A method for constructing wheel-rail three-dimensional wear map considering ambient temperature and material properties

By constructing a three-dimensional wear diagram of wheel and rails that consider ambient temperature and material characteristics, the problem that the existing two-dimensional wear model cannot effectively reflect the impact of ambient temperature is solved, and more accurate wheel and rail wear prediction is achieved, which is suitable for wheel wear under different conditions. analyze.

CN118628666BActive Publication Date: 2024-11-01SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088627.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-01
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing wheel and rail wear model only considers the two-dimensional function relationship between material wear rate and energy dissipation work, and fails to effectively reflect the impact of ambient temperature on the wear behavior of wheel and rail material, resulting in insufficient wear prediction.

Method used

The three-dimensional wear graph construction method considering ambient temperature and material characteristics was adopted, and the functional relationship between the wheel wear rate and the dissipation energy of the wheel rail contact spot per unit area was constructed through rolling friction wear experiments. The three-dimensional wear graph was obtained by fitting the MATLAB software, and combined with SIMPACK Multi-body dynamics simulation software performs wheel and rail contact parameters analysis to calculate the wheel and rail wear depth and wear profile.

Benefits of technology

It realizes a more accurate reflection of the impact of ambient temperature and material hardness on the wear rate of the wheel rail, and is suitable for wheel wear prediction under different ambient temperature and material hardness matching conditions, improving the accuracy and applicability of wear prediction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118628666B_ABST
    Figure CN118628666B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of wheel-rail material friction and wear, and provides a method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties, comprising: 1) obtaining the friction and wear performance of wheel materials under different ambient temperatures and different wheel-rail hardness ratios based on wheel-rail rolling friction and wear experiments under different contact parameters, and constructing a series of functional relationships between wheel wear rate and dissipated energy per unit area of ​​wheel-rail contact patch under different ambient temperatures and wheel-rail hardness ratios; 2) performing function fitting on experimental data, and respectively obtaining a wheel three-dimensional wear map taking into account ambient temperature and a wheel three-dimensional wear map taking into account wheel-rail material hardness ratio; 3) selecting a two-dimensional reference wear map and constructing a wheel three-dimensional wear map taking into account ambient temperature and material hardness ratio through normalization processing. Based on the constructed wear map, the present invention can better predict the wheel wear behavior under different ambient temperatures and different material property conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wheel-rail material friction and wear, and provides a method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties. Background Art

[0002] As railway transportation gradually becomes high-speed and heavy-loaded, the friction and wear behavior of wheel and rail materials, as one of the most core components to ensure the safety of train operation, will become more and more serious, which poses a challenge to the wear resistance, service life and safety and reliability of wheel and rail materials. At the same time, the wheel and rail system serves in a relatively open environment, and the complex and changeable operating conditions will also affect the friction and wear behavior of wheel and rail materials.

[0003] The wear model is a research method commonly used in tribological systems. It can comprehensively and intuitively integrate various tribological information of friction pair materials. In essence, it is a comprehensive information database containing wear rate data and wear surface morphology data, which provides a convenient data reference for the wear and life prediction research of friction pair materials. Tγ / A - Wear rate model is the two most commonly used wear models for wheel-rail system. Tγ / A -The wear rate model is based on a large number of wheel-rail friction and wear test results in the laboratory. The continuity of its wear rate input value can more accurately study the friction and wear behavior of the wheel-rail system. Tγ / A -The wear rate model only considers the material wear rate and energy dissipation work ( Tγ / A ), but different wheel-rail material properties and external ambient temperature will also greatly affect the wear behavior of wheel-rail materials. Therefore, it is necessary to carry out a three-dimensional wear model that considers the wheel-rail material properties (internal factors) and ambient temperature (external factors), and further draw a three-dimensional wear diagram that reflects the wheel-rail wear rate with energy dissipation work, material hardness and ambient temperature. At the same time, based on the constructed three-dimensional wear model, wheel-rail wear prediction that considers both ambient temperature and material properties can be further carried out. Summary of the invention

[0004] The present invention provides a method for constructing a three-dimensional wheel-rail wear map taking into account ambient temperature and material properties, which can solve the problem that the existing two-dimensional wear map cannot reflect the internal factors (material properties) and external factors (ambient temperature) of the wheel-rail service system affecting the wear behavior of the wheel-rail material involved in actual engineering applications.

[0005] A method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties according to the present invention comprises the following steps:

[0006] 1) Based on the wheel-rail rolling friction and wear experiments under different contact parameters, the friction and wear properties of the wheel material under different ambient temperatures and different wheel-rail hardness ratios were obtained, and the functional relationship between the wheel wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios was established;

[0007] 2) MATLAB software was used to fit the experimental data to obtain the three-dimensional wear map of the wheel considering the ambient temperature and the three-dimensional wear map of the wheel considering the hardness ratio of the wheel and rail materials;

[0008] 3) A two-dimensional reference wear map is selected and a three-dimensional wheel wear map is constructed by normalization, which takes into account both ambient temperature and material hardness ratio.

[0009] As a preferred embodiment, in step 1), the functional relationship between the wheel wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios is: Tγ / A - Wear rate function, where the wheel wear rate is the wear amount divided by the running distance and the wheel-rail contact area A The product of: the energy dissipated per unit area of ​​wheel-rail contact spot Tγ / A is the tangential force at the wheel-rail interface T and creep rate γ The product of A ; Tγ / A -The wear rate function relationship is divided into two areas, I and II, according to the slope of the curve.

