hole self-capture and polarization phenomena are prone to occur. Therefore, it is necessary to modulate and modify β-Ga2O3 to increase its valence band top energy level position and improve the dispersion relation to facilitate p-type doping. Summary of the invention

[0003] The present application discloses a semiconductor material, a semiconductor device and a preparation method. A novel wide bandgap semiconductor material β-(Rh x Ga 1-x ) 2y O3 improves the energy level position of the top of the valence band and improves the dispersion relation of the top of the valence band, which is expected to achieve p-type doping and improve the performance of semiconductor power devices.

[0004] In order to achieve the above objectives, this application provides the following technical solutions:

[0005] In a first aspect, the present application provides a semiconductor material, the chemical formula of which is β-(Rh x Ga 1-x ) 2y O3, wherein 0<x≤0.5, and 0.9≤y≤1.1.

[0006] The above semiconductor material is obtained by solid dissolving Rh in β-Ga2O3 to obtain a new wide bandgap semiconductor material β-(Rh x Ga 1-x ) 2y O3, where 0<x≤0.5, and 0.9≤y≤1.1. After Rh is dissolved in β-Ga2O3, the electron orbits of Rh and O form a new valence band top, and the energy level of the new valence band top is significantly higher than that of β-Ga2O3. Since the atomic radius of Rh is close to that of Ga, the obtained solid solution β-(Rhx Ga 1-x ) 2y O3 has high stability. In addition, the new valence band top dispersion relation is steep, and a steep dispersion relation represents a lower hole effective mass, which reduces the occurrence of hole self-capture and polarization. x Ga 1-x ) 2y O3 is expected to solve the p-type doping problem of β-Ga2O3 and can be used to prepare power semiconductor devices with better performance.

[0007] In some embodiments, the semiconductor material β-(Rh x Ga 1-x ) 2y In O3, the range of x is 0.125≤x≤0.25, and the range of y is 0.9≤y≤1.1. x Ga 1-x ) 2y When the atomic percentage of Rh in the O3 material is 0.125≤x≤0.25, β-(Rh x Ga 1-x ) 2y O3 material has a smaller hole effective mass and higher carrier mobility, which is more conducive to achieving p-type doping.

[0008] In some embodiments, the crystal structure of the semiconductor material is a monoclinic crystal structure. This structure is the most stable crystal configuration of β-Ga2O3. When Rh is dissolved in β-Ga2O3 of this configuration, the resulting solid solution β-(Rh x Ga 1-x ) 2y O3 is also relatively stable.

[0009] In some embodiments, the mixing enthalpy of the semiconductor material is 0 eV / cation-0.14 eV / cation. x Ga 1-x ) 2y The mixing enthalpy of O3 is low, indicating that it has good structural stability.

[0010] In some embodiments, the hole effective mass of the semiconductor material is 2 m e -7 m e The β-(Rh x Ga 1-x ) 2y The effective hole mass of O3 is small, which can reduce the occurrence of hole self-capture and other phenomena, and help achieve p-type doping.

[0011] In some embodiments, the difference between the valence band top energy level of the semiconductor material and β-Ga2O3 is greater than or equal to 1.1 eV. After Rh is dissolved in β-Ga2O3, the electron orbits of Rh and O interact to form a new valence band top, and the new valence band top energy level is significantly higher than that of β-Ga2O3.

[0012] In some embodiments, the energy band gap value of the semiconductor material is 3.77 eV-4.10 eV. After Rh is dissolved in β-Ga2O3, β-(Rh x Ga 1-x ) 2y O3 still has a relatively wide energy band gap value and is a wide band gap semiconductor, which is conducive to the preparation of high-power semiconductor devices.

[0013] In a second aspect, the present application provides a semiconductor device, comprising a substrate and a semiconductor layer, wherein the semiconductor layer is made of the semiconductor material as described in the first aspect.

[0014] In some embodiments, the semiconductor layer is a p-type semiconductor layer or an n-type semiconductor layer. x Ga 1-x ) 2y The O3 semiconductor layer can achieve p-type doping or n-type doping to improve the performance of semiconductor power devices.

[0015] In some embodiments, the crystal orientation of the substrate is

[010] . Using a substrate with a crystal orientation of

[010] , Rh is grown along the b axis, so that the obtained β-(Rh x Ga 1-x ) 2y The O3 semiconductor layer has lower energy, a more stable material system, and a lower effective hole mass, which is more conducive to achieving p-type doping.

[0016] In a third aspect, the present application provides a method for preparing a semiconductor device, comprising:

[0017] Substrate preheating: Place the β-Ga2O3 substrate in the growth chamber and preheat it;

[0018] Growth: Introducing source materials including an O source, a Ga source, and a Rh source into the growth chamber, and growing β-(Rh x Ga 1-x ) 2y O3 semiconductor layer, wherein 0<x≤0.5, and 0.9≤y≤1.1.

[0019] In some embodiments, the crystal orientation of the β-Ga2O3 substrate is

[010] .

[0020] In some embodiments, the temperature of the Ga source introduced is 800°C-900°C, and the temperature of the Rh source introduced is ≥1500°C. High temperature is conducive to regulating the evaporation rate of the Ga source and the Rh source, and thus is conducive to regulating the β-(Rh x Ga 1-x ) 2y Growth rate of O3 on substrate.

