Preparation method of metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material and vehicle

Through the preparation method of metal niobium doped with sodium ferrophosphate phosphate positive electrode material, the problems of poor conductivity and impurity generation of the positive electrode material are solved, and the efficient electrochemical performance of the material is improved.

CN118630202BActive Publication Date: 2024-12-03ZHEJIANG HUAYU NADIAN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110332.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The electronic conductivity of the cathode material of sodium ferric pyrophosphate is not ideal, and the synthesis process is complex and easy to produce inactive impurities, which affects its electrochemical performance.

Method used

Using metal niobium doped sodium iron pyrophosphate positive electrode material, excellent electrochemistry is prepared by mixing sodium, iron, niobium and phosphorus sources with carbon sources in water, grinding, spray drying and high-temperature annealing treatment. A pure phase material of performance.

Benefits of technology

The electrochemical performance of the sodium ferric pyrophosphate positive electrode material is improved, the generation of inactive impurities is reduced, and the reversible capacity and rate performance of the material is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118630202B_ABST
    Figure CN118630202B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and vehicle of a sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium, and belongs to the technical field of synthesis of positive electrode materials for sodium ion batteries. The specific preparation method comprises mixing a sodium source, an iron source, a niobium source, a phosphorus source, a carbon source and water to obtain a suspension, then sand-milling the suspension to obtain a precursor, then spray-drying the obtained precursor to obtain a dry powder, and finally annealing the dry powder at high temperature under nitrogen to obtain a sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium. The button battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium obtained by this preparation method has good electrochemical performance, high reversible capacity, first coulomb efficiency and capacity retention rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthesis of positive electrode materials for sodium ion batteries, and in particular relates to a preparation method and a vehicle for a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material. Background Art

[0002] With the growth of global energy demand and the intensification of environmental pollution problems, the development of clean energy and efficient energy storage technology has become particularly important. As an efficient electrochemical energy storage technology, lithium-ion batteries have been widely used in fields such as electric vehicles and energy storage power stations. However, with the expansion of global large-scale energy storage demand, the uneven distribution of lithium resources has become a bottleneck restricting the large-scale application of lithium-ion batteries in my country. Sodium has similar chemical properties to lithium and its abundance in the earth's crust is much higher than that of lithium, so the development of sodium-ion battery technology is of great significance. In the research of sodium-ion battery cathode materials, layered oxides, Prussian blue analogs and polyanion compounds are considered to be the three major mainstream routes. Compared with the other two, polyanion compounds have been widely studied due to their excellent structural stability and high voltage. Among them, sodium iron pyrophosphate is considered by the industry to be the best cathode material for energy storage sodium-ion batteries because of its low cost and environmental friendliness.

[0003] However, the electronic conductivity of sodium iron pyrophosphate positive electrode materials is not ideal, and the synthesis process requires high requirements, and it is very easy to produce inactive impurity phase NaFePO during the preparation process. 4 , affecting the rate performance and reversible capacity of the material. In response to the above problems, the current mainstream modification methods are carbon coating, nano-processing, electrolyte optimization and ion doping. For example: Patent CN 118164458A discloses a method for preparing a simple carbon-coated anion-doped sodium iron sulfate as a positive electrode material for sodium ion batteries. However, these methods have the problems of high production cost, low efficiency, limited improvement effect or difficulty in scale-up production. Therefore, there is an urgent need for a simple and efficient method for synthesizing sodium iron phosphate pyrophosphate positive electrode material with excellent electrochemical properties. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a metal niobium-doped sodium iron pyrophosphate positive electrode material and a vehicle to solve the technical problems that the sodium iron pyrophosphate positive electrode material has poor conductivity and is prone to produce inactive impurities during the preparation process, which affects its electrochemical performance.

[0005] In order to solve the above technical problems, the present invention specifically provides the following technical solutions:

[0006] The present invention discloses a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material, comprising the following structure: Na x Fe y Nb m (PO4 ) n (P 2 O 7 ); wherein x is 2-8, y is 1.5-6, m is 0.05-0.3, and n is 1-4.

[0007] Preferably, x is 3-5, y is 2-4, m is 0.05-0.2, and n is 1-3; or, x is 3.9-4.1, y is 2.8-3.5, m is 0.05-0.3, and n is 1-3; or, x is 4, y is 2.9, m is 0.1, and n is 2.

[0008] Preferably, Na x Fe y Nb m (PO 4 ) n (P 2 O 7 ) is a pure phase material.

[0009] The present invention discloses a method for preparing a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material, comprising:

[0010] The positive electrode material source and the carbon source are mixed in water, and subjected to grinding, spray drying and high-temperature annealing treatment to obtain a metal niobium element-doped sodium iron phosphate pyrophosphate positive electrode material; the positive electrode material source comprises a sodium source, an iron source, a niobium source and a phosphorus source, and the metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material has the following structure: Na x Fe y Nb m (PO 4 ) n (P 2 O 7 ); wherein x is 2-8, y is 1.5-6, m is 0.05-0.3, and n is 1-4.

