Chiral molecular intercalation molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect and preparation method and application thereof
Through the chiral molecular intercalation of molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect, the problem of insufficient cycle stability and rate capability of aluminum sulfur battery is solved, and high cycle stability and low cost catalytic effect is achieved. Suitable for portable electronic devices and energy storage devices.
Patent Information
- Application Number
- CN202410647486.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-23
AI Technical Summary
Due to the limited oxidation capacity of aluminum polysulfide species and the slow reaction kinetics, aluminum sulfur batteries have insufficient cyclic stability and rate capabilities, and it is difficult for the prior art to prepare aluminum sulfur batteries with high cycle stability.
The chiral molecular intercalation molybdenum aluminum sulfur battery catalyst based on chiral spin selection effect is used to prepare the catalyst by a one-step hydrothermal method, and the chiral molecules and ammonium tetrathiomolybdate are used to heat the reaction in hydrochloric acid medium to form A black-brown precipitate with high catalytic activity is used to improve the sulfur oxidation process.
The high cycle stability of aluminum sulfur batteries has been achieved, the stable cycle number exceeds 3,000 turns, the capacity retention rate exceeds 75%, and the raw material cost and synthesis process complexity are reduced, making it suitable for large-scale industrial production.
Smart Images

Figure CN118630211B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a chiral molecular intercalation molybdenum disulfide aluminum sulfur battery catalyst based on a chiral spin selection effect, and a preparation method and application thereof. Background Art
[0002] With the continuous development of human society and economy, the demand for fossil resources is increasing, which leads to the depletion of resources, the continuous aggravation of environmental pollution and the increasing global greenhouse effect. The development of new technologies such as exploring new energy and reducing carbon dioxide emissions has become an extremely urgent need for mankind. Aluminum-sulfur batteries have broad prospects for practical application due to their significant cost advantages, high theoretical specific capacity and excellent safety.
[0003] However, the limited oxidation capacity of aluminum polysulfide species retards the overall reaction kinetics of aluminum-sulfur batteries. In addition, the slow reaction kinetics defect is further aggravated by the use of insulating sulfur positive electrode, high-valent metal aluminum negative electrode and ionic liquid electrolyte. These factors jointly affect the long-term cycle stability and rate capability of aluminum-sulfur batteries.
[0004] At present, it is still very challenging to prepare aluminum-sulfur batteries with high cycle stability. A large number of studies have shown that the use of catalysts with strong adsorption capacity and high catalytic activity is an effective strategy to accelerate the sulfur reaction, and new aluminum-sulfur battery positive electrode materials that can effectively improve the reaction kinetics are urgently needed. Summary of the invention
[0005] The present invention provides a chiral molecular intercalation molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect and a preparation method and application thereof. The catalyst has a chiral selection effect, low raw material cost, simple synthesis process, and extremely high catalytic activity in sulfur oxidation process.
[0006] The technical solution of the present invention is:
[0007] In the first aspect, a method for preparing a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on a chiral spin selection effect is disclosed, comprising the following steps:
[0008] S1: dissolving ammonium tetrathiomolybdate in deionized water to form a solution, adding a chiral molecule to the solution, mixing evenly, adding hydrochloric acid to adjust the pH value, and heating the solution in a protective atmosphere to form a dark brown precipitate;
[0009] S2 centrifuges the dark brown precipitate, washes it, and vacuum dries it to obtain a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on the chiral spin selective effect.
[0010] Preferably, in step S1, the chiral molecule is a L-methylbenzylamine molecule or a D-methylbenzylamine molecule, and the molar ratio of ammonium tetrathiomolybdate to the chiral molecule is 1:0.9-1;
[0011] Preferably, in step S1, the pH is adjusted to 3-4 with hydrochloric acid.
[0012] Preferably, in step S1, the protective atmosphere is argon atmosphere, the reaction temperature is 200-220° C., and the reaction time is 12-14 h.
[0013] Preferably, the centrifugal separation speed is not less than 12000 rpm, the washing liquid is deionized water and acetone, and the washing is alternately performed 2-3 times; the drying temperature is 60-80° C., and the drying time is 10-12 hours.
[0014] In the second aspect, a chiral molecular intercalation molybdenum disulfide aluminum-sulfur battery catalyst based on the chiral spin selection effect is disclosed. The overall structure of the catalyst is chiral, and the interlayer spacing of molybdenum disulfide is 0.85 to 0.92 nm.
[0015] In a third aspect, an aluminum-sulfur battery positive electrode material is disclosed, comprising a mixed material of the chiral molecular intercalated molybdenum disulfide aluminum-sulfur battery catalyst, sublimated sulfur and Ketjen black.