[0021] In some embodiments, the β-(Rh x Ga 1-x ) 2y The growth temperature of O3 is 600℃-800℃. By controlling the growth temperature, a more ideal β-(Rh x Ga 1-x ) 2y O3 semiconductor material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of a process for preparing a semiconductor device according to an embodiment of the present application;

[0023] Figure 2 The molecular beam epitaxy method provided in the present application is used to prepare β-(Rh x Ga 1-x ) 2y Schematic diagram of O3;

[0024] Figure 3 Provided in the present application embodiment is β-(Rh x Ga 1-x ) 2y Real-space electron localized state density diagram of the highest valence band of O3;

[0025] Figure 4 The β-(Rh x Ga 1-x ) 2y Schematic diagram of the unit cell configuration structure of O3;

[0026] Figure 5 The β-(Rh x Ga 1-x ) 2y Unit cell parameter diagram of O3;

[0027] Figure 6 The calculated β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 and the corresponding volume of a single molecular formula;

[0028] Figure 7The β-(Rh x Ga 1-x ) 2y Energy band structure diagram of O3;

[0029] Figure 8 The β-(Rh x Ga 1-x ) 2y Average hole effective mass of O3;

[0030] Fig. 9 The β-(Rh x Ga 1-x ) 2y Band alignment diagram of O3. DETAILED DESCRIPTION

[0031] First, let me introduce the application scenarios. High-power semiconductor devices are crucial to the development of new energy vehicles, smart grids and other technologies, and can improve energy conversion efficiency. The power characteristics of semiconductor devices are positively correlated with the band gap and carrier mobility of semiconductor materials. Gallium oxide has an ultra-wide band gap (about 4.9 eV) and a mature preparation method, making it an ideal material for preparing high-power semiconductor devices. Gallium oxide has been reported to have five crystal configurations, and β-phase gallium oxide (β-Ga2O3, with a space group of monoclinic C2 / m) is the most stable crystal structure, which can be used in high temperature, high pressure and high power fields. Current research on gallium oxide is mostly based on this crystal configuration.

[0032] Similar to many oxides, the valence band top of β-Ga2O3 is mainly contributed by the 2p orbital of oxygen atoms, with low orbital energy level and flat dispersion relation. The energy levels of common neighboring elements (such as Mg, Zn, etc.) are mostly above 1eV, which makes it difficult to excite hole carriers. The flat dispersion relation indicates high hole effective mass, which is prone to hole self-capture and polarization. Due to the lack of p-type doping, the current semiconductor devices of β-Ga2O3 are mostly based on unipolar transport of Schottky junction and bipolar transport of pn heterojunction. For the same semiconductor material, the barrier of the Schottky junction formed with metal is lower than the barrier height of the pn junction, and the power characteristics of the Schottky junction device are significantly lower than the latter. For pn heterojunction devices composed of n-type β-Ga2O3 and other p-type oxides (such as NiO), the interface state caused by lattice mismatch often becomes the dominant mechanism of reverse leakage, and the power characteristics of the corresponding devices are still significantly lower than the theoretical limit of β-Ga2O3 materials. Therefore, it is necessary to modulate and modify β-Ga2O3, improve the position of its valence band top energy level and improve the dispersion relation in order to achieve p-type doping.

[0033] For metal oxides, metal cations with full electron shells can be used to increase the valence band top energy level and the dispersion relation curvature. For β-Ga2O3, in existing studies, the configuration of Bi solid solution β-Ga2O3 is β-(Bi x Ga 1-x )2O3, Bi with a larger atomic radius is used for solid solution. Due to the large difference in atomic radius between Bi and Ga, the corresponding mixing enthalpy is high, making it difficult to carry out solid solution at a higher concentration. The solid solution may easily decompose at high temperature, and the energy band gap value is small.

[0034] Based on the above problems, the present invention provides a semiconductor material, which is a novel wide bandgap semiconductor material β-(Rh x Ga 1-x ) 2y Compared with the existing solution of Bi solid solution β-Ga2O3, this application adopts Rh solid solution, which is close to the atomic radius of Ga, and the obtained solid solution has higher stability. Rh and O orbital interaction form a new valence band top, which increases the energy level of the valence band top and improves the dispersion relation of the valence band top. β-(Rh x Ga 1-x ) 2y Compared with commercial SiC and GaN, O3 still has a wider band gap value. x Ga 1-x ) 2y O3 is expected to achieve n-type and p-type doping of the same wide-bandgap semiconductor material and improve the performance of semiconductor power devices.

[0035] In a first aspect, the present invention provides a semiconductor material, the chemical formula of which is β-(Rh x Ga 1-x ) 2y O3, wherein 0<x≤0.5, and 0.9≤y≤1.1.