[0011] Preferably, the sodium source includes at least one of sodium carbonate, sodium oxalate, sodium acetate, sodium hydroxide, sodium citrate, sodium dihydrogen phosphate and sodium pyrophosphate; the iron source includes at least one of ferrous sulfate, ferrous oxalate, ferrous acetate, ferric phosphate, ferric nitrate, ferric oxide and ferric oxide; the niobium source includes at least one of niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, niobium nitrate, niobium acetate and niobium oxalate; the phosphorus source includes at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, triammonium phosphate and sodium dihydrogen phosphate; the carbon source includes at least one of sucrose, sucrose derivatives and polyethylene glycol. The sucrose derivatives can affect the grain morphology of the metal niobium doped sodium iron phosphate pyrophosphate positive electrode material, promote the dispersion of surface particles, improve the cleanliness and distribution uniformity of the grains, obtain a metal niobium doped sodium iron phosphate pyrophosphate positive electrode material with a smooth surface and relatively complete crystals, and then improve the electrochemical performance of the niobium doped sodium iron phosphate pyrophosphate positive electrode material.

[0012] Preferably, the sucrose derivative is made from sucrose, 2-chloro-N,N-dimethylacetamide and acetic anhydride.

[0013] Preferably, the molar ratio of sodium, iron, niobium and phosphorus in the sodium source, iron source, niobium source and phosphorus source is 3.9-4.1:2.8-3.5:0.05-0.3:3.95-4.1; the mass ratio of the carbon source to the positive electrode material source is 1:2-15.

[0014] Preferably, the grinding is nano-sand milling, the nano-sand milling speed is 1000-2500 rpm, the sand milling time is 1-4 h, and the particle size D50 after sand milling is 100-400 nm; or, the air inlet temperature of the spray drying is 150-210 ° C, the atomizer frequency is 200-450 Hz, and the feed amount is 3-5 L / h; or, the high temperature annealing temperature is 450-600 ° C, and the annealing time is 8-24 h.

[0015] The invention discloses a battery, comprising the above-mentioned metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material or the metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material prepared by the above-mentioned method.

[0016] The invention discloses a vehicle, comprising the battery mentioned above.

[0017] A method for preparing a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material, the specific steps of which are:

[0018] The cathode material source and the carbon source are added into water and stirred to obtain a suspension, the suspension is nano-milled to obtain a precursor, the precursor is then spray-dried to obtain a dry powder, and the dry powder is finally annealed at high temperature under nitrogen to obtain a metal niobium element-doped sodium iron phosphate pyrophosphate cathode material.

[0019] Preferably, the positive electrode material source includes a sodium source, an iron source, a niobium source and a phosphorus source; the sodium source includes but is not limited to at least one of sodium carbonate, sodium oxalate, sodium acetate, sodium hydroxide, sodium citrate, sodium dihydrogen phosphate and sodium pyrophosphate; the iron source includes but is not limited to at least one of ferrous sulfate, ferrous oxalate, ferrous acetate, ferric phosphate, ferric nitrate, ferric oxide and ferrous oxide; the niobium source includes but is not limited to at least one of niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, niobium nitrate, niobium acetate and niobium oxalate; the phosphorus source includes but is not limited to at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, triammonium phosphate and sodium dihydrogen phosphate; the carbon source includes but is not limited to at least one of sucrose, a sucrose derivative and polyethylene glycol.

[0020] Preferably, in the above technical solution, the molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 3.9-4.1:2.8-3.5:0.05-0.3:3.95-4.1.

[0021] Preferably, in the above technical solution, the mass ratio of the carbon source to the positive electrode material source is 1:2-15.

[0022] Preferably, in the above technical solution, the stirring and mixing time is 0.5-3 h.

[0023] Preferably, in the above technical solution, the nano-sand milling speed is 1000-2500 rpm, the sand milling time is 1-4 h, and the particle size D50 after sand milling is 100-400 nm.

[0024] Preferably, in the above technical solution, the air inlet temperature of the spray drying is 150-210°C, the atomizer frequency is 200-450 Hz, and the feed rate is 3-5 L / h.

[0025] Preferably, in the above technical solution, the high temperature annealing temperature is 450-600°C, and the high temperature annealing time is 8-24h.

[0026] Preferably, in a preferred embodiment of the present invention, the preparation of the niobium-doped sodium iron phosphate pyrophosphate positive electrode material is as follows: sodium carbonate is used as a sodium source, ferrous oxalate is used as an iron source, niobium oxalate is used as a niobium source, ammonium dihydrogen phosphate is used as a phosphorus source, and sucrose and polyethylene glycol are used as carbon sources; the steps are as follows: first, sodium carbonate, ferrous oxalate, niobium oxalate, ammonium dihydrogen phosphate, sucrose and polyethylene glycol are sequentially added to water and stirred for 0.5-3 h to obtain a suspension. Then, the suspension is nano-milled at 1000-2500 rpm for 1-4 h to obtain a precursor with a particle size D50 of 100-400 nm. The precursor is then spray dried at an air inlet temperature of 150-210 °C, an atomizer frequency of 200-450 Hz, and a feed rate of 3-5 L / h to obtain a dry powder, and then the dry powder is annealed at 450-600 °C under nitrogen for 8-24 h to obtain a metal niobium doped sodium iron phosphate pyrophosphate positive electrode material.