[0016] In a fourth aspect, an aluminum-sulfur battery is disclosed, comprising the aluminum-sulfur battery positive electrode material.
[0017] The phenomenon that electrons with different spin directions have different passing probabilities in the same chiral configuration is called the CISS effect. Theoretical calculations based on the Green's function method show that spin polarization exists in the non-equilibrium electronic structure at the interface between chiral molecules and metal atoms. 2 The key influence of the electronic structure in chiral MoS 2 It will show higher spin density and more spin-polarized electrons, and these electrons are gathered around the molybdenum atoms, which makes the chiral MoS 2 It is easier to accept or lose electrons, which indicates its excellent electron transfer ability and the potential to catalyze subsequent reactions.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The molybdenum disulfide aluminum-sulfur battery catalyst prepared by the present invention is based on the chiral spin selection effect, contains chiral molecular intercalation, and has extremely high catalytic activity in the sulfur oxidation process. The new aluminum-sulfur battery prepared using the molybdenum disulfide catalyst has high cycle stability, the number of stable cycles exceeds 3,000, and the capacity retention rate exceeds 75%.
[0020] 2. The preparation method of the present invention controls the raw materials and feed ratio, the pH of the mixed solution, the heating temperature, the washing and other conditions. The various conditions are interrelated and promote each other, so that the finally prepared catalyst has a good catalytic effect. The preparation method of the present invention is a one-step hydrothermal preparation, with low raw material cost, simple and easy synthesis process, standardized operation, convenience for large-scale industrial production, and high degree of practicality.
[0021] 3. The spin-selective effect of the chiral catalyst can accelerate the reaction activity of the aluminum-sulfur battery. While giving full play to the ultra-high capacity advantage of the aluminum-sulfur battery, it also has ultra-high cycle stability and can achieve rapid charging and discharging. It has broad application prospects in the fields of portable electronic devices and other energy storage devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the X-ray diffraction pattern of the novel molybdenum disulfide aluminum-sulfur battery catalytic material prepared in Examples 1-2 of the present invention and Comparative Example 1.
[0023] Figure 2 This is a scanning electron microscope image of the novel molybdenum disulfide aluminum-sulfur battery catalytic material prepared in Example 1 of the present invention.
[0024] Figure 3 This is a transmission electron microscope image of the novel molybdenum disulfide aluminum-sulfur battery catalytic material prepared in Example 1 of the present invention.
[0025] Figure 4 The aluminum-sulfur battery 2Ag prepared in Example 1 of the present invention under the action of the new molybdenum disulfide aluminum-sulfur battery catalytic material -1 Cycling performance diagram at different current densities.
[0026] Figure 5 The aluminum-sulfur battery 2Ag prepared in Example 2 of the present invention under the action of the new molybdenum disulfide aluminum-sulfur battery catalytic material -1 Cycling performance diagram at different current densities.
[0027] Figure 6 The aluminum-sulfur battery 2Ag prepared in the comparative example 1 of the present invention under the action of the new molybdenum disulfide aluminum-sulfur battery catalytic material -1 Cycling performance diagram at different current densities. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0029] Example 1
[0030] This embodiment provides a chiral molecular intercalation molybdenum disulfide aluminum sulfur battery catalyst based on the chiral spin selection effect, and the preparation method thereof is as follows:
[0031] Dissolve 66 mg of ammonium tetrathiomolybdate in 20 mL of deionized water. After fully dissolving, add 32.3 μL of dextrorotatory methylbenzylamine (R-MBA) to the solution to ensure that the molar ratio of the added chiral molecule to the added ammonium tetrathiomolybdate is 1:1. After uniform mixing, add hydrochloric acid to adjust the pH value to 3. Pour the solution into a high-pressure sealed reactor, fill with argon as a protective gas, heat at 200 ° C, and react for 14 h.
[0032] After the heating is completed, the solution is cooled naturally, and the dark brown precipitate in the solution is centrifuged and vacuum dried. The centrifugal separation speed is 12000rpm. Deionized water and acetone are used for alternating washing 3 times each. The drying temperature is 60°C and the drying time is 12h to obtain a molybdenum disulfide sulfur battery catalyst based on the chiral spin selection effect.