[0010] As a preferred method, in step 2), MATLAB software is used to analyze the temperature at different ambient temperatures using the ambient temperature as the independent variable. T γ / A -The slope of the wear rate curve in regions Ⅰ and Ⅱ and the horizontal coordinate of the intersection of regions Ⅰ and Ⅱ are fitted to obtain the value considering the ambient temperature. Tt The wheel wear model is based on the consideration of ambient temperature Tt The wheel wear model is constructed based on the wear rate, T γ / A and ambient temperature Tt The three-dimensional wear of the wheel considering the ambient temperature is the coordinate parameter Figure 3 DMAP ( Tt );

[0011] Under different wheel-rail hardness ratio conditions Tγ / A -Function fitting is performed on the slopes of the wear rate curve in regions Ⅰ and Ⅱ to obtain the hardness ratio of the material considered. Hv The wheel wear model is based on the consideration of the material hardness ratio Hv The wheel wear model is constructed based on the wear rate, Tγ / A Three-dimensional wheel wear considering wheel-rail material hardness ratio with wheel-rail hardness ratio as coordinate parameters Figure 3 DMAP ( Hv ) ; by wheel three-dimensional wear Figure 3 DMAP ( Tt ) and wheel 3D wear Figure 3 DMAP ( Hv ) to obtain the two-dimensional wear of the wheel under a certain ambient temperature or material hardness ratio Figure 2 DMAP ( Tt ) and 2DMAP ( Hv ).

[0012] As a preference, in step 2), the ambient temperature is considered Tt The fitting functions of the slopes of the line segments in regions Ⅰ and Ⅱ in the wheel wear model are and , the horizontal and vertical coordinate fitting functions of the junction point of regions Ⅰ and Ⅱ are , , considering the ambient temperature Tt The wheel wear model is as follows:

[0013] Region I: The wear rate is ;

[0014] II Area: The wear rate is .

[0015] As a preferred embodiment, in step 2), the slope fitting functions of the line segments in regions Ⅰ and Ⅱ in the wheel wear model considering the material hardness ratio are respectively and , the horizontal coordinate of the junction point of regions Ⅰ and Ⅱ x 2 Wheels at an ambient temperature of 20°C Tγ / A -Intersection value of the wear rate function relationship x 2 =16.657; Considering the material hardness ratio Hv The wheel wear model is as follows:

[0016] Region I: The wear rate is ;

[0017] II Area: The wear rate is .

[0018] As a preferred method, in step 3), the same ambient temperature is selected Tt 1 And material hardness ratio Hv 1 Two-dimensional wheel wear under conditions Figure 2 DMAP ( Tt 1 ) and 2DMAP ( Hv 1 ), and the two-dimensional wear of the two wheels was calculated using MATLAB software. Figure 2 DMAP ( Tt 1 ) and 2DMAP ( Hv 1 ) to construct the benchmark two-dimensional wear Figure 2 DMAP(S); will take into account the ambient temperature Tt Wheel wear model considering material hardness ratio Hv The wheel wear model is normalized with the benchmark two-dimensional wear Figure 2 DMAP(S) is used to fit the wheel wear model that takes both ambient temperature and material hardness ratio into consideration. Based on the wheel wear model that takes both ambient temperature and material hardness ratio into consideration, the variables involving both ambient temperature and material hardness ratio are derived. Tt ·e 4.9177·Hv , constructed based on wear rate, Tγ / A and Tt ·e 4.9177·Hv Three-dimensional wheel wear considering ambient temperature and wheel-rail material hardness ratio as coordinate parameters Figure 3 DMAP( Tt , Hv ).

[0019] As a preference, in step 3), the same ambient temperature Tt 1 And material hardness ratio Hv 1 Take 20℃ and 1.08 respectively; consider the wheel wear of ambient temperature and material hardness ratio at the same time Figure I , Ⅱ The slopes of the two regions are The horizontal coordinate of the intersection point of the two regions is ; Three-dimensional wheel wear considering both ambient temperature and material hardness ratio Figure 3 DMAP( Tt , Hv )’s wheel wear model is as follows:

[0020] Region I: The wear rate is ;

[0021] II Area: The wear rate is .

[0022] The present invention provides a wheel wear prediction method, which adopts the above-mentioned wheel-rail three-dimensional wear map construction method considering ambient temperature and material properties to construct a three-dimensional wear map, and comprises the following steps:

[0023] a) Use SIMPACK multi-body dynamics simulation software to establish a vehicle-track coupled multi-body dynamics model, and analyze and calculate the wheel-rail contact parameters;

[0024] b) Based on the wheel-rail contact parameters, the Hertz contact theory and FASTSIM theory are used to calculate the wheel-rail contact spot, creep force and stick-slip area distribution at each moment during the wheel-rail service process;