[0027] More preferably, in the above preferred embodiment, the molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 3.9-4.0:2.8-3.3:0.05-0.2:3.95-4.0, the mass ratio of the carbon source to the positive electrode material source is 1:2-14, and the positive electrode material source includes a sodium source, an iron source, a niobium source and a phosphorus source.

[0028] More preferably, in the present invention, when preparing the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium, sucrose can be replaced with a sucrose derivative. The present invention discloses a method for preparing a sucrose derivative.

[0029] More preferably, the preparation of the sucrose derivative is specifically as follows:

[0030] First, sucrose and DMAP are dissolved in pyridine, then cooled to 45-65 °C, 2-chloro-N,N-dimethylacetamide is added in batches within 1.5 h to obtain a mixed solution, and the mixed solution is heated to 50-80 °C and the reaction is continued for 0.5-6 h. After the reaction is completed, pyridine is evaporated to obtain the initial reactant, the temperature is lowered to room temperature, acetic anhydride is added to the initial reactant, the temperature is raised to 45-60 °C, and the reaction is continued for 1-8 h to obtain a reaction mixture. Then, the reaction mixture is poured into ice water under stirring to precipitate a white solid, the white solid is filtered out and washed with water to remove pyridine, the white solid is dried to obtain a white powder, and finally the white powder is recrystallized with methanol / acetone in a volume ratio of 80:20 to obtain a sucrose derivative.

[0031] Preferably, in the preparation of the sucrose derivative, the amount of sucrose added to pyridine is 200-400 g / L.

[0032] Preferably, in the preparation of sucrose derivatives, the amount of DMAP added to pyridine is 4-8 g / L.

[0033] Preferably, in the preparation of the sucrose derivative, the amount of 2-chloro-N,N-dimethylacetamide added to pyridine is 500-700 g / L.

[0034] Preferably, in the preparation of the sucrose derivative, the volume ratio of acetic anhydride to pyridine is 1:5.33-11.

[0035] More preferably, when preparing the niobium-doped sodium iron phosphate pyrophosphate positive electrode material, butyl oxamate can be added on the basis of using sucrose derivatives, which is helpful for the uniform dispersion and stability of the precursor particles. At the same time, the agglomeration and change of the niobium-doped sodium iron phosphate pyrophosphate positive electrode material can be reduced, and the electrochemical performance of the niobium-doped sodium iron phosphate pyrophosphate positive electrode material can be further improved.

[0036] Preferably, in a preferred embodiment of the present invention, the preparation of the niobium-doped sodium iron phosphate pyrophosphate positive electrode material is as follows: the preparation of the niobium-doped sodium iron phosphate pyrophosphate positive electrode material, using sodium carbonate as a sodium source, ferrous oxalate as an iron source, niobium oxalate as a niobium source, ammonium dihydrogen phosphate as a phosphorus source, sucrose derivatives and polyethylene glycol as carbon sources; the steps are as follows: first, sodium carbonate, ferrous oxalate, niobium oxalate, ammonium dihydrogen phosphate, sucrose derivatives, polyethylene glycol and butyl oxamate are sequentially added to water and stirred for 1 h to obtain a suspension. Then, the suspension is nano-milled at 1000-2500 rpm for 1-4 h to obtain a precursor with a particle size D50 of 100-400 nm. The precursor is then spray dried at an air inlet temperature of 150-210 °C, an atomizer frequency of 200-450 Hz, and a feed rate of 3-5 L / h to obtain a dry powder, and then the dry powder is annealed at 450-600 °C under nitrogen for 8-24 h to obtain a metal niobium doped sodium iron phosphate pyrophosphate positive electrode material.

[0037] More preferably, in the above preferred embodiment, the molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 3.9-4.0:2.8-3.3:0.05-0.2:3.95-4.0, the mass ratio of the carbon source to the positive electrode material source is 1:2-14, the positive electrode material source includes a sodium source, an iron source, a niobium source and a phosphorus source, and the amount of butyl oxalate added to water is 5-30 g / L.

[0038] Preferably, the present invention also provides a sodium iron phosphate pyrophosphate positive electrode material doped with metallic niobium, which is prepared by the above-mentioned preparation method.

[0039] Preferably, the present invention also discloses a use of the above-mentioned sodium iron phosphate pyrophosphate positive electrode material doped with the metal niobium element in the preparation of a positive electrode for a sodium ion battery.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The present invention obtains a sodium ferric phosphate pyrophosphate positive electrode material doped with metal niobium having good electrochemical performance through simple reaction, sand milling, spray drying and high-temperature annealing; the present invention uses high-valent metal niobium to occupy part of the active iron sites in the sodium ferric phosphate pyrophosphate positive electrode material, thereby improving the electrochemical performance of the sodium ferric phosphate pyrophosphate positive electrode material; the present invention prepares a sucrose derivative, which effectively improves the electrochemical performance of the sodium ferric phosphate pyrophosphate positive electrode material doped with metal niobium; BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0043] Figure 1 A technical roadmap for niobium-doped sodium iron pyrophosphate cathode materials;

[0044] Figure 2 is the IR spectrum of sucrose derivatives;

[0045] Figure 3 This is the XRD pattern of the sodium iron pyrophosphate positive electrode material doped with metal niobium;

[0046] Figure 4 This is a SEM image of the sodium iron pyrophosphate positive electrode material doped with metal niobium;

