A low-formaldehyde environmentally friendly laminate floor and preparation method thereof

Phenolic resin adhesive was prepared by the condensation reaction of cashew phenol and furfural, which solved the problem of formaldehyde pollution in laminate flooring and achieved a low-formaldehyde environmentally friendly laminate flooring with high bonding strength and good toughness.

CN118621614BActive Publication Date: 2024-11-01CHANGZHOU ZHONGLONG WOOD IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410750571.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-01
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The formaldehyde-based adhesives used in existing laminate flooring cause formaldehyde pollution, which harms human health. There is a need to develop low-formaldehyde and environmentally friendly laminate flooring.

Method used

Phenolic resin solution is prepared by polycondensation reaction using cashew phenol and furfural as raw materials. Low viscosity phenolic resin solution is prepared by reacting hydroxylated cashew phenol-terminated polyurethane prepolymer with isocyanate-terminated polyurethane prepolymer, which is used for hot-pressing lamination of decorative paper and fiberboard.

Benefits of technology

The prepared engineered flooring has high surface bonding strength, good toughness after the resin adhesive is cured, good water resistance, avoids formaldehyde pollution, and the material is a natural renewable resource, making it green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004887775030000091
    Figure BDA0004887775030000091
  • Figure BDA0004887775030000101
    Figure BDA0004887775030000101
Patent Text Reader

Abstract

The present invention relates to the technical field of laminate flooring, and specifically to a low-formaldehyde environment-friendly laminate flooring and a preparation method thereof. The present invention oxidizes cardanol to obtain hydroxylated cardanol, and uses the hydroxylated cardanol for polyurethane prepolymer end-capping to obtain cardanol end-capped polyurethane prepolymer; the cardanol end-capped polyurethane prepolymer is mixed with cardanol, and furfural is added for polycondensation reaction to obtain an impregnating resin glue; decorative paper is respectively immersed in the impregnating resin glue, and dried after being taken out to obtain impregnated decorative paper; the impregnated decorative paper is stacked on the surface of a fiberboard, and hot pressed, cut, and cured to obtain a low-formaldehyde environment-friendly laminate flooring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laminate flooring, in particular to a low-formaldehyde environment-friendly laminate flooring and a preparation method thereof. Background Art

[0002] Laminate flooring, also known as laminate flooring or composite wood flooring or impregnated paper laminated wood flooring, is a floor made of one or more layers of special paper impregnated with thermosetting resin, laid on the surface of a wood-based board substrate such as particleboard or fiberboard, with a balancing layer on the back and a wear-resistant layer on the front, bonded with adhesives, and then hot-pressed. At present, the adhesives used in laminate flooring are mainly "trialdehyde glue" (urea-formaldehyde, phenol-formaldehyde and melamine formaldehyde); among them, urea-formaldehyde resin adhesives are the most common due to their low cost and simple preparation process.

[0003] However, the extensive use of "trialdehyde glue" has caused serious formaldehyde pollution problems. Formaldehyde is extremely harmful to human health. Long-term exposure to high-concentration formaldehyde will irritate the nasal mucosa, retina, respiratory tract and liver of the human body, and will cause allergies, dizziness, fatigue, vomiting and other poisoning symptoms. In severe cases, it can cause cancer. Therefore, it is very necessary to invent a low-formaldehyde environmentally friendly laminate flooring. Summary of the invention

[0004] The object of the present invention is to provide a low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0006] Step 1:

[0007] Mixing cardanol and formic acid, stirring at 25-30°C, adding hydrogen peroxide, heating to 80-85°C, keeping the temperature for reaction for 2-3h, cooling and standing for 10-12h until stratification occurs, taking out the lower oil phase, washing with water until neutral, and obtaining epoxidized cardanol; adding sodium hydroxide solution to the epoxidized cardanol, adjusting the pH to 10-12, continuing to heat to 75-85°C, stirring for 2-3h, cooling and standing for 10-12h until stratification occurs, taking out the lower oil phase, washing with water until neutral, and obtaining hydroxylated cardanol;

[0008] Step 2:

[0009] S1: dehydrating the raw materials at 105-115° C., adding isophorone diisocyanate to polytetramethylene glycol, heating to 70-80° C., reacting for 1-2 hours, adding a catalyst dibutyltin dilaurate, and continuing the reaction for 2-4 hours to obtain an isocyanate-terminated polyurethane prepolymer; adding hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer, keeping the temperature for reaction for 1-2 hours, and obtaining a cardanol-terminated polyurethane prepolymer;

