High entropy alloy hydride catalyst for carbon dioxide methanation and preparation method thereof
By combining high-entropy alloy hydride catalyst with magnesium nitride film, the preparation is done by aerosolizing in situ reaction, the problems of active inactivation and carbon deposits of traditional catalysts at high temperatures are solved, and high-efficiency carbon dioxide conversion is achieved at low temperatures. Catalytic activity and stability, suitable for industrial applications.
Patent Information
- Application Number
- CN202411107567.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing carbon dioxide methanation catalysts are active inactivated at high temperatures and are prone to carbon accumulation, resulting in catalyst failure. It is difficult for traditional catalysts to achieve efficient conversion at low temperatures, and there are kinetic and thermodynamic limitations.
Using a high-entropy alloy hydride catalyst, composed of MgCuNixTiY hydride and magnesium nitride film, prepared by aerosolization in situ reaction to form a spherical particle catalyst, with high specific surface area and stability, and the magnesium nitride film prevents carbon deposits and disparity. reaction.
Under normal pressure and 200°C, the high-efficiency carbon dioxide conversion rate is more than 95%, the catalytic activity remains stable, which is significantly better than traditional catalysts, suitable for industrial production and has a high catalytic life.
Smart Images

Figure CN118634866B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of energy and environmental catalysis, and in particular relates to a high entropy alloy hydride catalyst for carbon dioxide methanation and a preparation method thereof. Background Art
[0002] According to statistics, from 1850 to 2018, the global average temperature has risen by more than 1°C. The use of fossil fuels is the culprit for the sharp increase in greenhouse gas emissions, of which carbon dioxide accounts for about three-quarters of the total greenhouse gas emissions, leading to a series of ecological and environmental problems such as global warming and ocean acidification. The energy problem and the ecological and environmental problem are equally severe. CO2 has the characteristics of being cheap, easily available, abundantly renewable, clean and non-toxic. It is an ideal and high-quality carbon-one resource for various high-value-added chemicals. Therefore, its reduction and conversion can not only alleviate the environmental problems caused by the greenhouse effect, but also provide a solution to the problem of energy depletion.
[0003] The stable thermodynamic properties and kinetic inertness of CO2 are the key obstacles to its direct conversion into high value-added chemicals. CO2 is a typical linear symmetrical triatomic molecule with 16 valence electrons. Its three atoms all contain ns and np orbitals. The bonding mode of the C atom in the molecule is sp hybrid orbital bonding with O atom. Two σ bonds plus two delocalized π bonds form (1σ g ) 2 (1σ u ) 2 (2σ g ) 2 (2σ u ) 2 (1π u ) 4 (1π g ) 4 (2π u ) 0 The electronic configuration of CO2. It can be seen from its electronic configuration that there are multiple potential activation sites in the CO2 molecule, among which the carbon shows Lewis acid properties and can serve as an electrophilic center, and the oxygen shows Lewis base properties and can serve as a nucleophilic center. The first ionization energy of CO2 (13.79eV) is significantly greater than that of COS, CS2 and N2O with isoelectronic configuration, making it a weak electron donor and not easy to form CO2 + ; However, since CO2 has a lower energy level empty orbital (2πu) and a higher electron affinity (38eV), it exhibits strong electron acceptor properties and is easy to form CO2 − Therefore, as long as electrons are input in an appropriate manner or electrons from other molecules are captured during the reaction, the activation and conversion of inert CO2 molecules can be achieved.