[0047] Figure 5 The coin cell made of niobium-doped sodium iron phosphate pyrophosphate cathode material has a high performance at 0.05 A g -1 The charge and discharge curve diagram below;

[0048] Figure 6 The button cell made of niobium-doped sodium iron phosphate positive electrode material was tested at -30 o C, 0.05 Ag -1 The charge and discharge curve diagram below;

[0049] Figure 7 The rate performance diagram of a button cell made of sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium;

[0050] Figure 8 This is a cycling performance diagram of a button cell made of sodium iron pyrophosphate positive electrode material doped with metal niobium. DETAILED DESCRIPTION

[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] The following first describes the concepts involved in the present application in conjunction with the accompanying drawings. It should be noted that the following description of each concept is only to make the content of the present application easier to understand, and does not limit the scope of protection of the present application; at the same time, the embodiments and features in the embodiments of the present application can be combined with each other in the absence of conflict. The present application will be described in detail with reference to the accompanying drawings and in conjunction with the embodiments.

[0053] Embodiment 1:

[0054] Preparation of niobium-doped sodium iron phosphate pyrophosphate cathode material: Sodium carbonate is used as the sodium source, ferrous oxalate is used as the iron source, niobium oxalate is used as the niobium source, ammonium dihydrogen phosphate is used as the phosphorus source, and sucrose and polyethylene glycol are used as the carbon source; the steps are as follows: First, sodium carbonate, ferrous oxalate, niobium oxalate, ammonium dihydrogen phosphate, sucrose and polyethylene glycol are added to deionized water in sequence and stirred for 1 h to obtain a suspension. Then, the suspension is nano-milled at 2000 rpm for 2 h to obtain a precursor with a particle size D50 of 150 nm. The precursor is then spray-dried at an air inlet temperature of 180 °C, an atomizer frequency of 350 Hz, and a feed rate of 4 L / h to obtain a dry powder, and then the dry powder is annealed at 550 °C for 12 h under nitrogen to obtain a niobium-doped sodium iron phosphate pyrophosphate cathode material. The molar ratio of sodium, iron, niobium and phosphorus in the sodium source, iron source, niobium source and phosphorus source is 4:2.9:0.1:4, that is, the amount of sodium carbonate added to deionized water is 1 mol / L, the amount of ferrous oxalate added to deionized water is 1.45 mol / L, the amount of niobium oxalate added to deionized water is 0.05 mol / L, and the amount of diammonium phosphate added to deionized water is 2 mol / L. The amount of sucrose added to deionized water is 50 g / L, and the amount of polyethylene glycol added to deionized water is 25 g / L.

[0055] like Figure 1 Shown is a technical roadmap for the preparation of metal niobium doped sodium iron phosphate pyrophosphate positive electrode material.

[0056] Embodiment 2:

[0057] Compared with Example 1, the present embodiment is different in that the molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 4:2.95:0.05:4, the addition amount of ferrous oxalate is 1.475 mol / L, the addition amount of niobium oxalate is 0.025 mol / L, and other conditions and parameters are the same as in Example 1.

[0058] Embodiment 3:

[0059] Compared with Example 1, the present embodiment is different in that the molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 4:2.85:0.15:4, the addition amount of ferrous oxalate is 1.425 mol / L, the addition amount of niobium oxalate is 0.075 mol / L, and other conditions and parameters are the same as in Example 1.

[0060] Embodiment 4:

[0061] Compared with Example 1, the present embodiment is different in that the molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 4:2.97:0.03:4, the addition amount of ferrous oxalate is 1.485 mol / L, the addition amount of niobium oxalate is 0.015 mol / L, and other conditions and parameters are the same as in Example 1.

[0062] Embodiment 5:

[0063] Preparation of sucrose derivatives: First, sucrose and DMAP are dissolved in pyridine, then cooled to 60°C, 2-chloro-N,N-dimethylacetamide is added in batches within 1.5 h to obtain a mixed solution, and the mixed solution is heated to 75°C and the reaction is continued for 2 h. After the reaction is completed, pyridine is evaporated to obtain the initial reactant, the temperature is lowered to room temperature, acetic anhydride is added to the initial reactant, the temperature is raised to 50°C, and the reaction is continued for 1.5 h to obtain a reaction mixture. Then, the reaction mixture is poured into ice water under stirring to precipitate a white solid, the white solid is filtered out and washed with water to remove pyridine, the white solid is dried to obtain a white powder, and finally the white powder is recrystallized with methanol / acetone in a volume ratio of 80:20 to obtain a sucrose derivative. The amount of sucrose added to pyridine was 213.75 g / L, the amount of DMAP added to pyridine was 6.25 g / L, the amount of 2-chloro-N,N-dimethylacetamide added to pyridine was 625 g / L, and the volume ratio of acetic anhydride to pyridine was 1:6.

[0064] Preparation of niobium-doped sodium iron phosphate pyrophosphate positive electrode material: The preparation of niobium-doped sodium iron phosphate pyrophosphate positive electrode material in this embodiment is the same as that in Example 1, except that sucrose is replaced by the sucrose derivative prepared in this embodiment.

[0065] Embodiment 6:

[0066] The preparation of sucrose derivatives is the same as in Example 5.