[0010] S2: Mixing cardanol-terminated polyurethane prepolymer and cardanol to obtain mixed phenol; mixing mixed dimethyl ester and dimethyl carbonate in a volume ratio of 1:1, adding mixed phenol, heating to 60-65° C., adding furfural, using sodium hydroxide as a catalyst, heating to 80-85° C., reacting for 0.5-1 h, then heating to 90-95° C., maintaining for 1-1.5 h, and after the reaction is completed, cooling and neutralizing with glacial acetic acid to pH=7 to obtain an impregnation resin glue solution with a solid content of 60-75%;

[0011] Step 3:

[0012] The decorative paper is immersed in the impregnating resin glue for 1 to 2 hours, taken out and dried to a volatile content of 5 to 8 wt.%, thereby obtaining the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot-pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate floor.

[0013] Furthermore, in step 1, the contents of the components, by weight, are 50 to 55 parts of cardanol, 4 to 6.5 parts of formic acid, and 38 to 43 parts of hydrogen peroxide.

[0014] Furthermore, in S1, isophorone diisocyanate is added to polytetramethylene oxide diol at a molar ratio of hydroxyl group to isocyanate group of 1:2.

[0015] Furthermore, in S1, the molecular weight of polytetramethylene ether glycol is 500-1000.

[0016] Furthermore, in S1, hydroxylated cardanol is added to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group (2.4-2.8):1.

[0017] Furthermore, in S2, the contents of the components in the mixed phenol are, by weight percentage, 30-40% of the cardanol-terminated polyurethane prepolymer and 60-70% of the cardanol.

[0018] Further, in S2, furfural is added to the mixed phenol at a phenol-formaldehyde ratio of 1:(1.3-1.6).

[0019] Furthermore, in step 3, the hot pressing temperature is 110-120° C., the hot pressing pressure is 8-10 MPa, and the hot pressing time is 90-100 s.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention uses furfural and cardanol as raw materials to prepare phenolic resin glue by polycondensation reaction. In order to improve the adhesion performance and toughness after curing of the phenolic resin glue, the present invention first uses polytetrahydrofuran ether diol to neutralize isophorone diisocyanate to prepare a polyurethane prepolymer, and reacts by controlling the molar ratio of hydroxyl group to isocyanate group to 1:2 to obtain an isocyanate-terminated polyurethane prepolymer; the isocyanate-terminated polyurethane prepolymer is terminated by using hydroxylated cardanol to terminate the isocyanate-terminated polyurethane prepolymer to obtain a cardanol-terminated polyurethane prepolymer; wherein the preparation method of hydroxylated cardanol is as follows: using cardanol as a raw material, hydrogen peroxide as an oxidant, and formic acid as a catalyst, oxidizing the carbon-carbon double bond of the cardanol side chain into an epoxy group, and then adjusting the pH value of the system with a sodium hydroxide solution, and further reacting with the epoxy group to obtain.

[0021] In the prior art, polyurethane-modified phenolic resin is mainly introduced into polyurethane prepolymer by reacting isocyanate group with hydroxymethyl generated in the polycondensation process of phenolic formaldehyde, and water is inevitably produced in the polycondensation process of phenolic formaldehyde, and water reacts with isocyanate group, thereby consuming isocyanate and affecting the modification effect. In the present invention, since the polyurethane prepolymer terminated with hydroxylated cardanol is added to the reaction system of cardanol and furfural, in the polycondensation process, cardanol and furfural are essentially subjected to polycondensation reaction, so the compatibility of the reaction is better; since two cardanols are contained at both ends of the prepolymer, while the reaction sites are increased, different molecular chains obtained by the polycondensation of phenolic formaldehyde are connected by flexible polyurethane molecular chains, which not only improves the crosslinking density, but also increases the toughness of the phenolic resin after curing.