[0004] The carbon dioxide methanation reaction is also called the Sabatier reaction, and the reaction equation is as follows:
[0005] CO2+4H2→CH4+2H2O, ΔH=-252.9kJ·mol -1
[0006] The reaction is thermodynamically favorable and exothermic (ΔG 298K =-130.8 kJ·mol -1 ), so from a thermodynamic point of view, low temperature is conducive to the reaction; however, the reduction of CO2 to methane has significant kinetic limitations, so it is usually necessary to use a catalyst to accelerate the kinetic conversion reaction rate of CO2 at a relatively low temperature in order to obtain a considerable methane yield. The selected catalyst must have good catalytic activity and stability for the dissociation of H2 molecules and CO2 molecules. Taking Ni-based catalysts as an example, Ni / Al2O3 catalysts are the most popular carbon dioxide methanation catalysts. Compared with other catalysts, Ni is cheap and has high catalytic activity for carbon dioxide methanation. However, Ni-based catalysts also have disadvantages. Due to their high catalytic temperature (300-450°C), excessive reaction heat will deactivate the active components of the catalyst. In addition, as the reaction process proceeds, carbon deposition is prone to occur on the catalyst surface, which blocks the surface active sites and catalyst pores, and eventually leads to catalyst deactivation. It can be seen that although great progress has been made in the catalyst for carbon dioxide methanation, there is still a long way to go before industrialization, and there is still a long way to go to find catalysts with high catalytic activity and high stability. In recent years, high entropy alloy catalysts have attracted great attention due to their unique high entropy structural stability, slow diffusion effect and cocktail effect (multi-principal component synergistic catalytic effect) and other special properties. The gas atomization method is to prepare catalyst alloy powder, which uses high-pressure and high-speed airflow to act on the molten alloy liquid flow. When the alloy liquid passes through the nozzle, it meets the high-speed airflow and is atomized into fine droplets, converting the kinetic energy of the high-speed gas into the surface energy of the droplets, and then breaking the melt into fine droplets and rapidly solidifying and cooling to form powder. Gas atomization powder preparation has the advantages of low environmental pollution, simple process, and fast cooling speed. The prepared catalyst alloy powder has the advantages of high sphericity, uniform composition, fine grains, and controllable powder particle size. It is especially suitable for the preparation of multi-component high entropy alloy catalysts with high specific surface area and high catalytic activity. The nozzle is the core component of the gas atomization equipment, which determines the key technical indicators of the prepared metal powder, such as diameter distribution, hollow ratio, satellite powder ratio, etc. The gas atomization nozzle is mainly divided into a tightly coupled nozzle and a free fall nozzle. The tightly coupled annular gap nozzle can greatly shorten the distance between the gas jet and the metal liquid flow at the outlet of the guide tube, and significantly improve the atomization efficiency.
[0007] The introduction of metal hydride hydrogen storage materials into the reaction system has played an inspiring role in solving the contradiction between the thermodynamics and kinetics of the CO2 methanation reaction. As a classic solid-state hydrogen storage material, metal hydride (MH) has unique reversible hydrogen absorption and desorption properties. During the hydrogen absorption process, H2 is adsorbed and dissociated on the surface of MH and diffuses into the bulk phase. The abundant hydrogen species on the surface and in the bulk phase promote hydrogen-related catalytic processes, while the dehydrogenation process is the opposite. This process can be used to regulate the hydrogen intermediates of chemical reactions and catalyze hydrogen-containing reactions. The negatively charged hydrogen atoms of metal hydrides have stronger reducing properties and can provide free electrons for the activation of CO2, thereby possibly achieving CO2 methanation at a lower temperature. The catalytic application research of MH began with simple hydrocarbon hydrogenation and dehydrogenation reactions. In recent years, it has gradually shown unique catalytic potential in important energy and environmental catalytic reactions such as NH3 synthesis, CO2 hydrogenation, and liquid