[0067] Preparation of niobium-doped sodium iron phosphate pyrophosphate cathode material, using sodium carbonate as sodium source, ferrous oxalate as iron source, niobium oxalate as niobium source, ammonium dihydrogen phosphate as phosphorus source, sucrose derivatives and polyethylene glycol as carbon sources; the steps are as follows: first, sodium carbonate, ferrous oxalate, niobium oxalate, ammonium dihydrogen phosphate, sucrose and polyethylene glycol are added to deionized water in sequence and stirred for 1 h to obtain a suspension. Then, the suspension is nano-milled at 2000 rpm for 2 h to obtain a precursor with a particle size D50 of 150 nm. The precursor is then spray-dried at an air inlet temperature of 180 ° C, an atomizer frequency of 350 Hz, and a feed rate of 4 L / h to obtain a dry powder, and then the dry powder is annealed at 550 ° C for 12 h under nitrogen to obtain a niobium-doped sodium iron phosphate pyrophosphate cathode material. The molar ratio of sodium, iron, niobium and phosphorus in the sodium source, iron source, niobium source and phosphorus source is 4:2.9:0.1:4, that is, the amount of sodium carbonate added to deionized water is 1 mol / L, the amount of ferrous oxalate added to deionized water is 1.45 mol / L, the amount of niobium oxalate added to deionized water is 0.05 mol / L, and the amount of diammonium phosphate added to deionized water is 2 mol / L. The amount of sucrose derivative added to deionized water is 32.15 g / L, and the amount of polyethylene glycol added to deionized water is 25 g / L.

[0068] Embodiment 7:

[0069] The preparation of sucrose derivatives is the same as in Example 5.

[0070] Preparation of sodium iron phosphate pyrophosphate cathode material doped with metal niobium, using sodium carbonate as sodium source, ferrous oxalate as iron source, niobium oxalate as niobium source, ammonium dihydrogen phosphate as phosphorus source, sucrose and polyethylene glycol as carbon source; the steps are as follows: first, sodium carbonate, ferrous oxalate, niobium oxalate, ammonium dihydrogen phosphate, sucrose derivatives, polyethylene glycol and butyl oxamate are added to deionized water in sequence and stirred for 1 h to obtain a suspension. Then, the suspension is nano-milled at 2000 rpm for 2 h to obtain a precursor with a particle size D50 of 150 nm. The precursor is then spray-dried at an air inlet temperature of 180 °C, an atomizer frequency of 350 Hz, and a feed rate of 4 L / h to obtain a dry powder, and then the dry powder is annealed at 550 °C for 12 h under nitrogen to obtain a sodium iron phosphate pyrophosphate cathode material doped with metal niobium. The molar ratio of sodium, iron, niobium and phosphorus in the sodium source, iron source, niobium source and phosphorus source is 4:2.9:0.1:4, that is, the amount of sodium carbonate added to deionized water is 1 mol / L, the amount of ferrous oxalate added to deionized water is 1.45 mol / L, the amount of niobium oxalate added to deionized water is 0.05 mol / L, and the amount of diammonium phosphate added to deionized water is 2 mol / L. The amount of sucrose derivative added to deionized water is 50 g / L, the amount of polyethylene glycol added to deionized water is 25 g / L. The amount of butyl oxamate added to deionized water is 25 g / L.

[0071] Embodiment 8:

[0072] The preparation of sucrose derivatives is the same as in Example 5.

[0073] Preparation of sodium iron phosphate pyrophosphate cathode material doped with metal niobium, using sodium carbonate as sodium source, ferrous oxalate as iron source, niobium oxalate as niobium source, ammonium dihydrogen phosphate as phosphorus source, sucrose and polyethylene glycol as carbon source; the steps are as follows: first, sodium carbonate, ferrous oxalate, niobium oxalate, ammonium dihydrogen phosphate, sucrose derivatives, polyethylene glycol and butyl oxamate are added to deionized water in sequence and stirred for 1 h to obtain a suspension. Then, the suspension is nano-milled at 2000 rpm for 2 h to obtain a precursor with a particle size D50 of 150 nm. Then, the precursor is spray-dried at an air inlet temperature of 180 ° C, an atomizer frequency of 350 Hz, and a feed rate of 4 L / h to obtain a dry powder, and then the dry powder is annealed at 550 ° C under nitrogen for 12 h to obtain a sodium iron phosphate pyrophosphate cathode material doped with metal niobium. The molar ratio of sodium, iron, niobium and phosphorus is 4:2.9:0.1:4. The molar ratio of sodium, iron, niobium and phosphorus in the sodium source, iron source, niobium source and phosphorus source is 4:2.9:0.1:4, that is, the amount of sodium carbonate added to deionized water is 1 mol / L, the amount of ferrous oxalate added to deionized water is 1.45 mol / L, the amount of niobium oxalate added to deionized water is 0.05 mol / L, and the amount of diammonium phosphate added to deionized water is 2 mol / L. The amount of sucrose derivative added to deionized water is 50 g / L, the amount of polyethylene glycol added to deionized water is 25 g / L. The amount of butyl oxalate added to deionized water is 10 g / L.

[0074] Comparative Example 1:

[0075] The difference between this comparative example and Example 1 is that the amount of ferrous oxalate added to deionized water is 1.5 mol / L, niobium oxalate is not used, and other conditions and parameters are the same as those in Example 1.