[0022] In practical applications, the viscosity of the resin affects fluidity and thus affects the bonding strength. On the one hand, as the polycondensation reaction proceeds, the viscosity of the system continues to increase; on the other hand, the molecular weight and dosage of the polyurethane prepolymer also affect the viscosity. Therefore, when the molecular weight of the polyurethane prepolymer is too high, the viscosity of the synthesized phenolic resin glue is relatively large and the adhesion is reduced. Polytetrahydrofuran ether diol with a molecular weight of 500 to 1000 is selected to prepare a low-viscosity polyurethane prepolymer, and at the same time, 30 to 40% cardanol-terminated polyurethane prepolymer and 60 to 70% cardanol are mixed by weight percentage, and the phenolic resin glue finally prepared has stronger adhesion. Decorative paper is soaked in the prepared resin glue to obtain impregnated decorative paper, and is compounded with fiberboard through a hot pressing process to obtain a laminate floor. The laminate floor prepared by the present invention has a large surface bonding strength, a large toughness after the resin glue is cured, and good water resistance. The present invention uses furfural instead of formaldehyde, so there is no need to worry about formaldehyde causing harm to the human body. In addition, furfural and cardanol are both natural renewable resources, green, environmentally friendly and easily degradable. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Materials and sources used in the present invention: polytetrahydrofuran ether glycol comes from Shandong Jiaying Chemical Technology Co., Ltd.; mixed dimethyl ester is a mixture of dimethyl succinate and dimethyl glutarate, which comes from Yuanli Chemical Group Co., Ltd.; decorative paper comes from Qifeng New Materials Co., Ltd., with a gram weight of 70g / m 2 Fiberboard comes from Yingang Board Factory, Lanshan District, Linyi City, item number AL676475587267, apparent density is 900kg / m 3 .

[0025] Embodiment 1: A low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0026] Step 1:

[0027] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 25° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 80° C., the reaction was kept at this temperature for 2 h, the temperature was lowered and allowed to stand for 10 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 10, the temperature was further raised to 75° C., stirred for 2 h, the temperature was lowered and allowed to stand for 10 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0028] Step 2:

[0029] S1: Dehydrate the raw materials at 105° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 70° C., react for 1 hour, add dibutyltin dilaurate as a catalyst, and continue to react for 2 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm for 1 hour, and obtain a cardanol-terminated polyurethane prepolymer;

[0030] S2: In percentage by weight, 30% cardanol-terminated polyurethane prepolymer and 70% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 60°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 80°C, the reaction is carried out for 0.5h, and then the mixture is heated to 90°C and maintained for 1h. After the reaction is completed, the mixture is cooled and neutralized with glacial acetic acid to a pH of 7 to obtain an impregnation resin glue solution with a solid content of 75%;

[0031] Step 3:

[0032] The decorative paper is immersed in the impregnating resin glue for 1 hour, taken out and dried to a volatile content of 5wt.%, thereby obtaining the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 110°C, the hot pressing pressure is 8MPa, and the hot pressing time is 90s.

[0033] Embodiment 2: A low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0034] Step 1:

[0035] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 30° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 80° C., the reaction was kept at this temperature for 2.5 h, the temperature was lowered and allowed to stand for 11 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 11, the temperature was further raised to 80° C., the mixture was stirred for 2.5 h, the temperature was lowered and allowed to stand for 11 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0036] Step 2:

[0037] S1: Dehydrate the raw materials at 110° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 70° C., react for 1.5 hours, add dibutyltin dilaurate as a catalyst, and continue to react for 2.5 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm and react for 1.5 hours to obtain a cardanol-terminated polyurethane prepolymer;

[0038] S2: In percentage by weight, 30% cardanol-terminated polyurethane prepolymer and 70% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 65°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 85°C, the reaction is carried out for 1 hour, and then the mixture is heated to 95°C and maintained for 1.5 hours. After the reaction is completed, the mixture is cooled and neutralized with glacial acetic acid to a pH of 7 to obtain an impregnation resin glue solution with a solid content of 75%;

[0039] Step 3:

[0040] The decorative paper is immersed in the impregnating resin glue for 1.5 hours, taken out and dried to a volatile content of 5wt.%, to obtain the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 115°C, the hot pressing pressure is 9MPa, and the hot pressing time is 95s.