organic hydrogen carrier (LOHC) hydrogen storage. MH catalysts have three outstanding advantages: (1) providing additional hydrogen and hydrogen transfer pathways; (2) changing the catalytic reaction mechanism; and (3) regulating the electronic structure of the catalyst. In his paper "CO2hydrogenation on a metal hydride surface", Andreas Zuttel studied the catalytic hydrogenation reaction of CO2 on the surface of metal hydride MgNiH4. CO2 molecules dissociated significantly on the surface of MgNiH4, and the CO2 methanation conversion reaction occurred significantly at 600 K. However, as the conversion reaction proceeded, the disproportionation reaction of MgNiH4 occurred. After 18 CO2 methanation conversion reactions, MgNiH4 decomposed to form MgO, Ni and MgNi2, resulting in a significant decrease in the amount of hydrogen absorption and desorption during the subsequent reaction. It was difficult for hydrogen molecules to share electrons with surface metal atoms, and the dissociation rate of hydrogen molecules and CO2 molecules decreased. In addition, the thicker oxide layer reduced the diffusion of hydrogen on the surface. Therefore, it is urgent to provide a carbon dioxide methanation catalyst with high catalytic activity and high stability and to develop a preparation method that is easy to achieve large-scale production. Summary of the invention
[0008] In order to solve the shortcomings and deficiencies of the prior art, the primary object of the present invention is to provide a high entropy alloy hydride catalyst for carbon dioxide methanation with extremely high catalytic conversion activity and high stability.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] A high entropy alloy hydride catalyst for carbon dioxide methanation, wherein the high entropy alloy hydride catalyst for carbon dioxide methanation consists of a high entropy alloy hydride phase and a magnesium nitride phase; the high entropy alloy hydride is MgCuNi xTiY hydride, MgCuNi x The TiY hydride is a spherical particle with a single-phase body-centered cubic BCC crystal structure, wherein, in atomic percentage, 0.5≤x≤1.0; the magnesium nitride is a thin film coated on the surface of the high-entropy alloy hydride spherical particle, the film layer is rough, uneven and discontinuous, and the film layer thickness is 0.01-0.15 μm.
[0011] Preferably, the high entropy alloy hydride catalyst can absorb and release hydrogen without being activated, and the amount of hydrogen absorbed and released is 0.552-0.869 wt.%.
[0012] The D50 average particle size of the high entropy alloy hydride catalyst for carbon dioxide methanation of the present invention is 15-25 μm.
[0013] Another object of the present invention is to provide a method for preparing the high entropy alloy hydride catalyst for carbon dioxide methanation, the method comprising the following steps:
[0014] (1) Weigh raw materials magnesium block, copper block, nickel block, titanium block and yttrium block according to the atomic ratio of Mg: Cu: Ni: Ti: Y = 1: 1: x: 1: 1, where 0.5≤x≤1.0;
[0015] (2) placing the raw materials prepared in step (1) into an induction melting furnace in sequence, and melting them under argon protection to obtain an alloy melt;
[0016] (3) The alloy melt obtained in step (2) is poured into a tundish with a φ5 mm leak hole at the bottom through a guide tube under argon protection, and a high-pressure nitrogen-hydrogen mixed gas is turned on to start atomization. The alloy melt and the mixed gas react in situ by gas atomization to generate MgCuNi x TiY hydride spherical particles and coated on MgCuNi x A magnesium nitride film on the surface of TiY hydride spherical particles; the volume percentage of hydrogen in the nitrogen-hydrogen mixed gas is 25%; the nozzle used for gas atomization is a tightly coupled annular gap nozzle;
[0017] (4) After atomization, the MgCuNi x TiY hydride spherical particles and coated on MgCuNi x The magnesium nitride film product on the surface of the TiY hydride spherical particles is cooled and sieved under a nitrogen protective atmosphere to obtain a high entropy alloy hydride catalyst.
[0018] Preferably, in step (2), the raw materials are placed in the order of copper block, titanium block, nickel block, yttrium block and magnesium block; the induction melting furnace is evacuated to 1.0~2.0×10 -3 Pa; the pressure range of protective gas argon is 1.0~1.2×10 5Pa; melting temperature range 1300~1450℃.
[0019] Preferably, the pressure of the high-pressure nitrogen-hydrogen mixed gas in step (3) is in the range of 1.5-10.0 MPa.