[0036] The above semiconductor material is obtained by solid dissolving β-Ga2O3 with metal rhodium Rh to obtain a new wide bandgap semiconductor material β-(Rh x Ga 1-x ) 2y O3, where 0<x≤0.5, and 0.9≤y≤1.1. After Rh is dissolved in β-Ga2O3, the electron orbits of Rh and O form a new valence band top, and the energy level of the new valence band top is significantly higher than that of β-Ga2O3. Since the atomic radius of Rh is close to that of Ga, the obtained solid solution β-(Rh x Ga 1-x ) 2yO3 has high stability. In addition, the new valence band top dispersion relation is steep, and a steep dispersion relation represents a lower hole effective mass, which reduces the occurrence of hole self-capture and polarization. x Ga 1-x ) 2y O3 is expected to solve the p-type doping problem of β-Ga2O3 and can be used to prepare power semiconductor devices with better performance.

[0037] The solid solution β-(Rh x Ga 1-x ) 2y O3 has high stability, wide band gap, high valence band top energy level and steep valence band top dispersion relation. It is easy to achieve p-type doping and can improve the performance of semiconductor power devices.

[0038] It should be noted that the β-(Rh x Ga 1-x ) 2y In O3, x and y represent atomic percentages, wherein 0<x≤0.5, and 0.9≤y≤1.1. For example, x can be 0.0625, 0.125, 0.1875, 0.25, 0.3125, 0.375, 0.4375, 0.5, etc., or a value between any two of the above values, and the specific value is not limited. y can be 0.9, 0.92, 0.94, 0.96, 0.98, 1, 1.02, 1.04, 1.06, 1.08, 1.1, etc., or a value between any two of the above values, and the specific value is not limited.

[0039] In some embodiments, 0.125≤x≤0.25, and 0.9≤y≤1.1. For example, x can be 0.125, 0.1875, 0.25, etc., or a value between any two of the above values, and the specific value is not limited. y can be 0.9, 0.92, 0.94, 0.96, 0.98, 1, 1.02, 1.04, 1.06, 1.08, 1.1, etc., or a value between any two of the above values, and the specific value is not limited. When β-(Rh x Ga 1-x ) 2y When the atomic percentage of Rh in the O3 material is 0.125≤x≤0.25, β-(Rh x Ga 1-x ) 2y O3 material has a smaller hole effective mass and higher carrier mobility, which is more conducive to achieving p-type doping.

[0040] In some embodiments, the crystal structure of the semiconductor material is a monoclinic crystal structure. This structure is the most stable crystal configuration of β-Ga2O3. When Rh is dissolved in β-Ga2O3 of this configuration, the resulting solid solution β-(Rh x Ga 1-x ) 2y O3 is also relatively stable.

[0041] In some embodiments, the mixing enthalpy of the semiconductor material is 0 eV / cation-0.14 eV / cation. Exemplarily, the mixing enthalpy of the semiconductor material can be 0 eV / cation, 0.02 eV / cation, 0.04 eV / cation, 0.06 eV / cation, 0.08 eV / cation, 0.10 eV / cation, 0.12 eV / cation, 0.14 eV / cation, etc., or a value between any two of the above values, and the specific value is not limited. The β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is low, indicating that it has good structural stability, which is conducive to the realization of high-concentration Rh solid solution, and the solid solution is not prone to phase decomposition at high temperature.

[0042] In some embodiments, the hole effective mass of the semiconductor material is 2 m e -7 m e For example, the effective mass of a hole in a semiconductor material may be 2 m e -7 m e , 2 m e -6 m e , 2 m e -5.5 m e , 2 m e -5 m e , 2 m e -4.5 m e , 2 m e -4m e , 2 m e -3.5 m e , 2 m e -3 m e In one possible implementation, the effective mass of the hole in the semiconductor material is 2.22 m e -4 m e The β-(Rh x Ga 1-x ) 2yThe effective hole mass of O3 is small, which can reduce the occurrence of hole self-capture and other phenomena, and is conducive to the realization of p-type doping.

[0043] In some embodiments, the difference between the semiconductor material and the valence band top energy level of β-Ga2O3 is greater than or equal to 1.1 eV. Exemplarily, the difference between the semiconductor material and the valence band top energy level of β-Ga2O3 can be 1.1 eV, 1.2 eV, 1.3 eV, 1.4 eV, 1.5 eV, 1.6 eV, 1.8 eV, 1.9 eV, 2.0 eV, 2.1 eV, 2.2 eV, 2.3 eV, etc., and the specific numerical range is not limited. After Rh is dissolved in β-Ga2O3, the electronic orbits of Rh and O form a new valence band top, and the new valence band top energy level has significantly increased compared to the valence band top energy of β-Ga2O3.

[0044] In some embodiments, the band gap value of the semiconductor material is 3.77 eV-4.10 eV. For example, the band gap value of the semiconductor material can be 3.77 eV, 3.78 eV, 3.80 eV, 3.88 eV, 3.95 eV, 4.02 eV, 4.07 eV, 4.10 eV, etc., or a value between any two of the above values, and the specific value is not limited. After Rh is dissolved in β-Ga2O3, β-(Rh x Ga 1-x ) 2y O3 still has a relatively wide energy band gap value and is a wide band gap semiconductor, which is conducive to the preparation of high-power semiconductor devices.