[0041] Embodiment 3: A low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0042] Step 1:

[0043] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 30° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 85° C., the reaction was kept at this temperature for 2.5 h, the temperature was lowered and allowed to stand for 11.5 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 12, the temperature was further raised to 85° C., stirred for 3 h, the temperature was lowered and allowed to stand for 12 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0044] Step 2:

[0045] S1: Dehydrate the raw materials at 115° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 80° C., react for 2 hours, add dibutyltin dilaurate as a catalyst, and continue to react for 4 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm and react for 2 hours to obtain a cardanol-terminated polyurethane prepolymer;

[0046] S2: In percentage by weight, 30% cardanol-terminated polyurethane prepolymer and 70% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 65°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 85°C, the reaction is carried out for 1 hour, and then the mixture is heated to 95°C and maintained for 1 hour. After the reaction is completed, the mixture is cooled and neutralized with glacial acetic acid to a pH of 7 to obtain an impregnation resin glue solution with a solid content of 75%;

[0047] Step 3:

[0048] The decorative paper is immersed in the impregnating resin glue for 2 hours, taken out and dried to a volatile content of 5wt.%, thereby obtaining the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 120°C, the hot pressing pressure is 10MPa, and the hot pressing time is 100s.

[0049] Example 4: A low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0050] Step 1:

[0051] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 30° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 80° C., the reaction was kept at this temperature for 2 h, the temperature was lowered and allowed to stand for 12 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 12, the temperature was further raised to 85° C., the mixture was stirred for 3 h, the temperature was lowered and allowed to stand for 12 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0052] Step 2:

[0053] S1: Dehydrate the raw materials at 105° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 70° C., react for 1 hour, add dibutyltin dilaurate as a catalyst, and continue to react for 2 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm for 1 hour, and obtain a cardanol-terminated polyurethane prepolymer;

[0054] S2: In terms of weight percentage, 33% cardanol-terminated polyurethane prepolymer and 67% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 65°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 80°C, the reaction is carried out for 1 hour, and then the mixture is heated to 95°C and maintained for 1.5 hours. After the reaction is completed, the mixture is cooled and neutralized to pH=7 with glacial acetic acid to obtain an impregnation resin glue solution with a solid content of 75%;

[0055] Step 3:

[0056] The decorative paper is immersed in the impregnating resin glue for 1 hour, taken out and dried to a volatile content of 5wt.%, thereby obtaining the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate floor, wherein the hot pressing temperature is 120°C, the hot pressing pressure is 10MPa, and the hot pressing time is 100s.

[0057] Embodiment 5: A low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0058] Step 1:

[0059] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 25° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 85° C., the reaction was kept at this temperature for 2.5 h, the temperature was lowered and allowed to stand for 12 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 12, the temperature was further raised to 85° C., stirred for 2 h, the temperature was lowered and allowed to stand for 10.5 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0060] Step 2:

[0061] S1: Dehydrate the raw materials at 115° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 75° C., react for 1.5 hours, add dibutyltin dilaurate as a catalyst, and continue to react for 3.5 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm and react for 1.5 hours to obtain a cardanol-terminated polyurethane prepolymer;

[0062] S2: In percentage by weight, 36% cardanol-terminated polyurethane prepolymer and 64% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 65°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 83°C, the reaction is carried out for 1 hour, and then the mixture is heated to 92°C and maintained for 1.5 hours. After the reaction is completed, the mixture is cooled and neutralized to pH=7 with glacial acetic acid to obtain an impregnation resin glue solution with a solid content of 75%;

[0063] Step 3:

[0064] The decorative paper is immersed in the impregnating resin glue for 1.5 hours, taken out and dried to a volatile content of 5wt.%, to obtain the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 115°C, the hot pressing pressure is 8.5MPa, and the hot pressing time is 95s.

[0065] Example 6: A low-formaldehyde environmentally friendly laminate floor and a preparation method thereof, comprising the following steps:

[0066] Step 1:

[0067] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 25° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 85° C., the reaction was kept at this temperature for 2 h, the temperature was lowered and allowed to stand for 12 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 11, the temperature was further raised to 85° C., stirred for 2 h, the temperature was lowered and allowed to stand for 12 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0068] Step 2:

[0069] S1: Dehydrate the raw materials at 110° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 75° C., react for 1.5 hours, add dibutyltin dilaurate as a catalyst, and continue to react for 3.5 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm for 1 hour, and obtain a cardanol-terminated polyurethane prepolymer;

[0070] S2: In terms of weight percentage, 40% cardanol-terminated polyurethane prepolymer and 60% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 60°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 85°C, the reaction is carried out for 0.5h, and then the mixture is heated to 90°C and maintained for 1h. After the reaction is completed, the mixture is cooled and neutralized to pH=7 with glacial acetic acid to obtain an impregnation resin glue solution with a solid content of 75%;

[0071] Step 3:

[0072] The decorative paper is immersed in the impregnating resin glue for 2 hours, taken out and dried to a volatile content of 5wt.%, thereby obtaining the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 115°C, the hot pressing pressure is 8MPa, and the hot pressing time is 100s.