[0020] Preferably, the pressure range of the protective gas nitrogen in step (4) is 1.0-1.2×10 5 Pa.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The first innovation of the present invention is the first high entropy alloy hydride catalyst for carbon dioxide methanation. The unique high entropy structural stability and multi-principal synergistic catalytic effect of the high entropy system are utilized. Under the mild conditions of normal pressure (~1 bar) and 200°C, after continuous carbon dioxide methanation conversion for 100 hours, the phase structure of the high entropy alloy hydride catalyst remains stable, and the carbon dioxide conversion rate exceeds 95% and remains basically constant. The discontinuous, uneven, and rough magnesium nitride film on the surface of the high entropy alloy hydride catalyst is conducive to the adsorption of CO2 molecules, while H2 molecules can easily pass through the rough magnesium nitride film and dissociate into H atoms under the catalytic action of the active metal sites. The highly active H atoms enter the high entropy alloy lattice and combine with it to form a high entropy alloy hydride MH. The CO2 molecules adsorbed on the surface of the high entropy alloy hydride catalyst accept the electrons of the negatively charged H atoms in the surface high entropy alloy hydride and are reduced. The negatively charged bulk H inside continuously diffuses to the surface to promote the continuous reduction of CO2 to methane. At the same time, the discontinuous, uneven and rough magnesium nitride film on the surface of the catalyst particles prevents the occurrence of carbon deposition and the blockage of surface active sites and catalyst pores, while delaying and isolating the contact between H2O molecules and high entropy alloy hydride to avoid the occurrence of disproportionation reaction. The second innovation is the gas atomization in-situ reaction preparation process of high-entropy alloy hydride catalysts. A high-pressure nitrogen-hydrogen mixture is used to impact a high-entropy alloy liquid flow at a temperature above 1000°C at high speed through a tightly coupled annular gap nozzle. While the high-entropy alloy liquid flow is impacted into ultrafine droplets and rapidly solidified to form a spherical powder with high sphericity, uniform composition and fine grains, N2 undergoes an in-situ nitridation reaction with the active element magnesium in the high-entropy alloy to form a discontinuous, uneven and rough magnesium nitride film on the surface of the ultrafine droplets. H2 undergoes an in-situ hydrogenation reaction both during the impact on the liquid flow and during the falling of the droplets. The H2 molecules dissociate into H atoms with the smallest atomic radius, which can easily penetrate into the lattice gaps to form high-entropy alloy hydrides, realizing a one-step, efficient and large-scale preparation of high-entropy alloy hydride catalysts with high specific surface area and high catalytic activity.
[0023] The high entropy alloy hydride catalyst for carbon dioxide methanation provided by the present invention is applied to carbon dioxide methanation conversion reaction under mild conditions, can obtain relatively excellent catalytic conversion performance under mild conditions of normal pressure and 200° C., and the carbon dioxide conversion rate can reach 97.8%. No gas products other than methane are detected in the gas chromatography, and after 100 hours of methanation conversion reaction, the catalytic activity of the high entropy alloy hydride catalyst remains stable and basically unchanged, which is significantly better than traditional carbon dioxide methanation catalysts and has extremely high catalytic conversion activity and catalytic life.
[0024] The invention adopts a gas atomization in-situ reaction preparation process to prepare a high entropy alloy hydride catalyst in one step. The preparation method is simple and efficient, green and pollution-free throughout the process, the raw materials used are cheap and easily available, and the catalyst is suitable for process operation and large-scale industrial production. It has broad industrial application prospects and significant application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 X-ray diffraction (XRD) patterns of the high entropy alloy hydride catalyst for carbon dioxide methanation prepared in Example 1, the catalyst prepared in the comparative example, and the high entropy alloy hydride catalyst for carbon dioxide methanation prepared in Example 1 after 100 hours of methanation reaction;
[0026] Figure 2 The scanning electron microscope (SEM) morphology of the high entropy alloy hydride catalyst for carbon dioxide methanation prepared in Example 2;
[0027] Figure 3 The scanning electron microscope (SEM) morphology of the high entropy alloy hydride catalyst for carbon dioxide methanation prepared in Example 3;
[0028] Figure 4 The scanning electron microscope (SEM) morphology of the catalyst prepared in the comparative example;
[0029] Figure 5 This is a comparison chart of the catalytic conversion performance of the high entropy alloy hydride catalyst for carbon dioxide methanation in Example 1 and the catalyst prepared in the comparative example after 100 hours of reaction;
[0030] Figure 6 The figure is a comparison chart of the carbon dioxide conversion rate at different temperatures of the high entropy alloy hydride catalyst for carbon dioxide methanation in Example 1 and the catalyst prepared in the comparative example (the catalyst activity evaluation is carried out on a fixed bed reactor at atmospheric pressure, the reaction gas H2 / CO2 molar ratio is 4, the reaction tail gas is passed through a condenser to remove the water vapor produced by the reaction, and then passed through a drying tube (filled with CaSO4 as a desiccant) for drying before entering an Agilent online gas chromatograph (Agilent7890A) for real-time online analysis of the tail gas to determine the gaseous products of the CO2 methanation reaction). DETAILED DESCRIPTION
[0031] For a better understanding of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments. However, the protection scope of the present invention is not limited to the description scope of the embodiments.