[0025] c) Combined with the three-dimensional wheel wear map that takes into account the ambient temperature and material hardness ratio, the wear distribution on the contact spot is calculated, and finally the wheel wear depth and wear profile are obtained. Tγ / A The wear rate model is obtained based on the test data of CL60 wheel and U71Mn rail matching at a certain temperature. Substituting this wear model into the above wheel wear prediction process can predict the corresponding wheel wear depth and wear profile. However, the ambient temperature and the wheel-rail material hardness ratio are inversely proportional to the material wear rate, that is, the wheel wear should be different at different ambient temperatures and different material hardness matching. Therefore, there are two disadvantages in the applicability of this wear model: i) It is not suitable for wear prediction of other wheel-rail hardness matching materials. If necessary, it is necessary to use other hardness matching wheel-rail material pairs to conduct friction and wear tests to obtain the corresponding Tγ / A Wear rate model; ii) When the wheel-rail material is matched with CL60-U71Mn, the influence of ambient temperature on the predicted value of wheel wear cannot be reflected;

[0026] The three-dimensional wheel wear map (model) that takes into account both the ambient temperature and the material hardness ratio can solve the above two drawbacks: i) by inputting the ambient temperature and the wheel-rail material hardness ratio values, the corresponding two-dimensional wear model under a certain ambient temperature and a certain material hardness ratio can be output, thereby making a more accurate prediction of the wheel wear under this condition; ii) under the same wheel-rail hardness matching condition, the corresponding two-dimensional wear model under different ambient temperatures can be obtained, thereby making a more accurate prediction of the wheel wear depth and wear profile under different ambient temperatures.

[0027] The beneficial effects of the present invention are as follows: the present invention provides a method for constructing a wheel-rail three-dimensional wear map taking into account the ambient temperature and material properties. Compared with the existing commonly used wheel-rail wear map, the wheel-rail three-dimensional wear map can simultaneously reflect the influence of ambient temperature and material hardness on the wheel-rail wear rate, and can directly obtain the wheel under specific ambient temperature and specific material property conditions. Tγ / AThe wear rate model is constructed, and based on the constructed three-dimensional wear map, the wheel-rail wear prediction method is used to predict the wheel-rail wear under the conditions of ambient temperature and material hardness ratio, which has important engineering application value and theoretical guiding significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is an overall flow chart of a method for constructing a wheel-rail three-dimensional wear map and a wear prediction method considering ambient temperature and material properties;

[0029] Figure 2 This is a simplified structural diagram of the wheel-rail rolling contact friction and wear testing machine;

[0030] Figure 3 This is a schematic diagram of the cryogenic chamber structure;

[0031] Figure 4 This is a sampling diagram for small-scale wheel-rail specimens;

[0032] In the figure, 1 is the driving motor, 2 is the torque sensor, 3 is the main shaft, 4 is the upper sample (wheel sample), 5 is the auxiliary shaft servo motor, 6 is the auxiliary shaft, 7 is the vertical load loading device, 8 is the lower sample (rail sample), 9 is the copper tube, 10 is the low temperature cavity, 11 is the wheel, and 12 is the rail;

[0033] Figure 5 The three-dimensional wear of the wheel considering the ambient temperature is calculated based on experimental data. Figure 3 DMAP( Tt );

[0034] Figure 6 Three-dimensional wheel wear considering material hardness ratio based on experimental data Figure 3 DMAP( Hv );

[0035] Figure 7 Two-dimensional wear of wheels at an ambient temperature of 20°C and a material hardness ratio of 0.8 Figure 2 DMAP (20°C, 0.8);

[0036] Figure 8 The three-dimensional wear of the wheel considering the ambient temperature and material hardness ratio based on experimental data Figure 3 DMAP( Tt , Hv );

[0037] Fig. 9 According to the most commonly used Tγ / A Schematic diagram of the corresponding wear profile obtained from the wear rate model;

[0038] Fig.10The wheel wear depth distribution diagram for the ambient temperature range of -40~40℃ and the wheel-rail hardness ratio range of 0.8~1.4 obtained by predicting and calculating the wheel three-dimensional wear model that considers both the ambient temperature and the material hardness ratio;

[0039] Fig.11 The wheel wear volume distribution diagram in the ambient temperature range of -40~40℃ and the wheel-rail hardness ratio range of 0.8~1.4 obtained by predicting the wheel three-dimensional wear model that considers both ambient temperature and material hardness ratio. DETAILED DESCRIPTION

[0040] In order to further understand the content of the present invention, the present invention is described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the embodiments are only for explaining the present invention and are not intended to limit it.

[0041] Example:

[0042] like Figure 1 As shown, this embodiment provides a method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties, which includes the following steps:

[0043] Step 1) Based on the wheel-rail rolling friction and wear experiments under different contact parameters, the friction and wear performance of the wheel material under different ambient temperatures and different material properties (the material property in this embodiment is the wheel-rail hardness ratio) is obtained, and the functional relationship between the wheel wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios is established;

[0044] All wheel-rail rolling contact tests were carried out on Figure 2 The wheel-rail rolling contact test machine shown in the figure is equipped with a low-temperature environment chamber to simulate different ambient temperatures, such as Figure 3 The wheel and rail disc specimens are taken from the wheel flange and rail head respectively. Figure 4 As shown in the figure, the specimen size is processed into a diameter of 60 mm according to the structure of the testing machine, the wheel specimen is stepped, and the contact width of the wheel-rail specimen is 5 mm.

[0045] The functional relationship between the wheel wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios is: Tγ / A - Wear rate function, where the wheel wear rate is the wear amount divided by the running distance and the wheel-rail contact area A The product of: the energy dissipated per unit area of ​​wheel-rail contact spot Tγ / A is the tangential force at the wheel-rail interface T and creep rate γ The product of A .