[0045] In a second aspect, an embodiment of the present application provides a semiconductor device, including a substrate and a semiconductor layer, wherein the semiconductor layer is made of the semiconductor material of the first aspect.

[0046] In some embodiments, the semiconductor layer is a p-type semiconductor layer or an n-type semiconductor layer. x Ga 1-x ) 2y The O3 semiconductor layer can achieve p-type doping or n-type doping to improve the performance of semiconductor power devices. x Ga 1-x ) 2y The O3 semiconductor layer can also achieve p-type doping and n-type doping at the same time.

[0047] In some embodiments, the crystal orientation of the substrate is

[010] . Using a substrate with a crystal orientation of

[010] , Rh is grown along the b-axis, so that the obtained β-(Rh x Ga 1-x ) 2yThe O3 semiconductor layer has lower energy, a more stable material system, and a lower effective hole mass, which is more conducive to achieving p-type doping.

[0048] In a third aspect, an embodiment of the present application provides a method for preparing a semiconductor device. Figure 1 The schematic flow chart of the method for preparing a semiconductor device provided in the embodiment of the present application specifically includes the following steps:

[0049] S101, substrate preheating: placing the β-Ga2O3 substrate in the growth chamber and preheating it;

[0050] S102, growth: introducing source materials including O source, Ga source and Rh source into the growth chamber, and growing β-(Rh x Ga 1-x ) 2y O3 semiconductor layer, wherein 0<x≤0.5, and 0.9≤y≤1.1.

[0051] Figure 2 The molecular beam epitaxy method provided in the present application is used to prepare β-(Rh x Ga 1-x ) 2y Schematic diagram of O3. Figure 2 As shown, the specific process of preparing semiconductor devices by molecular beam epitaxy (MBE) method in this application is as follows:

[0052] (1) Substrate preheating: Place the β-Ga2O3 substrate in the MBE growth chamber and gradually heat it to about 600℃-700℃ to remove surface contaminants.

[0053] (2) Growth process: ① Introduce an oxygen source and control the oxygen partial pressure at 10 -5 -10 -6 Torr range to ensure full oxidation; use high-purity O2 source, generate atomic O (O source) through radio frequency plasma source, and control the power of radio frequency source at 200-300W. ② Heat the growth source (Ga source and Rh source), the source material is evaporated by electron beam to generate molecular beam, and the molecular beam exchanges energy with β-Ga2O3 substrate, and then undergoes surface adsorption, migration, nucleation, growth and film formation to obtain β-(Rh x Ga 1-x ) 2y O3 semiconductor layer. ③ The evaporation rate of Ga and Rh is detected and adjusted by the beam detector, and the initial rate is controlled in the range of 0.1-1 Å / s.

[0054] (3) Post-growth treatment: gradually lower the substrate temperature to avoid thermal stress and cracks caused by sudden cooling; annealing treatment is possible, and low-temperature annealing (such as 400℃-600℃) can improve crystal quality.

[0055] It should be noted that the semiconductor device of the present application can also be prepared by various deformation physical and chemical vapor deposition epitaxial growth methods, such as pulsed laser deposition, atomized chemical vapor deposition, etc.

[0056] In some embodiments, the crystal orientation of the β-Ga2O3 substrate is

[010] . x Ga 1-x ) 2y O3 benefits from the state density of O-Rh-O delocalization along the b axis. Therefore, the experimental preparation uses

[010] crystal orientation β-Ga2O3 as β-(Rh x Ga 1-x ) 2y Epitaxial substrate for O3 thin film growth. β-(Rh x Ga 1-x ) 2y The crystal orientation of the O3 semiconductor material is also

[010] , that is, the

[010] crystal orientation of the substrate is consistent with that of β-(Rh x Ga 1-x ) 2y The crystal orientation of O3 is consistent, which is convenient for β-(Rh x Ga 1-x ) 2y O3 growth, so that the obtained β-(Rh x Ga 1-x ) 2y The effective mass of O3 holes is small.

[0057] In β-(Rh x Ga 1-x ) 2y In the configuration of O3, the configuration with Rh distributed along the b axis has lower energy and the system is more stable. x Ga 1-x ) 2y The effective mass of the configuration hole partially occupied by Rh along the b axis in O3 is 3.56 m e , and the effective mass of the hole in the fully occupied configuration along the b axis is 2.70 m e That is to say, the Rh distribution configuration along the b axis has lower energy and smaller hole effective mass. After analysis, the above phenomenon is due to the β-(Rh x Ga 1-x ) 2y The electronic state density of O-Rh-O delocalization when Rh is distributed along the b-axis in the O3 configuration.

[0058] Figure 3 The β-(Rh x Ga 1-x ) 2y The real-space electron localized state density diagram of the highest valence band of O3. Figure 3 As shown, Figure 3 (a) in the equation is β-(Rh 0.0625 Ga 0.9375 )The distribution diagram of the electron state density of the highest valence band of 2O3, Figure 3 (b) in the equation is β-(Rh 0.125 Ga 0.875 )The distribution diagram of the electron state density of the highest valence band of 2O3, Figure 3 (c) in the equation is β-(Rh 0.1825 Ga 0.8125 )The distribution diagram of the electron state density of the highest valence band of 2O3, Figure 3 The (d) in the equation is β-(Rh 0.25 Ga 0.75 )2O3 highest valence band electronic state density distribution diagram, where the electronic state density equipotential surface is set to 0.001 e / Å 3 As can be seen from the figure, Rh tends to be distributed along the b-axis. Therefore, in the experimental preparation, a β-Ga2O3 substrate with a crystal orientation of

[010] was used to grow β-(Rh x Ga 1-x ) 2y The crystal orientation of the O3 semiconductor material is also

[010] , and the resulting semiconductor device has a lower effective hole mass, which is more conducive to achieving p-type doping.