[0033] The X-ray diffraction pattern of the novel molybdenum disulfide aluminum-sulfur battery catalyst material prepared in Example 1 is as follows: Figure 1 As shown in the figure, it can be seen that Example 1 prepares pure phase intercalated molybdenum disulfide. It can be clearly seen that the 002 peaks shown in Examples 1-2 and Comparative Example 1 are significantly shifted to a small angle, proving that the three different organic molecules are successfully inserted, and the X-ray diffraction patterns of the three materials are basically the same, proving that the difference in organic molecules does not affect the intercalated MoS 2 The scanning electron microscope image and transmission electron microscope image of the novel molybdenum disulfide aluminum sulfur battery catalyst material prepared in Example 1 are as follows: Figure 2 and Figure 3 As shown, it is proved that the new molybdenum disulfide aluminum-sulfur battery catalytic material prepared in Example 1 is in the shape of a flower ball as a whole, and the chiral molecules are inserted into the molybdenum disulfide interlayer, and the distance between the molybdenum disulfide interlayers is 0.85nm. -1 The cycling performance at current density is Figure 4 As shown, it can be seen that the number of stable cycles of the aluminum-sulfur battery under the action of the new molybdenum disulfide aluminum-sulfur battery catalytic material exceeds 3,000 cycles, and the capacity retention rate exceeds 75%.
[0034] Example 2
[0035] This embodiment provides a chiral molecular intercalation molybdenum disulfide aluminum sulfur battery catalyst based on the chiral spin selection effect, and the preparation method thereof is as follows:
[0036] Dissolve 66 mg of ammonium tetrathiomolybdate in 20 mL of deionized water. After it is fully dissolved, add 32.3 μL of L-methylbenzylamine (S-MBA) to the solution, ensuring that the molar ratio of the added chiral molecule to the previously added ammonium tetrathiomolybdate is 1:1. After uniform mixing, add hydrochloric acid to adjust the pH value to 3. Pour the solution into a high-pressure sealed reactor, fill it with argon as a protective gas, heat it at 220°C, and react for 14 hours.
[0037] After the heating is completed, the solution is cooled naturally, and the dark brown precipitate in the solution is centrifuged and vacuum dried. The centrifugal separation speed is 12000rpm. Deionized water and acetone are used for alternating washing 3 times. The drying temperature is 80°C and the drying time is 10h to obtain a molybdenum disulfide sulfur battery catalyst based on the chiral spin selection effect.
[0038] Comparative Example 1
[0039] The difference from Example 1 is that in this comparative example, the dextrorotatory methylbenzylamine molecule is replaced by the exo-elimination methylbenzylamine molecule, and the rest is the same as Example 1.
[0040] Comparative Example 2
[0041] The difference from Example 1 is that in this comparative example, the dextrorotatory methylbenzylamine molecule is replaced by a dextrorotatory tryptophan molecule, and the rest is the same as Example 1.
[0042] Comparative Example 3
[0043] The difference from Example 1 is that the amount of dextrorotatory methylbenzylamine molecules added is 29 μL, the amount of ammonium tetrathiomolybdate added is 66 mg, and the rest is the same as Example 1.
[0044] Comparative Example 4
[0045] The difference from Example 1 is that hydrochloric acid is added to adjust the pH to 5, and the rest is the same as Example 1.
[0046] Comparative Example 5
[0047] The difference from Example 1 is that the reaction temperature is 230° C., and the rest is the same as Example 1.
[0048] Comparative Example 6
[0049] The difference from Example 1 is that ethanol is used for washing, and the rest is the same as Example 1.
[0050] The catalysts prepared in Examples 1-2 and Comparative Examples 1-6 were used to prepare positive electrode materials, and assembled into aluminum-sulfur batteries for performance testing. The specific method is as follows: 20 mg of the catalysts prepared in Examples 1-2 and Comparative Examples 1-6 were mixed with 80 mg of Ketjen black, 20 mL of deionized water was added to form a suspension, ultrasonic treatment was performed for 5 min to fully mix, and the mixture was dried in an oven at a temperature of 80° C. for 10 h until completely dry. 100 mg of sublimated sulfur and the dried mixed powder were placed in a 5 mL high-pressure sealed reactor, filled with argon as a protective gas, heated at 155° C. for 14 h, and taken out after natural cooling to obtain an aluminum-sulfur battery electrode active material. 70wt% electrode active material, 20wt% conductive additive (Super-P carbon black) and 10wt% polyvinylidene fluoride (PVDF) were fully mixed in a mortar, and an appropriate amount of N-methylpyrrolidone (NMP) was added to form a slurry (when the amount of electrode active material was 70mg, the amount of NMP was 3mL), and cast onto a molybdenum sheet with a scraper, and the scraper thickness parameter was 0.1mm. Then the molybdenum sheet was placed in a vacuum oven and dried at 60°C for 10h to evaporate the residual NMP solvent. The dried molybdenum sheet was cut into a 1cm diameter original sheet with a tablet press as the positive electrode material of the aluminum-sulfur battery, an aluminum sheet of the same size was used as the negative electrode, a glass fiber filter paper (GF / A) with a diameter of 1.8cm was used as a diaphragm, and AlCl 3 / urea ionic liquid as the electrolyte. 2 and H 2 O<0.1ppm) in a glove box, the electrodes, separators and electrolytes were assembled into 2032 button cells, i.e., the aluminum-sulfur batteries. A Xinwei battery test system (CT-4008T-5V20 mA-164, Shenzhen, China) was used to test the battery at 1.2 to 2.4 V (relative to Al 3+ / Al) were used for constant current charge and discharge measurement at room temperature with a current of 2Ag -1 All batteries were left to rest for 10 h before testing.