[0046] To construct a functional relationship between wheel wear rate and dissipated energy per unit area of ​​wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios ( Tγ / A - wear rate), different Tγ / A Value, where slip γ The tangential force can be calculated by controlling the speed difference of the wheel-rail specimen and combining the vertical load between the wheel and rail and the friction coefficient value during the experiment. T This embodiment is based on Tγ / A 0~60 N / mm 2 The wear rate statistics are conducted in a wide range of areas with rail / wheel hardness ratios of 0.8~1.3 and ambient temperatures of -40~20℃. The obtained Tγ / A-wear rate function relationship can be divided into two regions, I and II, according to the slope of the curve.

[0047] Step 2) Use MATLAB software to perform function fitting on the experimental data to obtain a three-dimensional wheel wear map considering the ambient temperature and a three-dimensional wheel wear map considering the wheel-rail material hardness ratio;

[0048] Using MATLAB software to take ambient temperature as the independent variable, the Tγ / A -The slope of the wear rate curve in regions Ⅰ and Ⅱ and the horizontal coordinate of the intersection of regions Ⅰ and Ⅱ are fitted to obtain the value considering the ambient temperature. Tt The wheel wear model is based on considering the ambient temperature Tt The wheel wear model is constructed based on the wear rate, Tγ / A and ambient temperature Tt The three-dimensional wear of the wheel considering the ambient temperature is the coordinate parameter Figure 3 DMAP ( Tt );

[0049] Under different wheel-rail hardness ratio conditions Tγ / A -Function fitting is performed on the slopes of the wear rate curve in regions Ⅰ and Ⅱ to obtain the hardness ratio of the material considered. Hv The wheel wear model is based on the consideration of the material hardness ratio Hv The wheel wear model is constructed based on the wear rate, Tγ / A Three-dimensional wheel wear considering wheel-rail material hardness ratio with wheel-rail hardness ratio as coordinate parameters Figure 3 DMAP ( Hv ) ; by wheel three-dimensional wear Figure 3 DMAP ( Tt ) and wheel 3D wear Figure 3 DMAP ( Hv ) to obtain the two-dimensional wear of the wheel under a certain ambient temperature or material hardness ratio Figure 2 DMAP ( Tt ) and 2DMAP ( Hv ).

[0050] Ambient temperature at -40, 0, 20°C Tγ / A -The wheel wear rate model data is shown in Table 1 below. The MATLAB software is used to analyze the wheel wear rate under different ambient temperatures with ambient temperature as the independent variable. Tγ / A -The slope of the wear rate curve in regions Ⅰ and Ⅱ and the horizontal coordinate of the intersection of regions Ⅰ and Ⅱ are linearly regressed to obtain the value considering the ambient temperature. Tt The wheel wear model is shown in Table 2, where the slope fitting functions of the line segments in regions Ⅰ and Ⅱ are respectively and , the horizontal and vertical coordinate fitting functions of the junction point of regions Ⅰ and Ⅱ are , Based on the consideration of ambient temperature Tt The wheel wear model is constructed based on the wear rate, Tγ / A and ambient temperature Tt The three-dimensional wear of the wheel considering the ambient temperature is the coordinate parameter Figure 3 DMAP ( Tt ),like Figure 5 As shown;

[0051] Table 1 Different ambient temperatures Tt Experimental data of wheel wear model

[0052]

[0053] Table 2 Considering ambient temperature Tt Wheel wear model

[0054]

[0055] The existing literature on the hardness matching of different wheel-rail materials Tγ / A - The wheel wear rate model data is shown in Table 3 below. Tγ / A -The slopes of the wear rate curves in regions Ⅰ and Ⅱ are fitted by least squares to obtain the hardness ratio of the material considered. Hv The wheel wear model is shown in Table 4, where the slope fitting functions of the line segments in regions Ⅰ and Ⅱ are and , the horizontal coordinate of the junction point of regions Ⅰ and Ⅱ x 2 The wheel in Table 1 at an ambient temperature of 20°C Tγ / A -Intersection value of the wear rate function relationship x 2 =16.657 (the existing hardness ratio data are all experimental results at an ambient temperature of 20°C). Hv The wheel wear model is constructed based on the wear rate, Tγ / AThree-dimensional wheel wear considering wheel-rail material hardness ratio with wheel-rail hardness ratio as coordinate parameters Figure 3 DMAP ( Hv ),like Figure 6 As shown;

[0056] Table 3 Different wheel-rail hardness ratios Hv Experimental data of wheel wear model

[0057]

[0058] Table 4 Considering ambient temperature Tt Wheel wear model

[0059]

[0060] 3D wear of wheels Figure 3 DMAP ( Tt ) and the three-dimensional wear of the wheel Figure 3 DMAP ( Hv ) can obtain the two-dimensional wear of the wheel under a certain ambient temperature and a certain material hardness ratio. Figure 2 DMAP ( Tt , Hv ),like Figure 7 The figure shows the two-dimensional wear of the wheel when the ambient temperature is 20°C and the material hardness ratio is 0.8. Figure 2 DMAP (20°C, 0.8).

[0061] Step 3) Select the two-dimensional reference wear map and construct a three-dimensional wheel wear map that takes into account both the ambient temperature and the material hardness ratio through normalization.