[0059] In some embodiments, the temperature of the Ga source introduced is 800°C-900°C, and the temperature of the Rh source introduced is ≥1500°C. High temperature is conducive to regulating the evaporation rate of the Ga source and the Rh source, and thus is conducive to regulating the β-(Rh x Ga 1-x ) 2y Growth rate of O3 on substrate.

[0060] In one possible implementation, the Ga source is heated by a high-temperature source furnace, and the temperature is controlled in the range of 800℃-900℃. Rh has a high melting point and a slow evaporation rate, so it is heated by multiple high-temperature source furnaces, and the temperature is generally above 1500℃, and electron beam evaporation is used to compensate for the problem of insufficient Rh evaporation rate.

[0061] In some embodiments, β-(Rh x Ga 1-x ) 2yThe suitable growth temperature of O3 is 600℃-800℃. The growth temperature of the present application is gradually optimized from low temperature to high temperature. By controlling the growth temperature, a more ideal β-(Rh x Ga 1-x ) 2y O3 semiconductor material.

[0062] The above β-(Rh x Ga 1-x ) 2y The structure and parameters of O3 are explained. The following will be combined with specific examples to explain the β-(Rh x Ga 1-x ) 2y O3 provides further details.

[0063] Examples 1-8

[0064] Embodiments 1 to 8 are semiconductor materials, respectively, and their molecular formulas are β-(Rh 0.0625 Ga 0.9375 )2O3、β-(Rh 0.125 Ga 0.875 )2O3、β-(Rh 0.1825 Ga 0.8125 )2O3、β-(Rh 0.25 Ga 0.75 )2O3、β-(Rh 0.3125 Ga 0.6875 )2O3、β-(Rh 0.375 Ga 0.625 )2O3、β-(Rh 0.4375 Ga 0.5625 )2O3、β-(Rh 0.5 Ga 0.5 )2O3.

[0065] The present application gives the unit cell configuration of the semiconductor materials of Examples 4 and 8, calculates the unit cell parameters of the semiconductor materials of Examples 1-8, calculates the mixing enthalpy of the semiconductor materials of Examples 1-8 and the volume corresponding to a single molecular formula, obtains the energy band structure diagram of the semiconductor materials of Examples 1-8, calculates the average hole effective mass of the semiconductor materials of Examples 1-8, and obtains the energy band alignment diagram of the semiconductor materials of Examples 1-8.

[0066] Figure 4 The β-(Rh x Ga 1-x ) 2y Schematic diagram of the unit cell structure of O3, where Figure 4 (a) in the equation is β-(Rh 0.25 Ga0.75 )2O3 unit cell configuration, Figure 4 (b) in the equation is β-(Rh 0.5 Ga 0.5 )2O3 unit cell configuration. Figure 4 As shown in the figure, for Rh solid solution β-Ga2O3, there are two unequal Ga atoms in the β-Ga2O3 unit cell, one located at the center of the octahedron formed by oxygen atoms, and the other located at the center of the tetrahedron formed by oxygen atoms. Energy analysis shows that the solid solution β-(Rh x Ga 1-x ) 2y In the O3 configuration, Rh is stable at the center of the octahedron. Then, the energy difference of Rh at different distributions at the center of the octahedron was investigated, and it was found that Rh is more likely to be dispersed in the ac plane. Figure 4 As shown, when β-(Rh x Ga 1-x ) 2y After x reaches 0.25 in O3, Rh begins to occupy adjacent octahedral centers. When x is 0.5, all octahedral centers in the unit cell are occupied.

[0067] Figure 5 The β-(Rh x Ga 1-x ) 2y Unit cell parameter diagram of O3, where Figure 5 (a) in the equation is the unit cell parameter on the a-axis. Figure 5 (b) in the equation is the unit cell parameter on the b-axis. Figure 5 (c) in the figure is the unit cell parameter on the c-axis. Based on the 1×2×2 β-Ga2O3 supercell, the unit cell configurations under different x values ​​were investigated, and the difference in x for each unit cell was 0.0625. x Ga 1-x ) 2y The lattice parameters of O3 are as follows Figure 5 As shown, the unit cell parameters in different directions have increased, but the increase percentages are very small. This is because the atomic radii of Rh and Ga are very close.

[0068] In the present application, the solid solution β-(Rh x Ga 1-x ) 2y The stability of O3 and the calculation formula of the mixing enthalpy of semiconductor materials are:

[0069]

[0070] in, is the energy of the solid solution, and Corresponding to the energies of the most stable configurations of Ga2O3 and Rh2O3 respectively. is the number of cations in the solid solution configuration.