[0032] In the following embodiments of the present invention, the induction melting furnace used is composed of a melting power supply, an induction coil, a melting crucible, etc., which are located together with the tundish in a closed circular melting furnace body, and the furnace body is provided with vacuum and gas filling pipeline interfaces. Example
[0033] Weigh 99% pure raw materials of magnesium, copper, nickel, titanium and yttrium according to the atomic ratio of Mg: Cu: Ni: Ti: Y=1: 1: 1: 1, and load them in the order of copper, titanium, nickel, yttrium and magnesium. Close the door of the induction melting furnace and evacuate the furnace to 1.0×10 -3 Pa, and fill the furnace with 1.0×10 5 Pa pressure argon gas, heated to 1400 ℃ under argon protection for smelting to obtain alloy melt; the obtained alloy melt was poured into a tundish with a φ5mm leak hole at the bottom through a guide tube under argon protection, and a high-pressure nitrogen-hydrogen mixture gas with a hydrogen volume percentage of 25% was opened to start atomization. The atomization pressure of the high-pressure nitrogen-hydrogen mixture gas was 6.0MPa, and the nozzle used for gas atomization was a tightly coupled annular gap nozzle; a gas atomization in-situ nitridation reaction occurred during the impact of the nitrogen in the high-pressure mixture gas on the alloy melt, generating a discontinuous, uneven, rough magnesium nitride film, which was coated on the surface of the high-entropy alloy hydride particles, and the film thickness was 0.1μm. The hydrogen in the high-pressure nitrogen-hydrogen mixture gas impacted the alloy melt and the droplets fell. In-situ hydrogenation reaction occurred to generate MgCuNiTiY high-entropy alloy hydride; after the powder was completely cooled after atomization, it was heated to 1.0×10 5 The single-phase body-centered cubic BCC high entropy alloy hydride catalyst spherical powder was obtained by sieving under a nitrogen protective atmosphere with a pressure of 1.4 Pa. The magnesium nitride content was too low to show the corresponding XRD diffraction peak. The D50 average particle size of the catalyst powder was 25 μm. The high entropy alloy hydride catalyst can absorb and desorb hydrogen without activation, and the amount of hydrogen absorbed and desorbed is 0.552 wt.%.
[0034] The high entropy alloy hydride catalyst of this embodiment is applied to the carbon dioxide methanation conversion reaction under mild conditions, and excellent catalytic conversion performance can be obtained under mild conditions of normal pressure and 200° C. The maximum carbon dioxide conversion rate can reach 97.8%, and no gas products other than methane are detected in the gas chromatography. Moreover, after 100 hours of methanation conversion reaction, the catalytic activity remains stable and basically unchanged, which is significantly better than traditional carbon dioxide methanation catalysts and has extremely high catalytic conversion activity and catalytic life.