[0073] Comparative Example 1: An isocyanate-terminated polyurethane prepolymer is used to modify the phenolic resin, and the other parameters are the same as those in Example 1.

[0074] Step 1:

[0075] S1: Dehydrate the raw materials at 105° C., add isophorone diisocyanate to polytetramethylene glycol 1000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 70° C., react for 1 hour, add catalyst dibutyltin dilaurate, and continue to react for 2 hours to obtain an isocyanate-terminated polyurethane prepolymer;

[0076] S2: Mix dimethyl ester and dimethyl carbonate in a volume ratio of 1:1, add cardanol, heat to 60°C, add furfural in a phenol-formaldehyde ratio of 1:1.6, use sodium hydroxide as a catalyst, heat to 80°C, react for 0.5h, then heat to 90°C and keep for 1h. After the reaction is completed, cool and neutralize with glacial acetic acid to pH=7, add isocyanate-terminated polyurethane prepolymer after dehydration, and react to obtain an impregnation resin glue with a solid content of 75%; wherein the weight ratio of isocyanate-terminated polyurethane prepolymer to cardanol is 3:7;

[0077] Step 2:

[0078] The decorative paper is immersed in the impregnating resin glue for 1 hour, taken out and dried to a volatile content of 5wt.%, thereby obtaining the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 110°C, the hot pressing pressure is 8MPa, and the hot pressing time is 90s.

[0079] Comparative Example 2: Polytetramethylene glycol 2000 was used instead of polytetramethylene glycol 1000, and the remaining parameters were the same as in Example 2.

[0080] Step 1:

[0081] 53 g of cardanol and 5.7 g of formic acid were mixed, stirred at 30° C., 41 g of hydrogen peroxide was added at the same time, the temperature was raised to 80° C., the reaction was kept at this temperature for 2.5 h, the temperature was lowered and allowed to stand for 11 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain epoxidized cardanol; sodium hydroxide solution was added to the epoxidized cardanol, the pH was adjusted to 11, the temperature was further raised to 80° C., the mixture was stirred for 2.5 h, the temperature was lowered and allowed to stand for 11 h until stratification occurred, the lower oil phase was removed, and the phase was washed with water until it was neutral to obtain hydroxylated cardanol;

[0082] Step 2:

[0083] S1: Dehydrate the raw materials at 110° C., add isophorone diisocyanate to polytetramethylene glycol 2000 at a molar ratio of hydroxyl group to isocyanate group of 1:2, heat to 70° C., react for 1.5 hours, add dibutyltin dilaurate as a catalyst, and continue to react for 2.5 hours to obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of 2.4:1, keep warm and react for 1.5 hours to obtain a cardanol-terminated polyurethane prepolymer;

[0084] S2: In percentage by weight, 30% cardanol-terminated polyurethane prepolymer and 70% cardanol are mixed to obtain mixed phenol; mixed dimethyl ester and dimethyl carbonate are mixed in a volume ratio of 1:1, and then added to the mixed phenol, the temperature is raised to 65°C, furfural is added in a phenol-formaldehyde ratio of 1:1.6, sodium hydroxide is used as a catalyst, the mixture is heated to 85°C, the reaction is carried out for 1 hour, and then the mixture is heated to 95°C and maintained for 1.5 hours. After the reaction is completed, the mixture is cooled and neutralized with glacial acetic acid to a pH of 7 to obtain an impregnation resin glue solution with a solid content of 75%;

[0085] Step 3:

[0086] The decorative paper is immersed in the impregnating resin glue for 1.5 hours, taken out and dried to a volatile content of 5wt.%, to obtain the impregnated decorative paper; the impregnated decorative paper is stacked on the surface of the fiberboard, hot pressed, cut and cured to obtain a low-formaldehyde environmentally friendly laminate flooring, wherein the hot pressing temperature is 115°C, the hot pressing pressure is 9MPa, and the hot pressing time is 95s.

[0087] Experiment: The laminate flooring and impregnated decorative paper prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were subjected to performance tests, and the experimental results are shown in the following table. Among them: the surface bonding strength test method of the laminate flooring is tested in accordance with GB / T 18102-2020; the water resistance test method of the impregnated decorative paper is: immerse the impregnated decorative paper in boiling water for 2 hours, and observe whether there is blistering and delamination on the surface of the decorative paper.