[0071] Figure 6 The calculations provided for Examples 1-8 yielded β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 and the volume corresponding to a single molecular formula. Figure 6 As shown, the figure also gives β-(Bi x Ga 1-x )2O3 data are compared. As can be seen from the figure, β-(Rh x Ga 1-x ) 2y O3 and β-(Bi x Ga 1-x )2O3 increases with the increase of x, but the former increases slowly while the latter increases rapidly. x Ga 1-x )2O3 has a mixing enthalpy of about 0.14 eV / cation when the Bi content is x=0.125. The high mixing enthalpy indicates that it is difficult to carry out solid solution at a higher concentration. x Ga 1-x ) 2y The mixing enthalpy of O3 reaches 0.14 eV / cation only when the Rh content is x=0.5, indicating that β-(Rh x Ga 1-x ) 2y O3 can achieve a higher Rh content in solid solution. And, corresponding to β-(Rh 0.5 Ga 0.5 )2O3 is even significantly smaller than β-(Bi 0.125 Ga 0.875 )2O3 volume. Based on the smaller volume change, at the same concentration, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is significantly lower than that of β-(Bi x Ga 1-x )2O3 value, indicating that β-(Rh x Ga 1-x ) 2y O3 has better structural stability.

[0072] And, from Figure 6 It can be seen that β-(Rh x Ga 1-x ) 2yThe mixing enthalpy of O3 semiconductor material is 0 eV / cation-0.14 eV / cation. Specifically, when x=0.0625, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.015 eV / cation. When x=0.125, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.03 eV / cation. When x=0.1875, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.046 eV / cation. When x=0.25, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.06 eV / cation. When x=0.3125, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.082 eV / cation. When x=0.375, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.1 eV / cation. When x=0.4375, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.12 eV / cation. When x=0.5, β-(Rh x Ga 1-x ) 2y The mixing enthalpy of O3 is about 0.14 eV / cation, which is conducive to achieving a higher concentration of Rh solid solution, and the solid solution is not prone to phase decomposition at high temperature.

[0073] Figure 7 The β-(Rh x Ga 1-x ) 2y The energy band structure diagram of O3, where Figure 7 (a) in the equation is β-(Rh 0.0625 Ga 0.9375 )2O3 energy band structure diagram, Figure 7 (b) in the equation is β-(Rh 0.125 Ga 0.875 )2O3 energy band structure diagram, Figure 7 (c) in the equation is β-(Rh 0.1825 Ga0.8125 )2O3 energy band structure diagram, Figure 7 The (d) in the equation is β-(Rh 0.25 Ga 0.75 )2O3 energy band structure diagram, Figure 7 The (e) in the equation is β-(Rh 0.3125 Ga 0.6875 )2O3 energy band structure diagram, Figure 7 The (f) in the equation is β-(Rh 0.375 Ga 0.625 )2O3 energy band structure diagram, Figure 7 The (g) in the equation is β-(Rh 0.4375 Ga 0.5625 )2O3 energy band structure diagram, Figure 7 The (h) in the formula is β-(Rh 0.5 Ga 0.5 )The energy band structure diagram of 2O3.

[0074] like Figure 7 As shown in the figure, solid solution Rh can improve the dispersion relation of the valence band top of β-Ga2O3. In the range of 0<x≤0.25, β-(Rh x Ga 1-x ) 2y O3 is a direct bandgap semiconductor. Both the bottom of the conduction band and the top of the valence band are located at the center of the Brillouin zone. The dispersion relation of the top of the valence band becomes steeper with the increase of x. Analysis shows that the top of the valence band is mainly contributed by the delocalized density of states of Rh and neighboring O. When x is greater than 0.25, Rh begins to occupy the center of the neighboring octahedron, and the interaction between neighboring Rh changes the position and dispersion relation of the top and bottom of the valence band. β-(Rh 0.3125 Ga 0.6875 )2O3 is still a direct bandgap semiconductor with the bottom of the conduction band and the top of the valence band located at the point. When x is 0.375 and 0.4375, the top of the valence band moves to the high symmetry N point. 0.5 Ga 0.5 )2O3, the valence band top is located between the high symmetry paths NX. 0.4375 Ga 0.5625 )2O3 and β-(Rh 0.5 Ga 0.5 )2O3 conduction band bottom is transferred to N point.

[0075] Based on β-(Rh x Ga 1-x ) 2y The dispersion relation of O3 is used to calculate the effective mass of holes. Specifically, this application is based on Figure 7 The band structure of β-(Rh x Ga 1-x ) 2yThe position of the valence band top of O3. According to the position of the valence band top, the energy band dispersion relation is drawn using high-density k points along the high-symmetry direction, and the dispersion relation near the valence band top is fitted using a second-order polynomial function. The hole effective mass in the direction of the high-symmetry path is calculated based on the fitting function.

[0076] The calculation formula of hole effective mass is:

[0077]

[0078] in, is the Dirac constant, is the k-point value in the Brillouin zone. After obtaining the hole mass in each high symmetry direction, the conductivity average hole effective mass of the system is further calculated.