[0062] Select the same ambient temperature ( Tt 1 ) and material hardness ratio ( Hv 1 ) condition. Figure 2 DMAP( Tt 1 ) and 2DMAP ( Hv 1 ), and the two-dimensional wear of the two wheels was calculated using MATLAB software. Figure 2 DMAP ( Tt 1 ) and 2DMAP ( Hv 1 ) to construct the benchmark two-dimensional wear Figure 2 DMAP(S); will take into account the ambient temperature Tt Wheel wear model considering material hardness ratio Hv The wheel wear model is normalized with the benchmark two-dimensional wear Figure 2 DMAP(S) is used to fit the wheel wear model that takes both ambient temperature and material hardness ratio into consideration. Based on the wheel wear model that takes both ambient temperature and material hardness ratio into consideration, the variables involving both ambient temperature and material hardness ratio are derived. Tt ·e 4.9177·Hv , constructed based on wear rate, Tγ / A and Tt ·e 4.9177·Hv Three-dimensional wheel wear considering ambient temperature and wheel-rail material hardness ratio as coordinate parameters Figure 3 DMAP( Tt , Hv ),like Figure 8 shown.

[0063] Same ambient temperature Tt 1 And material hardness ratio Hv 1 Take 20℃ and 1.08 respectively; consider the wheel wear of ambient temperature and material hardness ratio at the same time Figure I , Ⅱ The slopes of the two regions are The horizontal coordinate of the intersection point of the two regions is ; Three-dimensional wheel wear considering both ambient temperature and material hardness ratio Figure 3 DMAP( Tt , Hv ) is shown in Table 5.

[0064] Table 5 Considering the ambient temperature Tt And material hardness ratio Hv Wheel wear model

[0065]

[0066] Furthermore, the Hertz contact simulation criterion is used in the small-scale test, that is, the ratio of the long and short semi-axes of the elliptical spot in the contact area between the wheel and rail under laboratory conditions and the maximum contact stress are the same as those in the field, so that the actual working conditions of the wheel-rail friction pair in the field can be approximately simulated. The friction and wear data of the materials obtained in the test are used to establish the Tγ / A The wear model can further accurately and effectively predict the full-size wheel wear on site. Among them, the Hertz contact simulation criterion must satisfy the following formula 1:

[0067] ;

[0068] In formula (1): σ max is the maximum contact stress; F is the vertical force applied to the wheel-rail interface; μ 1 , μ 2 is the Poisson's ratio of the wheel / rail material; E 1 , E 2 is the elastic modulus of the wheel / rail material; L is the contact width of the wheel-rail specimen (the contact width of the specimen in the two testing machines L =5 mm); ρ is the curvature of the contact point between the wheel specimen and the rail specimen; Σρ It is the sum of the principal curvatures of the wheel specimen and the rail specimen.

[0069] ;

[0070] In formula (2): R 11 , R 21 is the transverse curve radius of the wheel-rail specimen. R 11 , R 21 is ∞; R 12 , R 22 is the longitudinal curve radius of the wheel-rail specimen.

[0071] When the Poisson's ratio and elastic modulus of the wheel-rail specimen are 0.3 and 2.06×10 5 MPa, maximum line contact stress It can be calculated according to the following formula (3):

[0072] ;

[0073] like Figure 1 As shown, this embodiment provides a wheel wear prediction method, which uses the above-mentioned wheel-rail three-dimensional wear map construction method considering ambient temperature and material properties to construct a three-dimensional wear map, and includes the following steps:

[0074] a) Use SIMPACK multi-body dynamics simulation software to establish a vehicle-track coupled multi-body dynamics model, and analyze and calculate the wheel-rail contact parameters;

[0075] b) Based on the wheel-rail contact parameters, the Hertz contact theory and FASTSIM theory are used to calculate the wheel-rail contact spot, creep force and stick-slip area distribution at each moment during the wheel-rail service process;

[0076] The Hertz contact theory is used to calculate the shape of the contact spot and the distribution of the contact pressure. The obtained elliptical contact spot is discretized into square units with a side length of 0.1 mm. xThe direction is longitudinal (wheel rolling direction), y The normal force is lateral (perpendicular to the rolling direction of the wheel). The specific calculation formula is as follows:

[0077] ;

[0078] In formula 4: N is the normal load; a , b are the major and minor semi-axes of the wheel-rail elliptical contact patch respectively.

[0079] The Kalker simplified theory FASTSIM algorithm is used to solve the wheel-rail tangential contact problem. Based on the force-displacement linear relationship of the generalized elastic theory and the integration of the elastic force on the contact area, the displacement along the contact area is determined. x , y Wheel-rail creep force in the direction and creep torque M A linear function of .

[0080] ;

[0081] In formula (5): C 11 is the longitudinal creep coefficient (quantifying the tangential force generated by unit longitudinal creep), C 22 is the transverse creep coefficient (quantifying the tangential force generated by unit transverse creep), C 23 is the transverse creep-rotational creep coefficient (quantifies the coupling effect of transverse creep and rotational creep), C 33 is the rotation creep coefficient (quantifying the torque generated by unit rotation creep), G is the shear modulus of the material, Denote the longitudinal, lateral and spin creep rates respectively. By using the longitudinal and lateral compliance coefficients , which simplifies the complex expression derived from general elastic theory. The compliance coefficient depends on the creep rate and spin coefficient of the linear theory. Wheel creep force , Rail creep force and wheel-rail contact spot displacement The relationship is as shown in formula (6):

[0082] ;

[0083] In formula (6): u w , u r are the final position and initial position of the contact spot, respectively.