[0035] Example 2
[0036] Weigh 99.5% pure raw materials of magnesium, copper, nickel, titanium and yttrium according to the atomic ratio of Mg: Cu: Ni: Ti: Y = 1: 1: 0.5: 1: 1, and load them in the order of copper, titanium, nickel, yttrium and magnesium. Close the door of the induction melting furnace and evacuate the furnace to 1.5×10 -3 Pa, and fill the furnace with 1.1×10 5 Pa pressure argon gas, under the protection of argon gas, the temperature is raised to 1300 ℃ for smelting to obtain an alloy melt; the obtained alloy melt is poured into a tundish with a φ5mm leak hole at the bottom through a guide tube under the protection of argon gas, and at the same time, a high-pressure nitrogen-hydrogen mixture gas with a hydrogen volume percentage of 25% is opened to start atomization, the atomization pressure of the high-pressure nitrogen-hydrogen mixture gas is 1.5MPa, and the nozzle used for gas atomization is a tightly coupled annular gap nozzle; gas atomization in-situ nitridation reaction occurs during the impact of nitrogen in the high-pressure mixed gas on the alloy melt, generating a discontinuous, uneven, rough magnesium nitride film, which is coated on the surface of the high-entropy alloy hydride particles, and the film thickness is 0.01μm. In-situ hydrogenation reaction occurs during the impact of hydrogen in the high-pressure nitrogen-hydrogen mixture gas on the alloy melt and during the droplet falling process to generate MgCuNi 0.5 TiY high entropy alloy hydride; after the atomization is completed, wait for the powder to cool completely and then 5 The body-centered cubic BCC single-phase high entropy alloy hydride catalyst spherical powder was obtained by sieving under a nitrogen protective atmosphere at a pressure of Pa. Figure 2 It can be seen that the average particle size D50 of the powder is 15 μm; the high entropy alloy hydride catalyst can absorb and release hydrogen without activation, and the amount of hydrogen absorbed and released is 0.869 wt.%. The high entropy alloy hydride catalyst of this embodiment is applied to the carbon dioxide methanation conversion reaction under mild conditions, and a better catalytic conversion performance can be obtained under mild conditions of normal pressure and 200°C, and the maximum carbon dioxide conversion rate can reach 95.4%. No gas products other than methane are detected in the gas chromatography, and after 100 hours of methanation conversion reaction, the catalytic activity remains stable and basically unchanged, which is significantly better than the traditional carbon dioxide methanation catalyst and has extremely high catalytic conversion activity and catalytic life. Example 3
[0037] Weigh 99% pure raw materials of magnesium, copper, nickel, titanium and yttrium according to the atomic ratio of Mg: Cu: Ni: Ti: Y = 1: 1: 0.75: 1: 1, and load them in the order of copper, titanium, nickel, yttrium and magnesium. Close the door of the induction melting furnace and evacuate the furnace to 2.0×10 -3 Pa, and fill the furnace with 1.2×10 5Pa pressure argon gas, heated to 1450 ℃ under argon protection for smelting to obtain an alloy melt; the obtained alloy melt is poured into a tundish with a φ5mm leak hole at the bottom through a guide tube under argon protection, and a high-pressure nitrogen-hydrogen mixture gas with a hydrogen volume percentage of 25% is opened to start atomization. The atomization pressure of the high-pressure nitrogen-hydrogen mixture gas is 10.0MPa, and the nozzle used for gas atomization is a tightly coupled annular gap nozzle; a gas atomization in-situ nitridation reaction occurs during the impact of nitrogen in the high-pressure nitrogen-hydrogen mixture gas on the alloy melt, generating a discontinuous, uneven, rough magnesium nitride film, which is coated on the surface of the high entropy alloy hydride particles, and the film thickness is 0.15μm, such as Figure 3 As shown in the figure, the hydrogen in the high-pressure nitrogen-hydrogen mixture gas impacts the alloy melt and the droplets fall, and in-situ hydrogenation reaction occurs to generate MgCuNi 0.75 TiY high entropy alloy hydride; after the powder is completely cooled after atomization, 5 The catalyst was sieved under a nitrogen protective atmosphere at a pressure of 1.3 Pa to obtain a body-centered cubic BCC single-phase high-entropy alloy hydride catalyst spherical powder, the average particle size of which was 18 μm. The high-entropy alloy hydride catalyst could absorb and release hydrogen without activation, and the amount of hydrogen absorbed and released was 0.673 wt.%. The high-entropy alloy hydride catalyst of this embodiment was applied to the carbon dioxide methanation reaction under mild conditions, and a better catalytic conversion performance could be obtained under mild conditions of normal pressure and 200°C. The maximum carbon dioxide conversion rate could reach 96.3%, and no gaseous products other than methane were detected in the gas chromatogram. After 100 h of methanation reaction, the catalytic activity remained stable and basically unchanged, which was significantly better than the traditional carbon dioxide methanation catalyst and had extremely high catalytic conversion activity and catalytic life. Comparative Example 1