[0079] Figure 8 The β-(Rh x Ga 1-x ) 2y The average hole effective mass of O3. Figure 8 As shown in Figure 2, overall, Rh solid solution increases the dispersion curvature of the valence band top and reduces the effective mass of holes. Specifically, when x = 0.125, β-(Rh x Ga 1-x ) 2y The effective mass of an O3 hole is about 4.2 m e , when x=0.1875, β-(Rh x Ga 1-x ) 2y The effective mass of an O3 hole is about 2.7 m e , when x=0.25, β-(Rh x Ga 1-x ) 2y The effective mass of an O3 hole is about 2.2 m e , when x=0.3125, β-(Rh x Ga 1-x ) 2y The effective mass of an O3 hole is about 6.4 m e , when x=0.375, β-(Rh x Ga 1-x ) 2y The effective mass of an O3 hole is about 3.04 m e , when x=0.4375, β-(Rh x Ga 1-x ) 2y The effective mass of an O3 hole is about 2.95 m e , when x=0.5, β-(Rh x Ga 1-x ) 2yThe effective mass of an O3 hole is about 2.98 m e In particular, in the range of 0<x≤0.25, the average hole effective mass decreases monotonically with the increase of x. The value of β-Ga2O3 is 4.24 m e , while β-(Rh 0.25 Ga 0.25 )2O3 is only 2.22m e , which is 52.3% of the former. In the range of 0.375≤x≤0.5, β-(Rh x Ga 1-x ) 2y The average hole effective mass of O3 is 2.95 m e -3.04 m e range, which is still significantly lower than the value of β-Ga2O3. This shows that the β-(Rh x Ga 1-x ) 2y The effective hole mass of O3 is small and the dispersion relation is steep, which can avoid phenomena such as hole self-capture and help achieve p-type doping.

[0080] It should be noted that when x is 0.0625, due to β-(Rh 0.0625 Ga 0.9375 )2O3 has a larger effective hole mass, and β-(Rh 0.0625 Ga 0.9375 The effective mass of holes in )2O3 is not fully given.

[0081] Fig. 9 The β-(Rh x Ga 1-x ) 2y The band alignment diagram of O3 shows the conduction band on the top and the valence band on the bottom. The value in the middle shows the band gap. x Ga 1-x ) 2y The electron orbitals of O3, Rh and O form the valence band top of the solid solution, which is significantly higher than the 2p orbital energy level position of O. Fig. 9 As shown, compared with β-Ga2O3, β-(Rh x Ga 1-x ) 2y The valence band top of O3 rises significantly, among which β-(Rh 0.0625 Ga 0.9375 )2O3's valence band top energy level position rises by 1.81 eV. In addition, β-(Rh x Ga 1-x ) 2y The valence band top of O3 increases slowly with the increase of Rh content. 0.5 Ga0.5 )2O3 has a valence band top that is higher than that of β-(Rh 0.0625 Ga 0.9375 )2O3 increased by 0.49 eV. Based on the higher valence band top, it is easy to find suitable elements for β-(Rh x Ga 1-x ) 2y O3 is p-type doped. Combined with the smaller hole effective mass and the increased valence band top energy level, β-(Rh x Ga 1-x ) 2y O3 is expected to achieve p-type doping.

[0082] It should be noted that according to the common acceptor energy level position of β-Ga2O3, β-(Rh x Ga 1-x ) 2y When the increase in the valence band top energy level of the O3 semiconductor material is greater than or equal to 1.1 eV, p-type doping can be achieved.

[0083] Continue to refer to Fig. 9 , the band gap value of β-Ga2O3 is 4.81 eV, when x=0.0625, β-(Rh x Ga 1-x ) 2y The band gap value of O3 is 3.77 eV, and when x=0.125, β-(Rh x Ga 1-x ) 2y The band gap value of O3 is 3.86 eV, and when x=0.1875, β-(Rh x Ga 1-x ) 2y The band gap value of O3 is 3.93 eV, when x=0.25, β-(Rh x Ga 1-x ) 2y The band gap value of O3 is 4.04eV, when x=0.3125, β-(Rh x Ga 1-x ) 2y The band gap of O3 is 4.10 eV, and when x=0.375, β-(Rh x Ga 1-x ) 2y The band gap value of O3 is 3.95 eV, and when x=0.4375, β-(Rh x Ga 1-x ) 2y The band gap value of O3 is 3.88 eV, when x=0.5, β-(Rh x Ga 1-x ) 2yThe O3 band gap is 3.93 eV. Due to the simultaneous rise of the conduction band bottom, β-(Rh x Ga 1-x ) 2y O3 still has a wide band gap value and belongs to a wide bandgap semiconductor. In the studied x range, β-(Rh 0.0625 Ga 0.9375 )2O3 has the smallest band gap value, which is still 3.77 eV. This value is significantly higher than the band gap values ​​of commercial SiC and GaN. This value is also larger than that of β-(Bi x Ga 1-x )2O3 solid solution reported the largest band gap value (3.60 eV). In the range of 0<x≤0.3125, β-(Rh x Ga 1-x ) 2y The band gap of O3 increases with the increase of Rh content, among which β-(Rh 0.3125 Ga 0.6875 )2O3 reaches 4.10 eV. The ultra-wide band gap indicates that β-(Rh x Ga 1-x ) 2y O3 can be used in high-power semiconductor devices.