[0051] The aluminum-sulfur battery prepared by using the catalysts of Examples 1-2 and Comparative Examples 1-6 was -1 The cycle performance under current density, the test results are shown in Table 1:
[0052] Table 1
[0053] <![CDATA[2Ag -1 Number of cycles at current density]]> Capacity retention rate Example 1 3000 75% Example 2 3000 75% Comparative Example 1 500 15% Comparative Example 2 2000 70% Comparative Example 3 2500 70% Comparative Example 4 1000 50% Comparative Example 5 500 10% Comparative Example 6 500 15%
[0054] Compared with Example 1, in Comparative Example 1, the right-handed methylbenzylamine molecule is replaced with an exogenous methylbenzylamine molecule. Since the exogenous methylbenzylamine molecule does not have a chiral structure and cannot trigger the CISS effect, there is no catalytic effect; in Comparative Example 2, the chiral molecule is replaced with a right-handed tryptophan molecule. Since the tryptophan molecular chain length is shorter than that of the methylbenzylamine molecule, the CISS effect produced is weak and the catalytic performance is poor; in Comparative Example 3, the molar ratio of the chiral molecule to ammonium tetrathiomolybdate is 0.9:1. The reduction of the chiral molecule weakens the density of the chiral structure, weakens the CISS effect, and the catalytic performance is weak; in Comparative Example 4, the pH value is adjusted to 5. The acidity of the reaction solution greatly affects the dispersion degree of MoS2 during the hydrothermal decomposition and molecular intercalation process. The higher the acidity, the better the dispersion degree. However, if the acidity is too large, the organic molecules will be inactivated. When the pH value is 5, there will be more MoS 2 Agglomeration affects the effect of molecular intercalation; in Comparative Example 5, the reaction temperature is adjusted to 230°C. Too high a temperature will inactivate the organic molecules and lose their spatial structure, affecting the final battery performance; in Comparative Example 6, the washing solvent is replaced with ethanol. Organic chiral molecules are easily soluble in ethanol, which will destroy the chiral MoS 2 The intercalation structure affects the catalytic effect.
[0055] Although the present invention has been described in detail by combining the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect, characterized in that: The following steps are involved: S1: dissolving ammonium tetrathiomolybdate in deionized water to form a solution, adding a chiral molecule to the solution, mixing evenly, adding hydrochloric acid to adjust the pH value, and heating the solution in a protective atmosphere to form a dark brown precipitate; S2 centrifuges the dark brown precipitate, washes it, and vacuum dries it to obtain a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on the chiral spin selective effect.
2. The method for preparing a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect according to claim 1, characterized in that: In step S1, the chiral molecule is a left-handed methylbenzylamine molecule or a right-handed methylbenzylamine molecule, and the molar ratio of ammonium tetrathiomolybdate to the chiral molecule is 1:0.9-1.
3. The method for preparing a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect according to claim 1, characterized in that: In step S1, hydrochloric acid is used to adjust the pH to 3-4.
4. The method for preparing a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect according to claim 1, characterized in that: In step S1, the protective atmosphere is argon atmosphere, the reaction temperature is 200-220° C., and the reaction time is 12-14 h.
5. The method for preparing a chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect according to claim 1, characterized in that: The centrifugal separation speed is not less than 12000rpm, the washing liquid is deionized water and acetone, and the washing is alternately performed 2 to 3 times; the drying temperature is 60 to 80°C, and the drying time is 10-12h.
6. A chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst based on chiral spin selection effect prepared by the method according to any one of claims 1 to 5, characterized in that: The overall structure of the catalyst is chiral, and the interlayer spacing of molybdenum disulfide is 0.85 to 0.92 nm.
7. An aluminum-sulfur battery positive electrode material, characterized in that: The invention comprises a mixed material of the chiral molecular intercalated molybdenum disulfide aluminum sulfur battery catalyst as claimed in claim 6, sublimated sulfur and Ketjen black.
8. An aluminum-sulfur battery, characterized in that: Including the aluminum-sulfur battery positive electrode material as described in claim 7.