[0038] Weigh 99% pure raw materials of magnesium, copper, nickel, titanium and yttrium according to the atomic ratio of Mg: Cu: Ni: Ti: Y=1: 1: 1: 1, and load them in the order of copper, titanium, nickel, yttrium and magnesium. Close the door of the induction melting furnace and evacuate the furnace to 1.0×10 -3 Pa, and fill the furnace with 1.0×10 5 Pa pressure argon gas, heated to 1400℃ under argon protection for smelting to obtain alloy melt; the obtained alloy melt was poured into the tundish with a φ5mm leak hole at the bottom through the guide pipe, and at the same time, 6.0MPa high pressure argon gas was turned on to start atomization, and the nozzle used for gas atomization was a tightly coupled annular gap nozzle; after the powder was completely cooled after atomization, it was heated to 1.0×10 5 The single-phase body-centered cubic BCC high entropy alloy MgCuNiTiY spherical powder was obtained by sieving under a nitrogen atmosphere with a pressure of 1.3 Pa. The average particle size of the powder was 30 μm. Figure 4The scanning electron microscope image of the high entropy alloy MgCuNiTiY particles shows that the particle surface is smooth, and traces of dendrite contraction when the high entropy alloy melt solidifies remain on the surface. The high entropy alloy catalyst of this embodiment is applied to the carbon dioxide methanation reaction under mild conditions. Under mild conditions of normal pressure and 200°C, the maximum carbon dioxide conversion rate is 59.3%, and no gas products other than methane are detected in the gas chromatography. After 100 hours of methanation reaction, the carbon dioxide conversion rate drops to 48.7%. Figure 5 The catalytic conversion performance comparison diagram of the catalyst of Example 1 and the comparative catalyst after 100 hours of reaction. Compared with the catalyst prepared in Example 1, the smooth surface of the high entropy alloy MgCuNiTiY catalyst prepared in the comparative example is more difficult to adsorb and activate CO2 molecules, and although H2 molecules can dissociate into H atoms on the surface of the active site of the MgCuNiTiY high entropy alloy to generate hydrides on the surface, it is difficult for H atoms to diffuse and migrate into the dense alloy, and it is not possible to fully provide negatively charged H atoms for the reduction of CO2 molecules, resulting in a decrease in the CO2 conversion rate. In addition, during the long-term methanation catalytic reaction, due to the lack of isolation and barrier of the surface magnesium nitride layer, H2O molecules are easy to contact the surface high entropy alloy hydrides, causing the occurrence of disproportionation reaction, resulting in a significant reduction in the catalytic life of the high entropy alloy.
[0039] Depend on Figure 1 From the X-ray diffraction (XRD) comparison patterns, it can be seen that the catalysts prepared in Example 1 and the comparative example are both single-phase body-centered cubic BCC structures. However, compared with the comparative example, the (110) and (200) crystal plane diffraction peaks of the high entropy alloy hydride catalyst in Example 1 are significantly shifted to the right, indicating that hydrogen atoms enter the high entropy alloy lattice to generate hydrides, causing the high entropy alloy lattice to deform, resulting in a decrease in the crystal plane spacing and the lattice constant, thereby causing the (110) and (200) crystal plane diffraction peaks to shift to the right; the X-ray diffraction (XRD) pattern of the high entropy alloy hydride catalyst after 100h of methanation reaction shows that it still maintains a single-phase body-centered cubic BCC crystal structure and no disproportionation reaction occurs, indicating that the high entropy alloy hydride catalyst has high structural stability. At the same time, it can be seen from the diffraction peak shape that the product diffraction peak width after 100h of methanation reaction is broadened, showing an amorphous trend.