[0084] By integrating the entire wheel-rail contact patch area, the wheel-rail creep force within the contact patch can be obtained: , for:

[0085] ;

[0086] In formula (7): f Tx is the longitudinal tangential force, f Ty is the transverse tangential force, L x is the longitudinal flexibility coefficient, L y1 is the lateral flexibility coefficient, L y2 is the rotational flexibility coefficient.

[0087] Flexibility coefficient L The calculation formula is:

[0088] ;

[0089] c) The wear distribution on the contact spot is calculated based on the three-dimensional wear map of the wheel that takes into account the ambient temperature and material hardness ratio, and finally the wheel wear depth and wear profile are obtained.

[0090] Based on the Hertz contact theory and FASTSIM theory, the wheel-rail contact spot, creep force and stick-slip area distribution at each moment are calculated, and the wear distribution on the contact spot (i.e., contact spot wear depth distribution) is calculated in combination with the wheel three-dimensional wear model, and finally the wheel wear depth and wear profile are obtained. The specific wear prediction calculation formula is as follows:

[0091] When calculating the wheel-rail tangential force in the FASTSIM algorithm, it is assumed that the displacement μ and surface stress p and flexibility coefficient L Relevant, namely:

[0092] ;

[0093] In formula (10): v x is the longitudinal sliding velocity between the wheel and rail at the unit, v y is the lateral sliding velocity between the wheel and rail at the unit, v v is the wheel linear speed, is the longitudinal creep rate, is the lateral creep rate, φx is the longitudinal spin creep rate, φy is the transverse spin creep rate, is the longitudinal elastic displacement, is the lateral elastic displacement, is the longitudinal elastic sliding vector, is the lateral elastic sliding vector.

[0094] Rewrite formula (10) into vector form and perform dimensional processing, that is:

[0095] ;

[0096] In formula (11): w is the total sliding vector, s is the rigid sliding vector, is the elastic sliding vector.

[0097] By integrating equation (11), the tangential stress of each unit in the contact patch can be calculated: Assuming that the FASTSIM algorithm satisfies Coulomb's friction law, the limiting tangential force of the unit in the contact patch can be obtained for:

[0098] ;

[0099] When the tangential force is less than the tangential force limit value, that is, When , the unit is in the adhesion area and there is no sliding; when When the wheel is in the sliding area, the corrected tangential force :

[0100] ;

[0101] In formula (13), P x ( x , y ) is the longitudinal tangential stress in the unit, P y ( x , y ) is the transverse tangential stress in the unit.

[0102] Since the rigid sliding amount in the contact patch is much larger than the elastic deformation, the effect of elastic sliding can be ignored in the calculation. Therefore, the sliding velocity in the contact patch can be simplified as:

[0103] ;

[0104] The creep rate of each unit in the contact patch can be expressed as:

[0105] ;

[0106] Sliding area of ​​the unit Tγ / AIt is equal to the product of the element tangential stress and the element total creep rate, which is used as the input of the wear model:

[0107] ;

[0108] Wear depth of each sliding unit in the contact patch for:

[0109] ;

[0110] In formula (18): K is the wear rate, given by Tγ / A The wear model is calculated to obtain is the density of the wheel material, is the relative sliding displacement of the unit on the contact spot.

[0111] After calculating the wear depth in each unit, the wear depth of the contact spot is superimposed in the longitudinal direction, and the wear amount of a single section can be obtained by the integration method:

[0112] ;

[0113] According to the lateral position of the wheel contact point, the contact spot wear is superimposed to obtain the wheel wear under this working condition. W ( y ):

[0114] ;

[0115] In formula (20): R is the nominal rolling circle radius of the wheel, and are the start and end positions of the calculation, s 1 is the sampling point interval, l is the lateral contact length.

[0116] In the actual train operation process, as the train mileage increases, the shape of the wheel will change continuously. However, in numerical simulation, this continuous change of the profile is difficult to simulate accurately. Therefore, this embodiment assumes that the wheel shape remains unchanged during a single calculation process, and after each iteration process is completed, the wheel shape is updated according to a pre-set update scheme. This can simplify the simulation process and reflect the changes in the wheel shape to a certain extent. The profile update basis selected in this embodiment is that the vehicle mileage reaches a threshold. The tread data is smoothed 3 times at 5 points to obtain the worn wheel tread and perform the next simulation.