[0076] Comparative Example 2:

[0077] The difference between this comparative example and Example 1 is that niobium oxalate is not used, and other conditions and parameters are the same as those in Example 1.

[0078] Comparative Example 3:

[0079] Preparation of sucrose derivatives: The preparation of sucrose derivatives in this example is compared with that in Example 2, except that the amount of 2-chloro-N,N-dimethylacetamide added to pyridine is 312.5 g / L.

[0080] The preparation of metal niobium doped sodium iron phosphate pyrophosphate positive electrode material is the same as in Example 5.

[0081] Comparative Example 4:

[0082] Preparation of sucrose derivatives: The preparation of sucrose derivatives in this example is compared with that in Example 5, except that the amount of 2-chloro-N,N-dimethylacetamide added to pyridine is 781.25 g / L.

[0083] The preparation of metal niobium doped sodium iron phosphate pyrophosphate positive electrode material is the same as in Example 5.

[0084] Comparative Example 5:

[0085] Preparation of sucrose derivatives: The preparation of sucrose derivatives in this example is compared with that in Example 5, except that the volume ratio of acetic anhydride to pyridine added is 1:16.

[0086] The preparation of metal niobium doped sodium iron phosphate pyrophosphate positive electrode material is the same as in Example 5.

[0087] Comparative Example 6:

[0088] Preparation of sucrose derivatives: The preparation of sucrose derivatives in this example is compared with that in Example 5, except that the volume ratio of acetic anhydride to pyridine added is 1:4.

[0089] The preparation of metal niobium doped sodium iron phosphate pyrophosphate positive electrode material is the same as in Example 5.

[0090] Experimental Example 1:

[0091] The sucrose derivatives prepared in Example 2 were characterized by infrared spectroscopy. The sucrose derivatives were dissolved in methanol and water and evenly coated on a pre-pressed KBr sheet. The scanning range was 400-4000 cm -1 The results are as follows Figure 2 As shown, 3400-3700 cm -1 The absorption peak in the range of 2800-3000 cm is the characteristic absorption of the stretching vibration of hydroxyl OH. -1 The absorption peak in the range of 1600-1800 cm -1 The stretching vibration absorption peak of C=O is consistent with the structural characteristics of sucrose derivatives.

[0092] Experimental Example 2:

[0093] The metal niobium doped sodium iron phosphate pyrophosphate positive electrode material was characterized by performing X-ray diffraction phase analysis on the metal niobium doped sodium iron phosphate pyrophosphate positive electrode material prepared in Example 1. The results are as follows Figure 3 As shown, pure phase material was successfully prepared.

[0094] Embodiment 3:

[0095] The niobium-doped sodium iron phosphate pyrophosphate positive electrode material was characterized by scanning electron microscopy analysis of the niobium-doped sodium iron phosphate pyrophosphate positive electrode material prepared in Example 1. The results are as follows Figure 4 As shown, the prepared metal niobium doped sodium iron phosphate pyrophosphate positive electrode material has a spherical morphology, and the product particle size is controllable.

[0096] Experimental Example 4:

[0097] The reversible capacity was measured. The sodium iron phosphate pyrophosphate positive electrode material prepared in Example 1-8 and Comparative Example 1-6, Ketjen black and N-methylpyrrolidone-polyvinylidene fluoride binder (5wt.%) were mixed at a mass ratio of 90:5:5 to obtain a mixture. The mixture was ground and mixed evenly, and then zirconium oxide beads were added to the vibration ball mill to obtain a mixed slurry. The mixed slurry was coated on aluminum foil and placed in a vacuum dryer at 80°C for 6 h, and the electrode was cut into pieces. The electrode was transferred and assembled in a glove box (O wt.%≤0.01, H 2 O wt.% ≤ 0.01), 1 M NaClO 4 -PC-FEC (5wt.%) was used as the electrolyte and sodium sheet as the counter electrode to assemble into a button cell for electrochemical testing. The current density was 0.05 A g -1 , the test voltage window is 2.0-4.0 V. The sodium iron pyrophosphate phosphate positive electrode material includes the sodium iron pyrophosphate phosphate positive electrode material doped with metal niobium prepared in Examples 1-8 and Comparative Examples 3-6 and the sodium iron pyrophosphate phosphate positive electrode material without metal niobium doping prepared in Comparative Examples 1-2.

[0098] Table 1 Reversible capacity performance of button cell

[0099]