[0088]

[0089]

[0090] Conclusion: The data of Examples 1 to 6 and Comparative Examples 1 to 2 show that the surface bonding strength of the laminate floor prepared by the present invention is good, reaching the standard strength (greater than or equal to 1 MPa), and the decorative paper has good water resistance. The data of Example 1 and Comparative Example 1 show that the resin glue prepared by the scheme of the present invention has a higher crosslinking density after curing, stronger adhesion performance, and better tolerance to water vapor; the data of Example 2 and Comparative Example 2 show that the excessive molecular weight of polytetrahydrofuran ether glycol has an adverse effect on the curing of the resin glue, resulting in poor performance of the laminate floor and poor water resistance of the impregnated decorative paper.

[0091] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing low-aldehyde environmentally friendly impregnated decorative paper, Features: The following steps are involved: Step 1: Mix cardanol and formic acid, stir at 25-30°C, add hydrogen peroxide, heat to 80-85°C, keep warm for 2-3h, cool and stand for 10-12h until stratification occurs, remove the lower oil phase, wash with water until neutral, and obtain epoxidized cardanol; add sodium hydroxide solution to the epoxidized cardanol, adjust the pH to 10-12, continue to heat to 75-85°C, stir for 2-3h, cool and stand for 10-12h until stratification occurs, remove the lower oil phase, wash with water until neutral, and obtain hydroxylated cardanol; wherein, by weight, 50-55 parts of cardanol, 4-6.5 parts of formic acid, and 38-43 parts of hydrogen peroxide; Step 2: S1: Dehydrate the raw materials at 105-115°C, add isophorone diisocyanate to polytetramethylene glycol, heat to 70-80°C, react for 1-2 hours, add dibutyltin dilaurate as a catalyst, continue to react for 2-4 hours, and obtain an isocyanate-terminated polyurethane prepolymer; add hydroxylated cardanol to the isocyanate-terminated polyurethane prepolymer, keep warm and react for 1-2 hours, and obtain a cardanol-terminated polyurethane prepolymer; wherein isophorone diisocyanate is added to polytetramethylene glycol at a molar ratio of hydroxyl group to isocyanate group of 1:2; the molecular weight of polytetramethylene glycol is 500-1000; hydroxylated cardanol is added to the isocyanate-terminated polyurethane prepolymer at a molar ratio of hydroxyl group to isocyanate group of (2.4-2.8):1; S2: Mixing cardanol-terminated polyurethane prepolymer and cardanol to obtain mixed phenol; mixing mixed acid dimethyl ester and dimethyl carbonate in a volume ratio of 1:1, adding the mixed phenol, heating to 60-65°C, adding furfural, using sodium hydroxide as a catalyst, heating to 80-85°C, reacting for 0.5-1h, and then heating to 90-95°C, maintaining for 1-1.5h, and after the reaction is completed, cooling and neutralizing with glacial acetic acid to pH=7 to obtain an impregnation resin glue; wherein the content of each component in the mixed phenol is, by weight percentage, 30-40% cardanol-terminated polyurethane prepolymer and 60-70% cardanol; furfural is added to the mixed phenol in a phenol-formaldehyde ratio of 1:(1.3-1.6); the mixed acid dimethyl ester is a mixture of dimethyl succinate and dimethyl glutarate; Step 3: Immerse the decorative paper in the impregnating resin glue solution for 1-2 hours, take it out and dry it until the volatile content is 5-8wt.%, so as to obtain low-formaldehyde environmentally friendly impregnated decorative paper.

2. A method for preparing a low-formaldehyde environmentally friendly impregnated decorative paper according to claim 1, Features: In S2, the solid content of the impregnating resin solution is 60~75%.

3. A low-formaldehyde, environmentally friendly impregnated decorative paper prepared by the preparation method according to any one of claims 1 to 2.

4. A low-formaldehyde, environmentally friendly laminate flooring prepared from the low-formaldehyde, environmentally friendly impregnated decorative paper as claimed in claim 3, Features: The low-formaldehyde environmentally friendly impregnated decorative paper is stacked on the surface of the fiberboard, and the low-formaldehyde environmentally friendly laminate flooring is obtained by hot pressing, slitting and curing; wherein the hot pressing temperature is 110-120°C, the hot pressing pressure is 8-10MPa, and the hot pressing time is 90-100s.