[0117] Furthermore, through wheel wear prediction calculation, the applicability of the three-dimensional wheel wear model that takes into account both ambient temperature and material hardness ratio is simulated and verified, specifically:

[0118] The most commonly used Tγ / A The wear rate model is based on the test data of CL60 wheel and U71Mn rail matching at a certain temperature. Substituting this wear model into the above wheel wear prediction method, the corresponding wear profile can be predicted as follows: Fig. 9 As shown in Figure 2, the wear depth and wear volume are 0.02972 mm and 3158.4906·10 -9 mm 3 However, the ambient temperature and wheel-rail material hardness ratio are inversely proportional to the material wear rate, that is, the wheel wear should be different when the ambient temperature and material hardness are different. Therefore, the applicability of this wear model has two disadvantages: i) It is not suitable for the wear prediction of other wheel-rail hardness matching materials. If necessary, it is necessary to use other hardness matching wheel-rail material pairs to conduct friction and wear tests to obtain the corresponding Tγ / A Wear rate model; ii) When the wheel-rail material is matched with CL60-U71Mn, the influence of ambient temperature on the predicted value of wheel wear cannot be reflected;

[0119] The three-dimensional wheel wear model constructed in this embodiment that takes into account both the ambient temperature and the material hardness ratio can solve the above two drawbacks: i) by inputting the ambient temperature and the wheel-rail material hardness ratio values, the corresponding two-dimensional wear model under a certain ambient temperature and a certain material hardness ratio condition can be output, thereby making a more accurate prediction of the wheel wear under this condition; ii) under the same wheel-rail hardness matching condition, the corresponding two-dimensional wear model under different ambient temperatures can be obtained, thereby making a more accurate prediction of the wheel wear depth and wear profile under different ambient temperatures.

[0120] The method for constructing a wheel-rail three-dimensional wear map considering ambient temperature and material properties can not only construct a wheel three-dimensional wear map and predict wheel wear that simultaneously considers ambient temperature and material hardness ratio, but also construct a three-dimensional wear map of a wheel pair (rail) and predict rail wear in a wheel-rail rolling contact experiment. The method for constructing a rail three-dimensional wear map and the method for predicting rail wear are consistent with the method for constructing a wheel three-dimensional wear map and the method for predicting wheel wear, with the only difference being that in step 1), the friction and wear properties of the rail material under different ambient temperatures and different wheel-rail hardness ratios are obtained based on the wheel-rail rolling friction and wear experiment under different contact parameters, and the functional relationship between the rail wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios is constructed. The construction of the relevant rail wear model and the prediction of rail wear in the subsequent steps are based on the functional relationship between the rail wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under the conditions of the series of different ambient temperatures and wheel-rail hardness ratios.

[0121] In this embodiment, the three-dimensional wheel wear model that considers both the ambient temperature and the material hardness ratio is used to predict and calculate the wear depth and wear volume at ambient temperatures of -40, -20, 0, 10 and 20°C under the condition of a wheel-rail hardness ratio of 0.8 (CL60 wheel-U71Mn rail), as shown in Table 6. It can be seen that the wear depth and wear volume at an ambient temperature of 10°C are similar to those of the above-mentioned commonly used Tγ / A The wheel wear data calculated by the wear rate model is approximately Tγ / A The wear rate model is based on the test results when the ambient temperature is about 10°C, and is only applicable to predicting the wheel wear behavior when the ambient temperature is 10°C. At the same time, it can be seen that as the ambient temperature decreases, the wheel wear shows an upward trend, that is, different ambient temperatures have an impact on the wheel wear prediction results. Tγ / A It is crucial to consider the ambient temperature in the wear diagram.

[0122] Table 6 Wheel wear prediction results at different ambient temperatures

[0123]

[0124] In this embodiment, the three-dimensional wheel wear model that considers both the ambient temperature and the material hardness ratio is used to predict and calculate the wear depth and wear volume when the ambient temperature is 20°C and the material hardness ratio is 0.8, 1.12, 1.4 and 1.6, as shown in Table 7. It can be seen that when the ambient temperature is constant, the wheel wear shows an upward trend with the increase of the hardness ratio, that is, different wheel-rail material hardness ratios have an impact on the wheel wear prediction results. Tγ / A It is also crucial to consider the material hardness ratio in the wear diagram.

[0125] Table 7 Wheel wear prediction results under different hardness matching

[0126]

[0127] Fig.10 and Fig.11 The figure shows the distribution diagram of wheel wear depth and wear volume in the range of -40 to 40°C and wheel-rail hardness ratio of 0.8 to 1.4, which are predicted and calculated by the three-dimensional wheel wear model that considers both the ambient temperature and the material hardness ratio. It can be seen that incorporating both the ambient temperature and the wheel-rail material hardness ratio into the wheel wear model can further and more accurately predict the wear behavior of the wheel.

[0128] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.