[0100] The sodium iron phosphate pyrophosphate positive electrode materials doped with metal niobium prepared in Example 1 of the present invention and without metal niobium doping prepared in Comparative Example 1 were made into button-type batteries for reversible capacity testing. The results are as follows: Figure 5 As shown in the figure, the reversible capacity of Example 1 is higher than that of Comparative Example 1, indicating that metal niobium may have suppressed the inactive impurity phase NaFePO during the preparation process. 4The generation of metal niobium, thereby improving the reversible capacity of the button battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium; under the same test conditions, the reversible capacity results of all embodiments and comparative examples are shown in Table 1. The button battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 of the present invention provides a higher reversible capacity than that of the comparative example 2 without metal niobium, further indicating that the doping of metal niobium can indeed improve the reversible capacity of the button battery made of the sodium iron phosphate pyrophosphate positive electrode material; the reversible capacity of the button battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Examples 5 and 6 of the present invention is higher than that of Example 1, indicating that the sucrose derivatives prepared in Examples 5 and 6 are better than sucrose, which may be due to the structural effect of 2-chloro-N,N-dimethylacetamide and acetic anhydride The reversible capacity of the button-type battery prepared by the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium can be improved; compared with Example 2, Examples 7 and 8 of the present invention show that when using sucrose derivatives to prepare the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium, butyl oxamate can be further used. The simultaneous use of butyl oxamate and sucrose derivatives can further improve the reversible capacity of the button-type battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium; Compared with Comparative Examples 3-6, Example 5 of the present invention shows that when preparing sucrose derivatives, the usage of 2-chloro-N,N-dimethylacetamide and acetic anhydride needs to be at a moderate value. Too high or too low a value will inhibit the reversible capacity effect of the button-type battery of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared from the sucrose derivatives.

[0101] Experimental Example 5:

[0102] The reversible capacity at -30°C was measured. The sodium iron phosphate pyrophosphate positive electrode materials prepared in Example 1 and Comparative Example 1 were made into button batteries. -1 , and the reversible capacity was tested at 2.0-4.0 V. The sodium iron phosphate pyrophosphate positive electrode material includes the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 and the sodium iron phosphate pyrophosphate positive electrode material without metal niobium doping prepared in Comparative Example 1. The results are as follows Figure 6 As shown, the reversible capacity of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 at -30°C is still high and higher than that of Comparative Example 1, indicating that metal niobium improves its low-temperature sodium storage performance.

[0103] Experimental Example 6:

[0104] The reversible capacity at different current densities was measured. The sodium iron phosphate pyrophosphate positive electrode materials prepared in Example 1 of the present invention and Comparative Example 1 were made into button batteries, and the reversible capacity was tested at 2.0-4.0 V. The sodium iron phosphate pyrophosphate positive electrode material includes the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 and the sodium iron phosphate pyrophosphate positive electrode material without metal niobium doping prepared in Comparative Example 1. The results are as follows Figure 7 As shown, the reversible capacity of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 is still high at different current densities, and is higher than that of Comparative Example 1, indicating that the rate performance has been significantly improved.

[0105] Experimental Example 7:

[0106] The first coulombic efficiency was measured, and the sodium iron phosphate pyrophosphate positive electrode materials prepared in Examples 1-8 and Comparative Examples 1-6 were assembled into button cells for testing. The current density was 0.05 A g -1 , the test voltage window is 2.0-4.0 V. The sodium iron pyrophosphate phosphate positive electrode material includes the sodium iron pyrophosphate phosphate positive electrode material doped with metal niobium prepared in Examples 1-8 and Comparative Examples 3-6 and the sodium iron pyrophosphate phosphate positive electrode material without metal niobium doping prepared in Comparative Examples 1-2.

[0107] Table 2 First coulombic efficiency performance of button cell

[0108]

[0109] The results are shown in Table 2. The first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 of the present invention is higher than that of the comparative example 2 without metal niobium, indicating that the doping of metal niobium can indeed improve the first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material; the first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Examples 5 and 6 of the present invention is higher than that of Example 1, indicating that the sucrose derivatives prepared in Examples 5 and 6 are better than sucrose, which may be due to the structural effect of 2-chloro-N,N-dimethylacetamide and acetic anhydride, which can improve the first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium. The first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium element is further improved by using butyl oxamate and sucrose derivatives simultaneously; the first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium element is further improved by using butyl oxamate and sucrose derivatives in Examples 7 and 8 of the present invention compared with Example 2; the first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium element is further improved by using butyl oxamate and sucrose derivatives simultaneously; the first coulombic efficiency of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium element is further improved by using butyl oxamate and sucrose derivatives in Example 5 of the present invention compared with Comparative Examples 3-6 is shown that when preparing the sucrose derivative, the usage of 2-chloro-N,N-dimethylacetamide and acetic anhydride needs to be at a moderate value, and too high or too low a value will inhibit the first coulombic efficiency effect of the button cell made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium element prepared by using the sucrose derivative.

[0110] Experimental Example 8:

[0111] The capacity retention rate was measured by assembling the sodium iron phosphate pyrophosphate positive electrode materials prepared in Examples 1-8 and Comparative Examples 1-6 into button-type batteries for testing. The current density was 2 A g -1 , the test voltage window is 2.0-4.0 V. The sodium iron pyrophosphate phosphate positive electrode material includes the sodium iron pyrophosphate phosphate positive electrode material doped with metal niobium prepared in Examples 1-8 and Comparative Examples 3-6 and the sodium iron pyrophosphate phosphate positive electrode material without metal niobium doping prepared in Comparative Examples 1-2.