[0084] When β-(Rh x Ga 1-x ) 2y In the O3 semiconductor material system, when 0.125≤x≤0.25 and 0.9≤y≤1.1, refer to Figure 8 and Fig. 9 , when x = 0.125, 0.1875 and 0.25, β-(Rh 0.125 Ga 0.875 )2O3、β-(Rh 0.1825 Ga 0.8125 )2O3 and β-(Rh 0.25 Ga 0.75 )2O3, the effective mass of the hole is 4.2 m e , 2.7 m e , and 2.2 m e , the band gap values ​​are 3.86 eV, 3.93 eV and 4.04 eV respectively. That is to say, when 0.125≤x≤0.25 and 0.9≤y≤1.1, β-(Rh x Ga 1-x ) 2y O3 semiconductor materials have lower hole effective mass and wider energy band gap value, better overall performance, and are more conducive to achieving p-type doping.

[0085] It should be noted that the growth of β-(Rhx Ga 1-x ) 2y The ratio x of the number of Rh atoms in the O3 semiconductor layer to the total number of Rh and Ga atoms is 0-50 at%. The Rh-containing gallium oxide semiconductor material has a β-Ga2O3 monoclinic structure. y is in the range of 0.9≤y≤1.1. The crystal structure is characterized by XRD diffraction patterns and found that β-(Rh x Ga 1-x ) 2y O3 has characteristic peaks similar to (-201) of β-Ga2O3, and the peak position shift is about 0.5°.

[0086] It should be noted that the new semiconductor β-(Rh x Ga 1-x ) 2y The O3 system contains three elements, Rh, Ga and O, and has Rh-O and Ga-O chemical bonds. In addition, other elements may be included. When other elements are included, Rh, Ga and O are the main element components. x Ga 1-x ) 2y O3 has direct bandgap semiconductor characteristics in a wide concentration range of 0<x≤0.3125 and 0.375<x<0.5, and the bandgap value is in the range of 3.77eV-4.10 eV, which can be applied to deep ultraviolet and other optoelectronic devices. x Ga 1-x ) 2y O3 has a higher valence band top energy level and a steep valence band top dispersion relation, which facilitates p-type doping. Based on this material, complementary metal oxide semiconductor (CMOS) technology can be used for logic devices.

[0087] Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application. In the description of the embodiments of this application, unless otherwise specified, " / " means or, for example, A / B can mean A or B; "and / or" in the text is only a description of the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In addition, in the description of the embodiments of this application, "multiple" means two or more than two.

[0088] The terms "first" and "second" are used for descriptive purposes only and should not be understood as suggesting or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present application, unless otherwise specified, "multiple" means two or more.

[0089] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A semiconductor material, characterized in that: The chemical formula of the semiconductor material is β-(Rh x Ga 1-x ) 2y O3, where 0.125≤x≤0.5 and 0.9≤y≤1.

1.

2. The semiconductor material according to claim 1, characterized in that The β-(Rh x Ga 1-x ) 2y In O3, the range of x is 0.125≤x≤0.25, and the range of y is 0.9≤y≤1.

1.

3. The semiconductor material according to claim 1, characterized in that The mixing enthalpy of the semiconductor material is 0 eV / cation-0.14 eV / cation.

4. The semiconductor material according to any one of claims 1 to 3, characterized in that: The effective mass of the hole in the semiconductor material is 2 m e -7 m e .

5. The semiconductor material according to any one of claims 1 to 3, characterized in that: The difference between the valence band top energy level of the semiconductor material and that of β-Ga2O3 is greater than or equal to 1.1 eV.

6. The semiconductor material according to any one of claims 1 to 3, characterized in that: The energy band gap value of the semiconductor material is 3.77 eV-4.10 eV.

7. A semiconductor device, characterized in that: The invention comprises a substrate and a semiconductor layer, wherein the semiconductor layer is made of the semiconductor material according to any one of claims 1 to 6.

8. The semiconductor device according to claim 7, characterized in that The semiconductor layer is a p-type semiconductor layer or an n-type semiconductor layer.

9. The semiconductor device according to claim 7 or 8, characterized in that: The crystal orientation of the substrate is [010].

10. A method for preparing a semiconductor device, characterized in that: include: Substrate preheating: Place the β-Ga2O3 substrate in the growth chamber and preheat it; Growth: Introducing source materials including an O source, a Ga source, and a Rh source into the growth chamber, and growing β-(Rh x Ga 1-x ) 2y O3 semiconductor layer, wherein 0.125≤x≤0.5, and 0.9≤y≤1.

1.

11. The preparation method according to claim 10, characterized in that: The crystal orientation of the β-Ga2O3 substrate is [010].

12. The preparation method according to claim 10, characterized in that: The temperature of the Ga source introduced is 800°C-900°C, and the temperature of the Rh source introduced is ≥1500°C.

13. The preparation method according to claim 10, characterized in that: The β-(Rh x Ga 1-x ) 2y The growth temperature of O3 is 600℃-800℃.