Claims

1. A method for constructing a three-dimensional wheel-rail wear map considering ambient temperature and material properties. Features: The following steps are involved: 1) Based on the wheel-rail rolling friction and wear experiments under different contact parameters, the friction and wear properties of the wheel material under different ambient temperatures and different wheel-rail hardness ratios were obtained, and the functional relationship between the wheel wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios was established; In step 1), the functional relationship between the wheel wear rate and the dissipated energy per unit area of ​​the wheel-rail contact patch under a series of different ambient temperatures and wheel-rail hardness ratios is the Tγ / A-wear rate functional relationship, wherein the wheel wear rate is the product of the wear amount divided by the running distance and the wheel-rail contact area A; the dissipated energy per unit area of ​​the wheel-rail contact patch Tγ / A is the product of the tangential force T of the wheel-rail interface and the creep rate γ divided by the wheel-rail contact area A; the Tγ / A-wear rate functional relationship is divided into two regions, I and II, according to the slope of the curve; 2) MATLAB software was used to fit the experimental data to obtain the three-dimensional wear diagram of the wheel considering the ambient temperature and the three-dimensional wear diagram of the wheel considering the hardness ratio of the wheel and rail materials; 3) Selecting a two-dimensional reference wear map and constructing a three-dimensional wheel wear map that takes into account both ambient temperature and material hardness ratio through normalization processing; In step 3), select the same ambient temperature Tt 1 And material hardness ratio Hv 1 Wheel two-dimensional wear diagram 2DMAP (Tt 1 ) and 2DMAP(Hv 1 ), and the two-dimensional wear maps 2DMAP (Tt 1 ) and 2DMAP(Hv 1 ) are interpolated and fitted by the slopes of regions Ⅰ and Ⅱ in the figure to construct a benchmark two-dimensional wear map 2DMAP(S); the wheel wear model considering the ambient temperature Tt and the wheel wear model considering the material hardness ratio Hv are normalized and fitted with the benchmark two-dimensional wear map 2DMAP(S) to obtain a wheel wear model that considers both the ambient temperature and the material hardness ratio; based on the wheel wear model that considers both the ambient temperature and the material hardness ratio, the variable Tt·e that involves both the ambient temperature and the material hardness ratio is derived. 4.9177·Hv , construct a wear rate, Tγ / A and Tt·e 4.9177·Hv The three-dimensional wheel wear diagram 3DMAP (Tt, Hv) takes into account the ambient temperature and the wheel-rail material hardness ratio while taking into account the coordinate parameters.

2. A method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties according to claim 1, Features: In step 2), the function fitting is performed on the slopes of the line segments in regions Ⅰ and Ⅱ of the Tγ / A-wear rate curve at different ambient temperatures and the horizontal coordinates of the intersection points of regions Ⅰ and Ⅱ using MATLAB software with ambient temperature as the independent variable to obtain a wheel wear model considering the ambient temperature Tt. Based on the wheel wear model considering the ambient temperature Tt, a three-dimensional wheel wear map 3DMAP(Tt) considering the ambient temperature is constructed with the wear rate, Tγ / A and ambient temperature Tt as coordinate parameters; Function fitting was performed on the slopes of regions Ⅰ and Ⅱ of the Tγ / A-wear rate curve under different wheel-rail hardness ratios to obtain the wheel wear model considering the material hardness ratio Hv. Based on the wheel wear model considering the material hardness ratio Hv, a three-dimensional wheel wear map 3DMAP(Hv) considering the wheel-rail material hardness ratio was constructed with wear rate, Tγ / A and wheel-rail hardness ratio as coordinate parameters. The two-dimensional wheel wear maps 2DMAP(Tt) and 2DMAP(Hv) under a certain ambient temperature or material hardness ratio were obtained from the three-dimensional wheel wear map 3DMAP(Tt) and the three-dimensional wheel wear map 3DMAP(Hv).

3. A method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties according to claim 2, Features: In step 2), the slope fitting functions of the line segments in regions Ⅰ and Ⅱ in the wheel wear model considering the ambient temperature Tt are k 1 =-0.0085·T t +1.816 and k 2 =-0.0035·T t +0.260, the horizontal and vertical coordinate fitting functions of the intersection of regions Ⅰ and Ⅱ are x 1 =-0.1054·T t +19.464, y 1 =-0.5155*T t +33.711, the wheel wear model considering the ambient temperature Tt is as follows: I Region: 0 <Tγ / A<x 1 , the wear rate is k 1 (Tγ / A); Region Ⅱ: x 1 <Tγ / A, wear rate is k 2 ·(Tγ / A) - k 2 ·x 1 +y 1 。 4. A method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties according to claim 3, Features: In step 2), the slope fitting functions of the line segments in regions Ⅰ and Ⅱ in the wheel wear model considering the material hardness ratio are k 3 =0.3872+0.0507·e 4.9177Hv and k 4 =0.0847+0.0056*e 4.7672Hv , the horizontal coordinate x of the intersection point of regions Ⅰ and Ⅱ 2 is the intersection value x of the wheel Tγ / A-wear rate function relationship at an ambient temperature of 20°C 2 =16.657; The wheel wear model considering the material hardness ratio Hv is as follows: I Region: 0 <Tγ / A<x 2 , the wear rate is k 3 *(Tγ / A); Region Ⅱ: x 2 <Tγ / A, wear rate is k 4 *(Tγ / A) + 16.657*(k 3 -k 4 )。 5. A method for constructing a wheel-rail three-dimensional wear map taking into account ambient temperature and material properties according to claim 4, Features: In step 3), the same ambient temperature Tt 1 And material hardness ratio Hv 1 Take 20℃ and 1.08 respectively; considering the ambient temperature and material hardness ratio, the slopes of the wheel wear diagram I and II are 0.6075*k 1 k 3 , 5.2604*k 2 k 4 The horizontal coordinate of the intersection of the two regions is 1.0394*x 1 ; The wheel wear model of the wheel three-dimensional wear diagram 3DMAP (Tt, Hv) considering both the ambient temperature and the material hardness ratio is as follows: I Region: 0 <Tγ / A<1.0394*x 1 , the wear rate is 0.6075*k 1 k 3 *(Tγ / A); Region Ⅱ: 1.0394 * x 1 <Tγ / A, wear rate is 5.2604 * k 2 k 4 *(Tγ / A) + 0.6314 * y 1 k 3 -1.0394 * y 1 k 2 k 4 / k 1 。