[0040] Figure 63 is a comparison chart of the carbon dioxide conversion rates of the catalyst in Example 1 and the comparative catalyst at different temperatures. It can be seen that with the increase of temperature, the carbon dioxide conversion rates of the catalyst in Example 1 and the comparative catalyst both increase. The high entropy alloy hydride catalyst has a carbon dioxide conversion rate of 27.9% at normal pressure and 150°C. The average carbon dioxide conversion rate of the high entropy alloy hydride catalyst in Example 1 at normal pressure and 200°C is 96.5%, while the average carbon dioxide conversion rate of the comparative high entropy alloy MgCuNiTiY catalyst at normal pressure and 200°C is only 56.6%.
Claims
1. A high entropy alloy hydride catalyst for carbon dioxide methanation, characterized in that: The high entropy alloy hydride catalyst for carbon dioxide methanation is composed of a high entropy alloy hydride phase and a magnesium nitride phase; the high entropy alloy hydride is MgCuNi x TiY hydride, MgCuNi x The TiY hydride is a spherical particle with a single-phase body-centered cubic BCC crystal structure, wherein, in atomic percentage, 0.5≤x≤1.0; the magnesium nitride is a thin film coated on the surface of the high-entropy alloy hydride spherical particle, the film layer is rough, uneven and discontinuous, and the film layer thickness is 0.01-0.15 μm.
2. The high entropy alloy hydride catalyst for carbon dioxide methanation according to claim 1, characterized in that: The high entropy alloy hydride catalyst for carbon dioxide methanation can absorb and release hydrogen without being activated, and the amount of hydrogen absorbed and released is 0.552-0.869wt.%.
3. The method for preparing a high entropy alloy hydride catalyst for carbon dioxide methanation according to claim 1 or 2, characterized in that: The steps include: (1) Weigh raw materials magnesium block, copper block, nickel block, titanium block and yttrium block according to the atomic ratio of Mg: Cu: Ni: Ti: Y = 1: 1: x: 1: 1, where 0.5≤x≤1.0; (2) placing the raw materials prepared in step (1) into an induction melting furnace in sequence, and melting them under argon protection to obtain an alloy melt; (3) The alloy melt obtained in step (2) is poured into a tundish with a φ5 mm leak hole at the bottom through a guide tube under argon protection, and a high-pressure nitrogen-hydrogen mixed gas is turned on to start atomization. The alloy melt and the mixed gas react in situ by gas atomization to generate MgCuNi x TiY hydride spherical particles and coated on MgCuNi x A magnesium nitride film on the surface of TiY hydride spherical particles; the volume percentage of hydrogen in the nitrogen-hydrogen mixed gas is 25%; the nozzle used for gas atomization is a tightly coupled annular gap nozzle; (4) After the atomization is completed, the product obtained in step (3) is cooled and sieved under a nitrogen protective atmosphere to obtain a high entropy alloy hydride catalyst for carbon dioxide methanation.
4. The method for preparing a high entropy alloy hydride catalyst for carbon dioxide methanation according to claim 3, characterized in that: In step (2), the raw materials are placed in the order of copper block, titanium block, nickel block, yttrium block and magnesium block; the induction melting furnace is evacuated to 1.0~2.0×10 -3 Pa; the pressure of argon is 1.0~1.2×10 5 Pa; the melting temperature is 1300~1450℃.
5. The method for preparing a high entropy alloy hydride catalyst for carbon dioxide methanation according to claim 3, characterized in that: In step (3), the pressure of the high-pressure nitrogen-hydrogen mixed gas is 1.5-10.0 MPa.
6. The method for preparing a high entropy alloy hydride catalyst for carbon dioxide methanation according to claim 3, characterized in that: The nitrogen protective atmosphere pressure in step (4) is 1.0~1.2×10 5 Pa; the D50 average particle size of the high entropy alloy hydride catalyst used for carbon dioxide methanation is 15~25μm.