[0112] Table 3 Capacity retention performance of button batteries

[0113]

[0114] The sodium iron phosphate pyrophosphate positive electrode materials doped with metal niobium prepared in Example 1 of the present invention and without metal niobium doping prepared in Comparative Example 1 were made into button-type batteries to test the capacity retention rate. The results are as follows: Figure 8As shown in Table 3, the capacity retention rate of Example 1 is higher than that of Comparative Example 1, indicating that metal niobium may stabilize the crystal structure of sodium iron phosphate pyrophosphate during the preparation process, thereby improving the capacity retention rate of the button-type battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium, that is, the cycle life; under the same test conditions, the capacity retention rate results of all embodiments and comparative examples are shown in Table 3, and the capacity retention rate provided by the button-type battery made of the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared in Example 1 of the present invention is higher than that of Comparative Example 2 without metal niobium, indicating that the doping of metal niobium can improve the capacity retention rate of the button-type battery made of the sodium iron phosphate pyrophosphate positive electrode material; Examples 5-8 of the present invention show that the sodium iron phosphate pyrophosphate positive electrode material doped with metal niobium prepared using sucrose derivatives and butyl oxamate still has a high capacity retention rate when made into a button-type battery.

[0115] The embodiments and / or implementation methods described above are only used to illustrate the preferred embodiments and / or implementation methods for realizing the technology of the present invention, and are not intended to limit the implementation methods of the technology of the present invention in any form. Any technical personnel in this field may make slight changes or modifications to other equivalent embodiments without departing from the scope of the technical means disclosed in the content of the present invention, but they should still be regarded as technologies or embodiments that are essentially the same as the present invention.

[0116] This article uses specific examples to illustrate the principles and implementation methods of this application. The description of the above embodiments is only used to help understand the method and its core ideas of this application. The above is only the preferred implementation method of this application. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, ordinary technicians in this technical field can make several improvements, modifications or changes without departing from the principles of this application, and can also combine the above technical features in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the concept and technical solution of the invention to other occasions without improvement, should be regarded as the scope of protection of this application.

Claims

1. A method for preparing a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material, comprising: The positive electrode material source and the carbon source are mixed in water, and subjected to grinding, spray drying and high-temperature annealing treatment to obtain a metal niobium element-doped sodium iron phosphate pyrophosphate positive electrode material; the positive electrode material source comprises a sodium source, an iron source, a niobium source and a phosphorus source, and the metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material has the following structure: Na x Fe y Nb m (PO4) n (P2O7); wherein x is 4, y is 2.9, m is 0.1, and n is 2; the carbon source comprises a sucrose derivative and polyethylene glycol, wherein the sucrose derivative is prepared from sucrose, 2-chloro-N,N-dimethylacetamide and acetic anhydride; In the preparation of sucrose derivatives: first, sucrose and DMAP are dissolved in pyridine, then after cooling to 45-65°C, 2-chloro-N,N-dimethylacetamide is added in batches within 1.5 hours to obtain a mixed solution, the mixed solution is heated to 50-80°C, and the reaction is continued for 0.5-6 hours; after the reaction is completed, pyridine is evaporated to obtain an initial reactant, the temperature is lowered to room temperature, acetic anhydride is added to the initial reactant, the temperature is raised to 45-60°C, and the reaction is continued for 1-8 hours to obtain a reaction mixture; then the reaction mixture is poured into ice water under stirring to precipitate a white solid, the white solid is filtered out and washed with water to remove pyridine, the white solid is dried to obtain a white powder, and finally the white powder is recrystallized with methanol / acetone in a volume ratio of 80:20 to obtain a sucrose derivative; the amount of sucrose added to pyridine is 200-400 g / L; the amount of DMAP added to pyridine is 4-8 g / L; the amount of 2-chloro-N,N-dimethylacetamide added to pyridine is 500-700 g / L; the volume ratio of acetic anhydride to pyridine added is 1:5.33-11.

2. The method for preparing a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The sodium source includes at least one of sodium carbonate, sodium oxalate, sodium acetate, sodium hydroxide, sodium citrate, sodium dihydrogen phosphate and sodium pyrophosphate; the iron source includes at least one of ferrous sulfate, ferrous oxalate, ferrous acetate, ferrous phosphate, ferric nitrate, ferric oxide and ferrous oxide; the niobium source includes at least one of niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, niobium nitrate, niobium acetate and niobium oxalate; the phosphorus source includes at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, triammonium phosphate and sodium dihydrogen phosphate.

3. The method for preparing a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The molar ratio of sodium element, iron element, niobium element and phosphorus element in the sodium source, iron source, niobium source and phosphorus source is 3.9-4.1:2.9:0.1:3.95-4.1; the mass ratio of the carbon source to the positive electrode material source is 1:2-15.

4. The method for preparing a metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The grinding is nano-sand milling, the nano-sand milling speed is 1000-2500 rpm, the sand milling time is 1-4 h, and the particle size D50 after sand milling is 100-400 nm; or, the air inlet temperature of the spray drying is 150-210 ° C, the atomizer frequency is 200-450 Hz, and the feed amount is 3-5 L / h; or, the temperature of the high temperature annealing is 450-600 ° C, and the annealing time is 8-24h.

5. The metal niobium doped sodium iron phosphate pyrophosphate positive electrode material prepared by the method according to any one of claims 1 to 4 comprises the following structure: Na x Fe y Nb m (PO4) n (P2O7); among which, x is 4, y is 2.9, m is 0.1, n is 2, and the Na x Fe y Nb m (PO4) n (P2O7) is a pure phase material.

6. A battery comprising the metal niobium-doped sodium iron phosphate pyrophosphate positive electrode material according to claim 5.

7. A vehicle comprising the battery according to claim 6.